Preparation method of high-environmental-stability reflecting electrode material for high-power LED (light-emitting diode)

By using a technology combining polysilicon substrate and double-layer graphene in LED chip packaging, the problem of insufficient stability and heat dissipation of reflective electrode materials is solved, and the stability and safety of LED electrodes in high environments is achieved, ensuring large-scale Reliability of power operation.

CN118943256AInactive Publication Date: 2024-11-12FANGBO TECHNOLOGY (CHANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410931037.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing LED chip packages, the stability and heat dissipation of reflective electrode materials are poor, resulting in unstable high-power LEDs when used in high environments.

Method used

The polysilicon substrate and bilayer graphene are combined with excimer laser annealing to reduce the roughness of polysilicon to form an Ag3Sn doped bilayer graphene film, and the thermal conductivity and energy band structure of graphene are used to improve the stability of the electrode material. And enhance coupling through high temperature and high pressure treatment.

Benefits of technology

The high environmental stability and mechanical properties of LED reflective electrode materials are achieved, ensuring stable and safe operation under high power conditions, reducing thermal effects, and improving the overall stability of electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-environmental-stability reflecting electrode material for a high-power LED, and relates to the technical field of optoelectronic devices. According to the method, the polycrystalline silicon substrate is prepared by using an excimer laser annealing process, so that crystal grains of a polycrystalline silicon growth bottom layer can fully grow, the roughness is reduced, and the problem of non-uniform voltage is solved. Secondly, a double-layer graphene film is formed on the surface of the polycrystalline silicon layer substrate, and Ag3Sn is doped into double-layer graphene and interacts with the double-layer graphene; therefore, the key length of a C-C key is increased, the key energy is weakened, and the stability of high-power use of an LED electrode is ensured in various environments; then, rapid annealing is carried out, so that the surface of the polycrystalline silicon and the metal Ag3Sn are mutually diffused, and the reaction is slow and balanced; in addition, a temperature gradient is formed by utilizing the thermal conductivity of the graphene, so that the thermal effect of the electrode is reduced, and the coupling between the double-layer graphene and the polycrystalline silicon and doped metal is improved under the assistance of high temperature and high pressure. The prepared electrode material has a stable effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optoelectronic devices, and in particular to a method for preparing a reflective electrode material with high environmental stability for high-power LEDs. Background Art

[0002] Light-emitting diodes are a new type of solid-state light source that can directly and efficiently convert electrical energy into light energy. Compared with traditional light sources, they have the advantages of long life, small size, energy saving, high efficiency, fast response speed, earthquake resistance, and no pollution. They are a new generation of semiconductor lighting sources after incandescent lamps and fluorescent lamps. At present, they have become a green industry that promotes rapid economic development. However, due to the influence of LED chip packaging, usually only the light emitted from the front can be effectively utilized, and the light escaping from the bottom and sides needs to be reflected to the front through a reflective cup. In order to avoid the absorption of light by the solid crystal material between the chip and the reflective cup, a high-reflectivity back electrode can be prepared on the back of the chip substrate.

[0003] Graphene has excellent electrical and optical properties, and is therefore expected to be used to develop a new generation of electronic components, transistors, and optoelectronic devices that are thinner and conduct electricity faster. Double-layer graphene is composed of two layers of carbon atoms. Due to the coupling between the atomic layers, a band gap will appear in the energy band structure, which makes graphene have a wide range of application prospects in the field of optoelectronics. Through the synergistic effect between graphene, polysilicon, and Ag alloys, doping metals with semiconductor materials can easily lead to problems such as material instability and poor heat dissipation. In order to solve the above problems, the present invention provides a method for preparing a reflective electrode material with high environmental stability for high-power LEDs. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a reflective electrode material with high environmental stability for high-power LEDs, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a reflective electrode material with high environmental stability for high-power LEDs, comprising the following preparation steps: (1) Place the tinning solution in an electrolytic cell, and use a pure copper workpiece that has been cleaned, derusted and blown dry as the cathode, and a tin sheet as the anode. The cathode and anode plating sheet area ratio is 1:1, and a tin-plated copper sheet is electroplated by direct current deposition; the current density is controlled at 0.5-2A / dm 2 The plating solution temperature is controlled at 10-30℃, and the electroplating time is 10min. The silver plating solution is placed in an electrolytic cell, and the tin-plated copper sheet is cleaned once with acetone and alcohol respectively, and blown dry as the cathode, and the silver sheet is used as the anode. The silver-plated layer is electroplated by direct current deposition, and the cathode current density is 0.2-0.4A / dm 2, the plating solution temperature is controlled at 10-30°C, the electroplating time is 30-300s, and the Sn-Ag composite plated copper sheet is obtained; the Sn-Ag composite plated copper sheet is placed in a vacuum resistance furnace, the temperature is raised to 150°C with the furnace, the heating rate is 5-7°C / min, the temperature is kept for 2-30min, and then the furnace is cooled to room temperature to obtain an Ag3Sn thin film copper sheet; (2) A 100 nm silicon nitride layer was first deposited on the glass substrate by plasma enhanced chemical vapor deposition, the deposition temperature was 300°C, the chamber pressure was 133 Pa, the RF power was maintained at 50 W, the flow rate of NH3 was 11 sccm, the flow rate of N2 was 500 sccm, and the flow rate of 5% SiH4 / N2 was sccm; then a 200 nm silicon dioxide layer was deposited, the flow rate of the silicon source was 1500 sccm, the flow rate of the oxygen source was 1200 sccm, the deposition temperature was 300°C, the chamber pressure was 133 Pa, and the RF power was 50 W, to obtain SiN x / SiO2 thin film layer; then depositing a first amorphous silicon layer of 30-100nm thereon, with a SiH4 flow rate of 1000sccm and a deposition rate of 0.5-2nm / s, and then depositing a second amorphous silicon layer of 60nm, with a deposition rate of 4-10nm / s, the first and second deposition amorphous silicon layer chamber pressures are both 133Pa, and the temperature is 350°C; then heat treating at 450°C for 2h, using 1 shot to perform a first laser annealing treatment on the amorphous silicon layer, using a xenon chloride excimer laser for the laser annealing treatment, and then using a 1-10wt% hydrofluoric acid aqueous solution for cleaning, the time is 10-60s, using 19 shots to perform a second laser annealing, using a xenon chloride excimer laser for the laser annealing treatment, to obtain a polycrystalline silicon substrate; (3) A pure copper sheet is used as a substrate, and a layer of catalyst promoter is coated on its surface, the coating thickness of the catalyst layer is 30-150nm, and then baked at a temperature of 20-60°C for 2-10min to obtain a combination; the combination is placed in a chemical vapor deposition equipment reaction chamber, evacuated to 5×10 Pa, and then hydrogen is introduced to make the pressure in the equipment reaction chamber reach 50-2000Pa, and then the temperature in the equipment reaction chamber is increased to 850-1000°C and kept warm for 10-60min, and the temperature is maintained unchanged, and hydrogen and gaseous carbon source are introduced, wherein the hydrogen flow rate is controlled at 10-50sccm, and the gaseous carbon source flow rate is controlled at 10-100sccm, and then the pressure in the equipment reaction chamber is controlled in the range of 150-4000Pa and kept warm for 10-60min; the temperature in the equipment reaction chamber is reduced to room temperature at a rate of 20-100°C while maintaining the hydrogen flow rate, the gaseous carbon source flow rate and the pressure in the equipment reaction chamber, to obtain a double-layer graphene film; (4) The prepared double-layer graphene film is transferred onto the polycrystalline silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting is completed, open the evaporation source baffle for evaporation coating, set the target film thickness to 20-30nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at a temperature of 450-650℃, an annealing atmosphere of inert atmosphere, and a time of 50-80s to obtain a thin film combination; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 2-5cm above the acetone liquid level, place the thin film combination on the bracket, and seal the container, heat to 150-250℃, the pressure in the sealed container reaches 1500-2000KPa, maintain for 2-6h, drop to 25℃, and take it out, so as to prepare a reflective electrode material with high environmental stability for LED.

[0006] Furthermore, the components of the tin plating solution in step (1) are: 3-4 parts of stannous sulfate, 18-22 parts of concentrated sulfuric acid, 3 parts of cyanide zinc plating brightener and 100 parts of deionized water.

[0007] Furthermore, the components of the silver plating solution in step (1) are: 4-5 parts of silver nitrate, 9-11 parts of nicotinic acid, 7-8 parts of ammonium acetate, 4.5-5.5 parts of potassium hydroxide, 7-8 parts of potassium carbonate, 3-4 parts of 27wt% ammonia water and 100 parts of deionized water.

[0008] Furthermore, the thickness of the Ag3Sn film in step (1) is about 0.8 μm.

[0009] Furthermore, in step (2), the wavelength of the xenon chloride excimer laser is 308 nm, the laser linear beam width is 300 μm, the laser pulse frequency is 300 Hz, the laser energy density is 300-500 mJ / cm, the scanning speed is 3-5 mm / s, and the pulse width is 25 nanoseconds.

[0010] Furthermore, the thickness of the pure copper sheet in step (3) is 25 μm.

[0011] Furthermore, in step (3), the co-catalyst is a decaborane-anisole solution with a concentration of 0.02-0.1 g / mL.

[0012] Furthermore, in step (3), the gaseous carbon source is methane.

[0013] Furthermore, the electron beam evaporation parameters in step (4) are: substrate temperature 20-30° C., evaporation distance 50-70 cm, electron gun voltage 10-520 kV, electron beam spot shape is circular, and evaporation rate 0.1-1 nm / s.

[0014] Furthermore, in step (4), the inert atmosphere is N2 or Ar.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention uses polycrystalline silicon as a substrate, deposits double-layer graphene, and dopes Ag3Sn alloy to form a thin film as an electrode material to achieve a stable effect.

[0016] First, the present invention uses an excimer laser annealing process to prepare a polysilicon substrate with low surface roughness. After being treated with a special laser annealing process, the grains at the bottom layer of the polysilicon growth can be fully grown, and the polysilicon substrate can be free of huge protrusions, thereby reducing the roughness and improving the problem of voltage unevenness, which is beneficial to the subsequent deposition of graphene and the overall stability of the film as a motor material.

[0017] Secondly, a graphene film is formed on the surface of the polysilicon layer substrate. The graphene film has a double-layer structure. Due to its adjustable band structure and high mobility, the double-layer graphene can give the electrode material film stable optoelectronic and mechanical properties. On this basis, the surface layer graphene is modified by metal intercalation: Ag3Sn is doped into the double-layer graphene and interacts with the double-layer graphene. This will increase the CC bond length, weaken the bond energy, and require more energy to destroy the structure. Therefore, the film itself has a more stable structure. Therefore, the stronger interaction between the Ag3Sn molecules and the double-layer graphene means that the two are more stable when forming a doped structure. The stability of LED electrodes at high power is ensured in various environments. At the same time, a double-layer graphene film is coated on the polysilicon layer, and a part of the atoms on the surface of the polysilicon diffuse with the upper metal Ag3Sn through rapid annealing. The reaction is slow and balanced, and the mixed layer formed is more stable and stable, while the thickness of the film is controlled. In addition, the thermal conductivity of graphene is used to form a temperature gradient in the polysilicon film, thereby reducing the thermal effect of the electrode, so that the electrode can work stably and safely under high power conditions. Finally, high temperature and high pressure are used to further improve the coupling between the double-layer graphene and the polysilicon and doped metal, further improving the stability of the electrode material film. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a reflective electrode material with high environmental stability for high-power LEDs prepared in the following examples are as follows: Heat resistance: The examples and comparative examples were subjected to a heat treatment at 500°C for 30 min in an inert gas N2 atmosphere to simulate the heat treatment applied to the electrode material during the use of LED components. The surface properties of the electrode material film after the heat treatment were observed with an optical microscope (magnification: 500 times) and the hillock density (number / m 2 ) (with hillocks with a diameter of 0.1 μm or more as the target), and the average value was calculated.

[0020] Moisture resistance: The examples and comparative examples were stored at 25°C and 85% RH for 500 hours for reliability testing. The surface properties of the electrode material film after heating were observed with an optical microscope (magnification: 500 times) and the hillock density (number / m 2 ) (with hillocks with a diameter of 0.1 μm or more as the target), and the average value was calculated.

[0021] Embodiment 1; (1) a tin-plating solution is placed in an electrolytic cell, and a pure copper workpiece after cleaning, derusting and drying is used as a cathode, and a tin sheet is used as an anode, and the cathode-anode electroplating sheet area ratio is 1:1, and a tin-plated copper sheet is electroplated by direct current deposition; the components of the tin-plating solution are: 3 parts of stannous sulfate, 18 parts of concentrated sulfuric acid, 3 parts of cyanide zinc plating brightener and 100 parts of deionized water; the components of the silver-plating solution are: 4 parts of silver nitrate, 9 parts of nicotinic acid, 7 parts of ammonium acetate, 4.5 parts of potassium hydroxide, 7 parts of potassium carbonate, 3 parts of 27wt% ammonia water and 100 parts of deionized water; the current density is controlled at 0.5A / dm 2 The plating solution temperature was controlled at 10°C and the electroplating time was 10 min. The silver plating solution was placed in an electrolytic cell, and the tin-plated copper sheet was cleaned once with acetone and alcohol respectively, and then dried as the cathode. The silver sheet was used as the anode, and the silver layer was electroplated by direct current deposition. The cathode current density was 0.2 A / dm 2, the plating solution temperature is controlled at 10°C, the electroplating time is 30s, and a Sn-Ag composite-coated copper sheet is obtained; the Sn-Ag composite-coated copper sheet is placed in a vacuum resistance furnace, and the temperature is raised to 150°C with the furnace, the heating rate is 5°C / min, and the temperature is kept for 2min, and then the furnace is cooled to room temperature to obtain a Ag3Sn thin film copper sheet with a thickness of about 0.8μm; (2) A 100 nm silicon nitride layer was first deposited on the glass substrate by plasma enhanced chemical vapor deposition, the deposition temperature was 300°C, the chamber pressure was 133 Pa, the RF power was maintained at 50 W, the flow rate of NH3 was 11 sccm, the flow rate of N2 was 500 sccm, and the flow rate of 5% SiH4 / N2 was sccm; then a 200 nm silicon dioxide layer was deposited, the flow rate of the silicon source was 1500 sccm, the flow rate of the oxygen source was 1200 sccm, the deposition temperature was 300°C, the chamber pressure was 133 Pa, and the RF power was 50 W, to obtain SiN x / SiO2 thin film layer; then deposit a 30nm first amorphous silicon layer thereon, with a SiH4 flow rate of 1000sccm and a deposition rate of 0.5nm / s, and then deposit a 60nm second amorphous silicon layer at a deposition rate of 4nm / s, the first and second deposition amorphous silicon layer chamber pressures are both 133Pa, and the temperature is 350°C; then heat treat at 450°C for 2h, use 1 shot to perform the first laser annealing treatment on the amorphous silicon layer, the laser annealing treatment uses a xenon chloride excimer laser, and then use a 1wt% hydrofluoric acid aqueous solution for cleaning, the time is 10s, use 19 shots to perform the second laser annealing treatment, the laser annealing treatment uses a xenon chloride excimer laser, and obtain a polycrystalline silicon substrate; the wavelength of the xenon chloride excimer laser is 308nm, the laser linear beam width is 300μm, the laser pulse frequency is 300Hz, the laser energy density is 300mJ / cm, the scanning speed is 3mm / s, and the pulse width is 25 nanoseconds; (3) A pure copper sheet is used as a substrate, and a layer of catalyst promoter is coated on its surface. The coating thickness of the catalyst layer is 30 nm, and then it is baked at a temperature of 20°C for 2 minutes to obtain a combination; the catalyst is a decaborane-anisole solution with a concentration of 0.02 g / mL; the combination is placed in a chemical vapor deposition equipment reaction chamber, evacuated to 5×10 Pa, and then hydrogen is introduced to make the pressure in the equipment reaction chamber reach 50 Pa, and then the temperature in the equipment reaction chamber is increased to 850°C and kept warm for 10 minutes, and the temperature is maintained unchanged, and hydrogen and gaseous carbon source are introduced, wherein the hydrogen flow rate is controlled at 10 sccm, and the gaseous carbon source methane flow rate is controlled at 10 sccm, and then the pressure in the equipment reaction chamber is controlled to be within the range of 150 Pa and kept warm for 10 minutes; maintaining the hydrogen flow rate, gaseous carbon source flow rate and pressure in the equipment reaction chamber, the temperature in the equipment reaction chamber is reduced to room temperature at a rate of 20°C to obtain a double-layer graphene film; (4) The prepared double-layer graphene film is transferred onto the polycrystalline silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting is completed, open the evaporation source baffle for evaporation coating, set the target film thickness to 20nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at 450℃ in an inert atmosphere of N2 for 50s to obtain a thin film combination; the electron beam evaporation parameters are: substrate temperature 20℃, evaporation distance 50cm, electron gun voltage 10 kV, the electron beam spot shape is circular, and the evaporation rate is 0.1nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 2cm above the acetone liquid level, place the film combination on the bracket, and seal the container, heat to 150℃, the pressure in the sealed container reaches 1500KPa, maintain for 2h, drop to 25℃, and take out, thus preparing a reflective electrode material with high environmental stability for LED.

[0022] Embodiment 2; (1) a tin-plating solution is placed in an electrolytic cell, and a pure copper workpiece after cleaning, derusting and drying is used as a cathode, and a tin sheet is used as an anode, and the cathode-anode electroplating sheet area ratio is 1:1, and a tin-plated copper sheet is electroplated by direct current deposition; the components of the tin-plating solution are: 3.5 parts of stannous sulfate, 20 parts of concentrated sulfuric acid, 3 parts of cyanide zinc plating brightener and 100 parts of deionized water; the components of the silver-plating solution are: 4.5 parts of silver nitrate, 10 parts of nicotinic acid, 7.5 parts of ammonium acetate, 4 parts of potassium hydroxide, 7.5 parts of potassium carbonate, 3.5 parts of 27wt% ammonia water and 100 parts of deionized water; the current density is controlled at 1.25A / dm 2 The plating solution temperature was controlled at 20°C and the electroplating time was 10 min. The silver plating solution was placed in an electrolytic cell, and the tin-plated copper sheet was cleaned once with acetone and alcohol respectively, and then dried as the cathode. The silver sheet was used as the anode, and the silver layer was electroplated by direct current deposition. The cathode current density was 0.3 A / dm 2 , the plating solution temperature is controlled at 20°C, the electroplating time is 160s, and a Sn-Ag composite-coated copper sheet is obtained; the Sn-Ag composite-coated copper sheet is placed in a vacuum resistance furnace, and the temperature is raised to 150°C with the furnace, the heating rate is 6°C / min, and the temperature is kept for 16min, and then the furnace is cooled to room temperature, and a Ag3Sn thin film copper sheet with a thickness of about 0.8μm is obtained; (2) A 100 nm silicon nitride layer was first deposited on the glass substrate by plasma enhanced chemical vapor deposition, the deposition temperature was 300°C, the chamber pressure was 133 Pa, the RF power was maintained at 50 W, the flow rate of NH3 was 11 sccm, the flow rate of N2 was 500 sccm, and the flow rate of 5% SiH4 / N2 was sccm; then a 200 nm silicon dioxide layer was deposited, the flow rate of the silicon source was 1500 sccm, the flow rate of the oxygen source was 1200 sccm, the deposition temperature was 300°C, the chamber pressure was 133 Pa, and the RF power was 50 W, to obtain SiN x / SiO2 thin film layer; then deposit a first amorphous silicon layer of 65nm on it, the SiH4 flow rate is 1000sccm, the deposition rate is 1.25nm / s, and then deposit a second amorphous silicon layer of 60nm, the deposition rate is 7nm / s, the first and second deposition amorphous silicon layer chamber pressure is 133Pa, the temperature is 350℃; then heat treat at 450℃ for 2h, use 1 shot to perform the first laser annealing treatment on the amorphous silicon layer, the laser annealing treatment uses a xenon chloride excimer laser, and then use 5wt% hydrofluoric acid aqueous solution for cleaning, the time is 35s, use 19 shots to perform the second laser annealing treatment, the laser annealing treatment uses a xenon chloride excimer laser, and obtain a polycrystalline silicon substrate; the wavelength of the xenon chloride excimer laser is 308nm, the laser linear beam width size is 300μm, the laser pulse frequency is 300Hz, the laser energy density is 400mJ / cm, the scanning speed is 4mm / s, and the pulse width is 25 nanoseconds; (3) A pure copper sheet is used as a substrate, and a layer of catalyst promoter is coated on its surface. The coating thickness of the catalyst layer is 80 nm, and then it is baked at a temperature of 40°C for 6 minutes to obtain a combination; the catalyst is a decaborane-anisole solution with a concentration of 0.06 g / mL; the combination is placed in a chemical vapor deposition equipment reaction chamber, evacuated to 5×10 Pa, and then hydrogen is introduced to make the pressure in the equipment reaction chamber reach 1000 Pa, and then the temperature in the equipment reaction chamber is increased to 925°C and kept warm for 35 minutes, and the temperature is maintained unchanged, and hydrogen and gaseous carbon source are introduced, wherein the hydrogen flow rate is controlled at 30 sccm, and the gaseous carbon source methane flow rate is controlled at 55 sccm, and then the pressure in the equipment reaction chamber is controlled within the range of 2000 Pa and kept warm for 35 minutes; while maintaining the hydrogen flow rate, gaseous carbon source flow rate and pressure in the equipment reaction chamber, the temperature in the equipment reaction chamber is reduced to room temperature at a rate of 60°C to obtain a double-layer graphene film; (4) The prepared double-layer graphene film is transferred onto the polycrystalline silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting, open the evaporation source baffle for evaporation coating, set the target film thickness to 25nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at 550℃, annealing atmosphere is inert atmosphere N2, time is 65s, and a thin film combination is obtained; the electron beam evaporation parameters are: substrate temperature 25℃, evaporation distance 60cm, electron gun voltage 265 kV, the electron beam spot shape is circular, and the evaporation rate is 0.5nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 3.5cm above the acetone liquid level, place the film combination on the bracket, and seal the container, heat to 200℃, the pressure in the sealed container reaches 1750KPa, maintain for 4h, drop to 25℃, and take out, thus preparing a reflective electrode material with high environmental stability for LED.

[0023] Embodiment 3; (1) a tin-plating solution is placed in an electrolytic cell, and a pure copper workpiece after cleaning, derusting and drying is used as a cathode, and a tin sheet is used as an anode, and the cathode-anode electroplating sheet area ratio is 1:1, and a tin-plated copper sheet is electroplated by direct current deposition; the components of the tin-plating solution are: 4 parts of stannous sulfate, 22 parts of concentrated sulfuric acid, 3 parts of cyanide zinc plating brightener and 100 parts of deionized water; the components of the silver-plating solution are: 5 parts of silver nitrate, 11 parts of nicotinic acid, 8 parts of ammonium acetate, 5.5 parts of potassium hydroxide, 8 parts of potassium carbonate 7, 4 parts of 27wt% ammonia water and 100 parts of deionized water; the current density is controlled at 2A / dm 2 The plating solution temperature was controlled at 30°C and the electroplating time was 10 min. The silver plating solution was placed in an electrolytic cell, and the tin-plated copper sheet was cleaned once with acetone and alcohol respectively, and then dried as the cathode. The silver sheet was used as the anode, and the silver layer was electroplated by direct current deposition. The cathode current density was 0.4 A / dm 2 , the plating solution temperature is controlled at 30°C, the electroplating time is 300s, and a Sn-Ag composite plated copper sheet is obtained; the Sn-Ag composite plated copper sheet is placed in a vacuum resistance furnace, and the temperature is raised to 150°C with the furnace, the heating rate is 7°C / min, and the temperature is kept for 30min, and then the furnace is cooled to room temperature to obtain a Ag3Sn thin film copper sheet with a thickness of about 0.8μm; (2) A 100 nm silicon nitride layer was first deposited on the glass substrate by plasma enhanced chemical vapor deposition, the deposition temperature was 300°C, the chamber pressure was 133 Pa, the RF power was maintained at 50 W, the flow rate of NH3 was 11 sccm, the flow rate of N2 was 500 sccm, and the flow rate of 5% SiH4 / N2 was sccm; then a 200 nm silicon dioxide layer was deposited, the flow rate of the silicon source was 1500 sccm, the flow rate of the oxygen source was 1200 sccm, the deposition temperature was 300°C, the chamber pressure was 133 Pa, and the RF power was 50 W, to obtain SiN x / SiO2 thin film layer; then deposit a 100nm first amorphous silicon layer thereon, with a SiH4 flow rate of 1000sccm and a deposition rate of 2nm / s, and then deposit a 60nm second amorphous silicon layer at a deposition rate of 10nm / s, the first and second deposition amorphous silicon layer chamber pressures are both 133Pa, and the temperature is 350°C; then heat treat at 450°C for 2h, use 1 shot to perform the first laser annealing treatment on the amorphous silicon layer, the laser annealing treatment uses a xenon chloride excimer laser, and then use a 10wt% hydrofluoric acid aqueous solution for cleaning, the time is 60s, and use 19 shots to perform the second laser annealing treatment, the laser annealing treatment uses a xenon chloride excimer laser, and obtain a polycrystalline silicon substrate; the wavelength of the xenon chloride excimer laser is 308nm, the laser linear beam width is 300μm, the laser pulse frequency is 300Hz, the laser energy density is 500mJ / cm, the scanning speed is 5mm / s, and the pulse width is 25 nanoseconds; (3) A pure copper sheet is used as a substrate, and a layer of catalyst promoter is coated on its surface. The coating thickness of the catalyst layer is 150 nm, and then it is baked at a temperature of 60°C for 10 minutes to obtain a combination; the catalyst is a decaborane-anisole solution with a concentration of 0.1 g / mL; the combination is placed in a chemical vapor deposition equipment reaction chamber, evacuated to 5×10 Pa, and then hydrogen is introduced to make the pressure in the equipment reaction chamber reach 2000 Pa, and then the temperature in the equipment reaction chamber is increased to 1000°C and kept warm for 60 minutes, and the temperature is maintained unchanged, and hydrogen and gaseous carbon source are introduced, wherein the hydrogen flow rate is controlled at 50 sccm, and the gaseous carbon source methane flow rate is controlled at 100 sccm, and then the pressure in the equipment reaction chamber is controlled within the range of 4000 Pa and kept warm for 60 minutes; maintaining the hydrogen flow rate, gaseous carbon source flow rate and pressure in the equipment reaction chamber, the temperature in the equipment reaction chamber is reduced to room temperature at a rate of 100°C to obtain a double-layer graphene film; (4) The prepared double-layer graphene film is transferred onto the polycrystalline silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting is completed, open the evaporation source baffle for evaporation coating, set the target film thickness to 30nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at 650℃, annealing atmosphere is inert atmosphere Ar, time is 80s, and a thin film combination is obtained; the electron beam evaporation parameters are: substrate temperature 30℃, evaporation distance 70cm, electron gun voltage 520 kV, the electron beam spot shape is circular, and the evaporation rate is 1nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 5cm above the acetone liquid level, place the film combination on the bracket, and seal the container, heat to 250℃, the pressure in the sealed container reaches 2000KPa, maintain for 6h, drop to 25℃, and take out, thus preparing a reflective electrode material with high environmental stability for LED.

[0024] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (2) is different. Step (2) is changed to: a 100 nm silicon nitride layer is first deposited on the glass substrate by a plasma enhanced chemical vapor deposition method, the deposition temperature is 300 ° C, the chamber pressure is 133 Pa, the RF power is maintained at 50 W, the flow rate of NH3 is 11 sccm, the flow rate of N2 is 500 sccm, and the flow rate of 5% SiH4 / N2 is sccm; then a 200 nm silicon dioxide layer is deposited, the flow rate of the silicon source is 1500 sccm, the flow rate of the oxygen source is 1200 sccm, the deposition temperature is 300 ° C, the chamber pressure is 133 Pa, and the RF power is 50 W, to obtain SiN x / SiO2 thin film layer; then deposit a first amorphous silicon layer of 65nm on it, the SiH4 flow rate is 1000sccm, the deposition rate is 1.25nm / s, and then deposit a second amorphous silicon layer of 60nm, the deposition rate is 7nm / s, the chamber pressure of the first and second deposited amorphous silicon layers are both 133Pa, and the temperature is 350℃; then heat treat at 450℃ for 2h, adopt room temperature annealing, the annealing temperature is 450℃, the annealing time is 90s, and cool to room temperature after annealing to obtain a polycrystalline silicon substrate; the remaining steps are the same as Example 2.

[0025] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that there is no step (3), and step (4) is changed to: using electron beam evaporation to deposit the prepared Ag3Sn film on a polycrystalline silicon substrate, which is then placed on a planetary substrate rack in the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting, open the evaporation source baffle for evaporation coating, set the target film thickness to 25nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at 550℃, annealing atmosphere is inert atmosphere N2, time is 65s, and a thin film combination is obtained; the electron beam evaporation parameters are: substrate temperature 25℃, evaporation distance 60cm, electron gun voltage 265 kV, the electron beam spot shape is circular, and the evaporation rate is 0.5nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 3.5cm above the acetone liquid level, place the film combination on the bracket, and seal the container, heat to 200℃, the pressure in the sealed container reaches 1750KPa, maintain for 4h, drop to 25℃, take out, and prepare the reflective electrode material with high environmental stability for LED; the remaining steps are the same as Example 2.

[0026] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (2) is different, and step (3) is changed to: the prepared double-layer graphene film is covered on the polycrystalline silicon substrate in a transfer manner, and the prepared Ag3Sn film is deposited on the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the mechanical pump, the Roots pump and the condensation pump are used to evacuate the chamber in turn, and the background vacuum degree is 1.0×10 −5Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting is completed, open the evaporation source baffle for evaporation coating, set the target film thickness to 25nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, and take out the thin film combination; the electron beam evaporation parameters are: substrate temperature 25°C, evaporation distance 60 cm, electron gun voltage 265 kV, electron beam spot shape is circular, and evaporation rate 0.5nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 3.5cm above the acetone liquid level, place the thin film combination on the bracket, and seal the container, heat to 200°C, the pressure in the sealed container reaches 1750KPa, maintain for 4h, drop to 25°C, and take out, so as to prepare a reflective electrode material with high environmental stability for LED; the remaining steps are the same as Example 2.

[0027] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that steps (2) (4) are different. Steps (2) (4) are changed to: (2) a 100 nm silicon nitride layer is first deposited on a glass substrate by a plasma enhanced chemical vapor deposition method. The deposition temperature is 300° C., the chamber pressure is 133 Pa, the RF power is maintained at 50 W, the flow rate of NH3 is 11 sccm, the flow rate of N2 is 500 sccm, and the flow rate of 5% SiH4 / N2 is sccm; then a 200 nm silicon dioxide layer is deposited. The flow rate of the silicon source is 1500 sccm, the flow rate of the oxygen source is 1200 sccm, the deposition temperature is 300° C., the chamber pressure is 133 Pa, and the RF power is 50 W. SiN x / SiO2 thin film layer; then depositing a 65nm first amorphous silicon layer thereon, with a SiH4 flow rate of 1000sccm and a deposition rate of 1.25nm / s, and then depositing a 60nm second amorphous silicon layer at a deposition rate of 7nm / s, the first and second deposition chambers of the amorphous silicon layer are both at a pressure of 133Pa and a temperature of 350°C, to obtain an amorphous silicon substrate; (4) The prepared double-layer graphene film is transferred onto the amorphous silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the amorphous silicon substrate covered with the double-layer graphene is placed on the planetary substrate holder of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting, open the evaporation source baffle for evaporation coating, set the target film thickness to 25nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at 550℃, annealing atmosphere is inert atmosphere N2, time is 65s, and a thin film combination is obtained; the electron beam evaporation parameters are: substrate temperature 25℃, evaporation distance 60cm, electron gun voltage 265 kV, the electron beam spot shape is circular, and the evaporation rate is 0.5nm / s; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 3.5cm above the acetone liquid level, place the film combination on the bracket, and seal the container, heat to 200℃, the pressure in the sealed container reaches 1750KPa, maintain for 4h, drop to 25℃, take out, and prepare the reflective electrode material with high environmental stability for LED; the remaining steps are the same as Example 2.

[0028] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (4) is different, and step (4) is changed to: the prepared double-layer graphene film is covered on the polycrystalline silicon substrate in a transfer manner, and the prepared Ag3Sn film is deposited on the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the mechanical pump, the Roots pump and the condensation pump are used to evacuate the chamber in turn, and the background vacuum degree is 1.0×10 −5 When the temperature is 0.0407 W / m2, the electron gun power is turned on to pre-melt the Ag3Sn film for 300 s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting, the evaporation source baffle is opened for evaporation coating, and the target film thickness is set to 25 nm. The evaporation source is cooled for 10 min using the system's built-in water cooling system, and dry nitrogen is introduced into the chamber to atmospheric pressure. Then the vacuum chamber door is opened, the chamber is taken out, and rapid thermal annealing is performed at a temperature of 550 ° C. The annealing atmosphere is an inert atmosphere of N2 for 65 s, thereby preparing a reflective electrode material with high environmental stability for LED. The electron beam evaporation parameters are as follows: substrate temperature of 25 ° C, evaporation distance of 60 cm, electron gun voltage of 265 kV, electron beam spot shape of circular, and evaporation rate of 0.5 nm / s. The remaining steps are the same as those in Example 2.

[0029] Effect example Table 1 below shows the performance analysis results of a reflective electrode material with high environmental stability for high-power LEDs using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.

[0030] Table 1

[0031] From the comparison of experimental data on the stability of the embodiment and the comparative example, it can be found that the present invention uses an excimer laser annealing process to prepare a polycrystalline silicon substrate with low surface roughness. After being treated with a special laser annealing process, the grains of the polycrystalline silicon growth bottom layer can be fully grown, and the polycrystalline silicon substrate can be free of huge protrusions, reducing the roughness and improving the problem of voltage unevenness, which is beneficial to the subsequent deposition of graphene and the overall stability of the film as a motor material. Secondly, the present invention forms a double-layer graphene film on the surface of the polycrystalline silicon layer substrate. Due to its adjustable band structure and high mobility, it can give the electrode material film stable optoelectronic properties and mechanical properties; on this basis, the surface layer graphene is modified by metal intercalation: Ag3Sn is doped into the double-layer graphene and interacts with the double-layer graphene; this will lead to an increase in the CC bond length and a weakening of the bond energy. The stronger interaction between the Ag3Sn molecule and the double-layer graphene means that the two are more stable when forming a doped structure, ensuring the high power of the LED electrode in various environments. At the same time, a double-layer graphene film is coated on the polysilicon layer, and a part of the atoms on the surface of the polysilicon diffuse with the upper metal Ag3Sn through rapid annealing. The reaction is slow and balanced, and the mixed layer formed is more stable and stable. In addition, the thermal conductivity of graphene is used to form a temperature gradient in the polysilicon film, thereby reducing the thermal effect of the electrode, so that the electrode can work stably and safely under high-power conditions. Finally, high temperature and high pressure are used to further improve the coupling between the double-layer graphene and the polysilicon and doped metal, thereby further improving the stability of the electrode material film.

[0032] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a reflective electrode material with high environmental stability for high-power LEDs, characterized in that: The method comprises the following preparation steps: (1) Place the tinning solution in an electrolytic cell, and use a pure copper workpiece that has been cleaned, derusted and blown dry as the cathode, and a tin sheet as the anode. The cathode and anode plating sheet area ratio is 1:1, and a tin-plated copper sheet is electroplated by direct current deposition; the current density is controlled at 0.5-2A / dm 2 The plating solution temperature is controlled at 10-30℃, and the electroplating time is 10min. The silver plating solution is placed in an electrolytic cell, and the tin-plated copper sheet is cleaned once with acetone and alcohol respectively, and blown dry as the cathode, and the silver sheet is used as the anode. The silver-plated layer is electroplated by direct current deposition, and the cathode current density is 0.2-0.4A / dm 2 , the plating solution temperature is controlled at 10-30°C, the electroplating time is 30-300s, and the Sn-Ag composite plated copper sheet is obtained; the Sn-Ag composite plated copper sheet is placed in a vacuum resistance furnace, the temperature is raised to 150°C with the furnace, the heating rate is 5-7°C / min, the temperature is kept for 2-30min, and then the furnace is cooled to room temperature to obtain an Ag3Sn thin film copper sheet; (2) A 100 nm silicon nitride layer was first deposited on the glass substrate by plasma enhanced chemical vapor deposition, the deposition temperature was 300°C, the chamber pressure was 133 Pa, the RF power was maintained at 50 W, the flow rate of NH3 was 11 sccm, the flow rate of N2 was 500 sccm, and the flow rate of 5% SiH4 / N2 was sccm; then a 200 nm silicon dioxide layer was deposited, the flow rate of the silicon source was 1500 sccm, the flow rate of the oxygen source was 1200 sccm, the deposition temperature was 300°C, the chamber pressure was 133 Pa, and the RF power was 50 W, to obtain SiN x / SiO2 thin film layer; then depositing a first amorphous silicon layer of 30-100nm thereon, with a SiH4 flow rate of 1000sccm and a deposition rate of 0.5-2nm / s, and then depositing a second amorphous silicon layer of 60nm, with a deposition rate of 4-10nm / s, the first and second deposition amorphous silicon layer chamber pressures are both 133Pa, and the temperature is 350°C; then heat treating at 450°C for 2h, using 1 shot to perform a first laser annealing treatment on the amorphous silicon layer, using a xenon chloride excimer laser for the laser annealing treatment, and then using a 1-10wt% hydrofluoric acid aqueous solution for cleaning, the time is 10-60s, using 19 shots to perform a second laser annealing, using a xenon chloride excimer laser for the laser annealing treatment, to obtain a polycrystalline silicon substrate; (3) A pure copper sheet is used as a substrate, and a layer of catalyst promoter is coated on its surface, the coating thickness of the catalyst layer is 30-150nm, and then baked at a temperature of 20-60°C for 2-10min to obtain a combination; the combination is placed in a chemical vapor deposition equipment reaction chamber, evacuated to 5×10 Pa, and then hydrogen is introduced to make the pressure in the equipment reaction chamber reach 50-2000Pa, and then the temperature in the equipment reaction chamber is increased to 850-1000°C and kept warm for 10-60min, and the temperature is maintained unchanged, and hydrogen and gaseous carbon source are introduced, wherein the hydrogen flow rate is controlled at 10-50sccm, and the gaseous carbon source flow rate is controlled at 10-100sccm, and then the pressure in the equipment reaction chamber is controlled in the range of 150-4000Pa and kept warm for 10-60min; the temperature in the equipment reaction chamber is reduced to room temperature at a rate of 20-100°C while maintaining the hydrogen flow rate, the gaseous carbon source flow rate and the pressure in the equipment reaction chamber, to obtain a double-layer graphene film; (4) The prepared double-layer graphene film is transferred onto the polycrystalline silicon substrate, and the prepared Ag3Sn film is deposited onto the double-layer graphene film by electron beam evaporation: the polycrystalline silicon substrate covered with the double-layer graphene is placed on the planetary substrate rack of the evaporation chamber, the chamber door is closed, and the chamber is evacuated using a mechanical pump, a Roots pump, and a condensation pump in sequence until the background vacuum reaches 1.0×10 −5 Pa, turn on the electron gun power to pre-melt the Ag3Sn film for 300s, during which the evaporation source baffle is in a closed state, and no film is plated on the substrate. After the pre-melting is completed, open the evaporation source baffle for evaporation coating, set the target film thickness to 20-30nm, and then use the system's built-in water cooling system to cool the evaporation source for 10min, introduce dry nitrogen into the chamber to atmospheric pressure, then open the vacuum chamber door, take it out, and perform rapid thermal annealing at a temperature of 450-650℃, an annealing atmosphere of inert atmosphere, and a time of 50-80s to obtain a thin film combination; fix the bracket at the lower 1 / 3 of the container, add acetone, the bracket is 2-5cm above the acetone liquid level, place the thin film combination on the bracket, and seal the container, heat to 150-250℃, the pressure in the sealed container reaches 1500-2000KPa, maintain for 2-6h, drop to 25℃, and take it out, so as to prepare a reflective electrode material with high environmental stability for LED.

2. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The components of the tin plating solution in step (1) are: 3-4 parts of stannous sulfate, 18-22 parts of concentrated sulfuric acid, 3 parts of cyanide zinc plating brightener and 100 parts of deionized water.

3. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The components of the silver plating solution in step (1) are: 4-5 parts of silver nitrate, 9-11 parts of nicotinic acid, 7-8 parts of ammonium acetate, 4.5-5.5 parts of potassium hydroxide, 7-8 parts of potassium carbonate, 3-4 parts of 27wt% ammonia water and 100 parts of deionized water.

4. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The thickness of the Ag3Sn film in step (1) is about 0.8 μm.

5. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: In step (2), the wavelength of the xenon chloride excimer laser is 308 nm, the laser linear beam width is 300 μm, the laser pulse frequency is 300 Hz, the laser energy density is 300-500 mJ / cm, the scanning speed is 3-5 mm / s, and the pulse width is 25 nanoseconds.

6. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The thickness of the pure copper sheet in step (3) is 25 μm.

7. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: In the step (3), the catalyst promoter is a decaborane-anisole solution with a concentration of 0.02-0.1 g / mL.

8. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: In step (3), the gaseous carbon source is methane.

9. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The electron beam evaporation parameters in step (4) are: substrate temperature 20-30° C., evaporation distance 50-70 cm, electron gun voltage 10-520 kV, electron beam spot shape is circular, and evaporation rate 0.1-1 nm / s.

10. The method for preparing a reflective electrode material with high environmental stability for high-power LED according to claim 1, characterized in that: The inert atmosphere in step (4) is N2 or Ar.