Porous silicon-carbon composite material and preparation method thereof

By depositing lithium-doped porous carbon in the nickel foam template and depositing amorphous carbon on the outer layer, the conductivity and pore size problems of silicon carbon materials of silane cracking method are solved, the circulation and expansion performance of lithium-ion batteries are improved, and high pore capacity is achieved and porous silicon-carbon composite materials with high specific capacity.

CN118943273APending Publication Date: 2024-11-12HUIYANG (GUIZHOU) NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410563218.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor electronic conductivity, uneven pore size distribution and fast charging performance of existing silane cracking methods of silicon carbon materials lead to the cycling performance and expansion problems of the material. The low compressive strength of traditional high-porous porous porous carbon materials limits its application.

Method used

Porous silicon-carbon composite material with core-shell structure, the inner core is lithium-doped porous silicon-carbon, and the outer shell is amorphous carbon. Polyaniline is formed by depositing aniline in the nickel foam template and reacting with an oxidant. The silane compound is carbonized, and the vapor deposition method is used to externally The layer deposits amorphous carbon to enhance the electron conductivity and pore capacity.

Benefits of technology

The electronic conductivity, pore capacity and specific capacity of the material are significantly improved, expansion is reduced, rate performance and first-time efficiency are improved, and the circulation performance and diffusion coefficient of lithium-ion batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943273A_ABST
    Figure CN118943273A_ABST
Patent Text Reader

Abstract

The invention discloses a porous silicon-carbon composite material and a preparation method thereof, the porous silicon-carbon composite material has a core-shell structure, the core is lithium-doped porous silicon carbon, and the shell is amorphous carbon; the mass ratio of the shell is 1-5wt% according to 100% of the mass ratio of the composite material. The preparation method comprises the following steps: depositing aniline in a foamed nickel template through a chemical method, reacting with an oxidizing agent to generate polyaniline, silane and lithium stearate, carrying out acid pickling to remove foamed nickel, carrying out carbonization to obtain lithium-silicon-doped porous carbon, depositing nano silicon through a silane cracking method, and finally depositing amorphous carbon on the outer layer of the nano silicon through a vapor deposition method to obtain the lithium-silicon-doped porous carbon composite material. The porous silicon-carbon composite material is obtained. The electronic conductivity of the material can be improved, and the rate capability and the first efficiency can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of secondary battery material preparation, and specifically relates to a porous silicon-carbon composite material, and also relates to a preparation method of the porous silicon-carbon composite material. Background Art

[0002] At present, silicon-based materials are mainly divided into silicon-oxygen materials and silicon-carbon materials. Silicon-carbon materials are divided into sand-milling silicon-carbon and silane cracking silicon-carbon. Silane cracking silicon-carbon materials have become the main materials for high-energy-density lithium-ion batteries due to their high specific capacity, low expansion, and good cycle performance. However, due to the high specific surface area, poor electronic conductivity, and uneven pore size distribution of the porous carbon materials used in silane cracking silicon-carbon, the fast-charging performance of the materials deviates. Measures to improve the fast-charging performance of silicon-carbon materials mainly improve the electronic conductivity of porous carbon materials by physically doping metals or non-metallic materials. However, there are poor consistency and doped materials can easily reduce the pore volume of porous carbon, and reduce the deposition amount of nano-silicon, thereby reducing the specific capacity. At the same time, the use of traditional high-pore-volume porous carbon will cause the material to have low compressive strength, resulting in limited application of compaction density during the use of the material. To solve these problems, patent application number 202311025471.3 discloses a resin porous silicon-carbon negative electrode material and its preparation method and lithium-ion battery. The preparation method includes the following steps: heating the hardened resin to 600-900°C to make the resin porous, then introducing silane gas, heating to 400-500°C to crack the silane; then mixing with the hardened resin to obtain a resin porous silicon-carbon precursor, and then heating to 1000-1500°C to obtain a resin porous silicon-carbon negative electrode material. Although the specific capacity of the material obtained by this method is improved, the power performance is biased, the pore volume is small, and the expansion is large, which is not conducive to the improvement of cycle performance. Summary of the invention

[0003] The purpose of the present invention is to overcome the above disadvantages and provide a porous silicon-carbon composite material that can enhance electronic conductivity, improve rate performance and initial efficiency.

[0004] Another object of the present invention is to provide a method for preparing the porous silicon-carbon composite material.

[0005] The porous silicon-carbon composite material of the present invention presents a core-shell structure, wherein the core is lithium-doped porous silicon-carbon and the shell is composed of amorphous carbon; based on the mass ratio of the composite material being 100%, the mass ratio of the shell is 1-5wt%.

[0006] A method for preparing a porous silicon-carbon composite material of the present invention comprises the following steps:

[0007] Step S1: according to the mass ratio of lithium stearate: nickel foam: liquid silane: aniline: oxidant solution = 1-5: 500: 100: 50-150: 20-50, lithium stearate is added to a benzene solution to prepare a 1-5wt% solution, nickel foam is added and dispersed evenly, liquid silane is added, aniline is dispersed evenly, and then an oxidant solution is added, reacted at a temperature of 25-80°C for 2-12h, filtered, the obtained filter residue is added to a 5wt% dilute nitric acid solution and soaked for 24-48h, filtered, and the obtained filter residue is transferred to a tubular furnace and carbonized at a temperature of 1000-1400°C for 1-6h to obtain lithium silicon doped porous carbon;

[0008] Step S2: transfer the lithium silicon doped porous carbon to a tubular furnace, introduce inert gas to exhaust the air in the tube, and deposit for 30-300 min at a temperature of 400-600°C, a pressure of 2-10 MPa, and a silane gas flow rate of 100-500 ml / min. Stop introducing silane gas and replace it with carbon source gas, and raise the temperature to 500-900°C, and deposit for 1-6 h at a gas flow rate of 50-200 ml / min to obtain a porous silicon-carbon composite material.

[0009] In the above-mentioned method for preparing a porous silicon-carbon composite material, the liquid silane in step S1 is at least one of tetradecane, pentadecane, hexadecane, heptadecane or octadecane.

[0010] In the above-mentioned method for preparing a porous silicon-carbon composite material, the oxidant solution in step S1 is one of hydrogen peroxide, ferric chloride or ammonium persulfate, with a concentration of 10-30wt%.

[0011] In the above-mentioned method for preparing a porous silicon-carbon composite material, the silane described in step S2 is one of tetrahydrosilane, trichlorosilane, tetrachlorosilane, dimethylchlorosilane or disilane; and the carbon source gas is one of methane, ethane, ethylene or acetylene.

[0012] Compared with the prior art, the present invention has obvious beneficial effects. It can be seen from the above technical scheme that the present invention deposits polyaniline, silane and lithium stearate generated by aniline reacting with an oxidant in a foam nickel template by a chemical method, removes the foam nickel by pickling, and carbonizes to obtain lithium silicon doped porous carbon, which has the characteristics of large pore size, high pore volume, high electronic conductivity, etc.; the high pore volume can increase the deposition amount of nano silicon by silane cracking method, increase specific capacity and reduce expansion. Amorphous carbon is deposited on its outer layer by vapor deposition method to improve the electronic conductivity of the material, improve the rate performance and the first efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is the SEM image of the porous silicon-carbon composite material prepared in Example 1. DETAILED DESCRIPTION

[0014] Embodiment 1:

[0015] A method for preparing a porous silicon-carbon composite material comprises the following steps:

[0016] Step S1: 3g of lithium stearate is added to 100g of benzene solution to prepare a 3wt% solution, then 500g of nickel foam is added and dispersed evenly, then 100g of tetradecane and 100g of aniline are added and dispersed evenly, then 30g of 20wt% ferric chloride solution is added, reacted at a temperature of 50°C for 6h, filtered, the obtained filter residue is added to 500g of 5wt% dilute nitric acid solution and soaked for 36h, filtered, and the obtained filter residue is transferred to a tubular furnace and carbonized at a temperature of 1200°C for 3h to obtain lithium silicon doped porous carbon;

[0017] Step S2: The lithium silicon-doped porous carbon is transferred to a tubular furnace, argon inert gas is introduced to exhaust the air in the tube, and then tetrahydrosilane gas is introduced through a silane cracking method at a temperature of 500°C and a pressure of 8Mpa, and deposited at a flow rate of 300ml / min for 120min to deposit nanosilicon in the lithium silicon-doped porous carbon; then the introduction of tetrahydrosilane is stopped and ethylene gas is introduced instead, and the temperature is raised to 700°C, and deposited at a gas flow rate of 100ml / min for 3h to obtain a porous silicon-carbon composite material.

[0018] Embodiment 2:

[0019] A method for preparing a porous silicon-carbon composite material comprises the following steps:

[0020] Step S1: 1g of lithium stearate is added to 100g of benzene solution to prepare a 1% solution, then 500g of nickel foam is added and dispersed evenly, then 100g of pentadecane and 50g of aniline are added and dispersed evenly, then 20g of a 10% hydrogen peroxide solution is added, reacted at a temperature of 25°C for 12h, filtered, the obtained filter residue is added to 500g of a 5wt% dilute nitric acid solution and soaked for 24h, filtered, and the obtained filter residue is transferred to a tubular furnace and carbonized at a temperature of 1000°C for 6h to obtain lithium silicon doped porous carbon;

[0021] Step S2: The lithium silicon-doped porous carbon is transferred to a tubular furnace, and then argon inert gas is introduced to exhaust the air in the tube, and then trichlorosilane gas is introduced by a silane cracking method at a temperature of 400°C and a pressure of 10Mpa, and deposited at a flow rate of 100ml / min for 300min to deposit nanosilicon in the lithium silicon-doped porous carbon; then the introduction of trichlorosilane gas is stopped and acetylene gas is introduced instead, and the temperature is raised to 500°C, and deposited at a gas flow rate of 50ml / min for 6h to obtain a porous silicon-carbon composite material.

[0022] Embodiment 3:

[0023] A method for preparing a porous silicon-carbon composite material comprises the following steps:

[0024] Step S1: 5g of lithium stearate is added to 100g of benzene solution to prepare a 5wt% solution, then 500g of nickel foam is added and dispersed evenly, then 100g of hexadecane and 150g of aniline are added and dispersed evenly, then 50g of 20wt% ammonium persulfate solution is added, reacted at 80°C for 2h, filtered, the obtained filter residue is added to 500g of 5wt% dilute nitric acid solution and soaked for 48h, filtered, and the obtained filter residue is transferred to a tubular furnace and carbonized at 1400°C for 1h to obtain lithium silicon doped porous carbon;

[0025] Step S2: The lithium silicon-doped porous carbon is transferred to a tubular furnace, and then argon inert gas is introduced to exhaust the air in the tube, and then tetrachlorosilane gas is introduced by a silane cracking method at a temperature of 600°C and a pressure of 2Mpa, and deposited at a flow rate of 500ml / min for 30min, thereby depositing nanosilicon in the lithium silicon-doped porous carbon; then the introduction of tetrachlorosilane gas is stopped and replaced with methane gas, and the temperature is raised to 900°C, and deposited at a gas flow rate of 200ml / min for 1h to obtain a porous silicon-carbon composite material.

[0026] Comparative Example 1:

[0027] A method for preparing a silicon-carbon composite material, comprising:

[0028] The difference from Example 1 is that lithium stearate, aniline and ferric chloride are not added in step S1, and the rest is the same as Example 1.

[0029] Comparative Example 2:

[0030] A method for preparing a silicon-carbon composite material, comprising:

[0031] The difference from Example 1 is that porous carbon is used to replace lithium silicon-doped porous carbon in step S1, and the rest is the same as Example 1.

[0032] Test example:

[0033] (1) SEM test

[0034] Figure 1 This is a SEM picture of the silicon-carbon composite material prepared in Example 1. It can be seen from the picture that the material has a granular structure, a porous structure on the surface, and fine powder material is bonded to the surface with a particle size of about 5 μm.

[0035] (2) Physical and chemical properties test:

[0036] Referring to the national standard GB / T 38823-2020 "Silicon Carbon", the specific surface area and tap density of each silicon-carbon composite material were tested, and the powder conductivity of each composite material was tested by a four-probe tester, and the gas production of the powder material was tested (test method: 100g of powder material was added to 45°C deionized water and allowed to stand for 48 hours to test its gas production); at the same time, the pore volume and pore size of the lithium-silicon doped porous carbon were tested by a micropore tester; the test results are shown in Table 1 below.

[0037] (3) Button battery test:

[0038] The silicon-carbon composite materials corresponding to Examples 1-3 and Comparative Examples 1-2 were used as negative electrode materials for lithium-ion batteries to prepare button batteries according to the following method:

[0039] A binder, a conductive agent and a solvent are added to each corresponding silicon-carbon composite material, stirred to make a slurry, coated on a copper foil, and dried and rolled to obtain a negative electrode sheet; the binder used is LA132, the conductive agent is SP (conductive carbon black), the solvent is NMP, and the usage ratio of the composite material, SP, LA132, and NMP is 95g:1g:4g:220mL; the electrolyte is a solution with LiPF6 as the electrolyte, and the concentration is 1mol / L, wherein the solvent is a mixture of EC and DEC in a volume ratio of 1:1; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film.

[0040] Each button cell was assembled in an argon-filled glove box, and then the electrochemical performance was tested. Specifically, the electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester with a charge and discharge voltage range of 0.005V to 2.0V and a charge and discharge rate of 0.1C. The discharge specific capacity and the first efficiency of the material were tested. The diffusion coefficient of the material was tested by GI TT. The test results are shown in Table 1 below.

[0041] The negative electrode sheet of the above button battery was also tested for full-charge expansion. The specific test process is: the thickness D1 of the negative electrode sheet of the rolled button battery was tested, and then the full-charge thickness D2 of the negative electrode sheet was dissected when the button battery was fully charged to 100% SOC, and then the expansion rate was calculated (expansion rate = (D1-D2) / D1*100%); the test results are shown in Table 1 below.

[0042] Table 1

[0043]

[0044] It can be seen from the data in Table 1 above that the specific capacity, first efficiency and powder conductivity of the silicon-carbon composite materials prepared in Examples 1-3 of the present application are significantly better than those in Comparative Examples 1-2; the reason may be that: by doping lithium salts and their conductive polymers in the foam nickel template, after carbonization, the electronic conductivity of the material is improved, and at the same time, the silicon oxygen formed after carbonization of the doped silane compound also improves the specific capacity of the material, and the lithium silicon porous carbon has a high pore volume, which reduces expansion and increases the specific surface area, thereby improving the diffusion coefficient of the material.

[0045] (4)Soft pack performance test:

[0046] The silicon-carbon composite materials corresponding to Examples 1-3 and Comparative Examples 1-2 were doped with 95% artificial graphite as negative electrode materials (i.e., negative electrode plates) and positive electrode ternary materials (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), electrolyte and separator are assembled into a 5Ah soft-pack battery; wherein the separator is celegard 2400, the electrolyte is LiPF6 solution (the solvent is a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 is 1.3 mol / L) to prepare the soft-pack battery.

[0047] The following performance tests are performed on each soft pack battery:

[0048] A. HPPC test of the test material, after 3C pulse for 10S, the charging DCR under different SOC (97%, 95%, 90%, 70%, 50%, 30%, 10%, 5%) was tested. The test data is shown in Table 2.

[0049] Table 2

[0050]

[0051] It can be seen from Table 2 that the HPPC of the silicon-carbon composite materials provided in Examples 1-3 is lower than that in Comparative Examples 1-2; the reason may be that the silicon-carbon composite materials provided in the examples of the present application have a larger specific surface area, a high powder conductivity, a high diffusion coefficient, a reduced DCR, and improved rate performance.

[0052] b. Cycle performance test:

[0053] The test conditions for the cycle performance test are: charge and discharge voltage range of 2.5~4.2V, temperature of 25±3.0℃, charge and discharge rate of 1.0C / 1.0C, and cycle number of 500 times; at the same time, the full charge rebound of the negative electrode of the initial battery is tested.

[0054] The test results are shown in Table 3 below.

[0055] Table 3

[0056] example Initial pole piece full charge rebound Capacity retention after 500 cycles (%) Example 1 28.9% 95.2 Example 2 27.8% 95.9 Example 3 29.2% 94.2 Comparative Example 1 31.8% 91.8 Comparative Example 2 32.5% 90.2

[0057] It can be seen from Table 3 that the rate and cycle performance of the soft-pack lithium-ion batteries prepared using the silicon-carbon composite materials provided in Examples 1-3 are significantly better than those in Comparative Examples 1-2. The reason may be that the example materials have a high specific surface area, which improves the liquid retention performance of the material, while having low expansion and improving the cycle performance.

[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A porous silicon-carbon composite material presents a core-shell structure, wherein the core is lithium-doped porous silicon-carbon and the shell is composed of amorphous carbon; calculated based on the mass ratio of the composite material as 100%, the mass ratio of the shell is 1-5wt%.

2. A method for preparing a porous silicon-carbon composite material, comprising the following steps: Step S1: according to the mass ratio of lithium stearate: nickel foam: liquid silane: aniline: oxidant solution = 1-5: 500: 100: 50-150: 20-50, lithium stearate is added to the benzene solution to prepare a 1-5wt% solution, nickel foam is added and dispersed evenly, liquid silane and aniline are added and dispersed evenly, and then the oxidant solution is added, and the reaction is carried out at a temperature of 25-80°C for 2-12h, filtered, and the obtained filter residue is added to a 5wt% dilute nitric acid solution and soaked for 24-48h, filtered, and the obtained filter residue is transferred to a tubular furnace and carbonized at a temperature of 1000-1400°C for 1-6h to obtain lithium silicon doped porous carbon; Step S2: transfer the lithium silicon doped porous carbon to a tubular furnace, introduce inert gas to exhaust the air in the tube, and deposit for 30-300 min at a temperature of 400-600°C, a pressure of 2-10 MPa, and a silane gas flow rate of 100-500 ml / min. Stop introducing silane gas and replace it with carbon source gas, and raise the temperature to 500-900°C, and deposit for 1-6 h at a gas flow rate of 50-200 ml / min to obtain a porous silicon-carbon composite material.

3. A method for preparing a porous silicon-carbon composite material as claimed in claim 2, wherein the liquid silane described in step S1 is at least one of tetradecane, pentadecane, hexadecane, heptadecane or octadecane.

4. A method for preparing a porous silicon-carbon composite material as claimed in claim 2, wherein the oxidant solution in step S1 is one of hydrogen peroxide, ferric chloride or ammonium persulfate, with a concentration of 10-30wt%.

5. A method for preparing a porous silicon-carbon composite material as described in claim 2, wherein the silane described in step S2 is one of tetrahydrosilane, trichlorosilane, tetrachlorosilane, dimethylchlorosilane or disilane; and the carbon source gas is one of methane, ethane, ethylene or acetylene.