Carbon-based composite metal lithium negative electrode with hollow carbon fibers modified by lithium-loving layers inside and outside tube as well as preparation method and application of carbon-based composite metal lithium negative electrode

By growing manganese dioxide nanosheet arrays inside and outside hollow carbon fibers and filling them with molten lithium, a hollow carbon fiber composite lithium metal anode with lithium-affinity layers inside and outside the tube was prepared. This solved the problems of lithium dendrite growth and volume expansion, and improved the cycle stability and life of the battery.

CN118943303APending Publication Date: 2024-11-12NAT UNIV OF DEFENSE TECH

Patent Information

Application Number
CN202411000288.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Lithium metal anodes suffer from problems such as lithium dendrite growth, unstable SEI, and volume expansion, leading to rapid performance degradation and safety hazards in batteries.

Method used

Hollow carbon fibers were prepared by high-temperature calcination, manganese dioxide nanosheet arrays were grown by liquid-phase reduction, and hollow carbon fiber composite lithium metal anodes modified with lithiophilic layers inside and outside the tube were prepared by melt infiltration method, thus constructing a three-dimensional carbon-based current collector.

Benefits of technology

It significantly improves the wetting speed of lithium, promotes uniform deposition and inhibits dendrite growth, enhances the cycle stability and lifespan of the battery, alleviates volume expansion, and has a large specific surface area, light weight, good conductivity and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943303A_ABST
    Figure CN118943303A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon-based composite metal lithium negative electrode with hollow carbon fibers modified by lithium-loving layers inside and outside a tube as well as a preparation method and application of the carbon-based composite metal lithium negative electrode. The preparation method comprises the following steps: firstly, carbonizing cotton cloth to obtain carbonized cotton cloth with hollow carbon fibers; placing the carbonized cotton cloth in a potassium permanganate acid solution, and growing a lithium-loving layer of the MnO2 nanosheet array inside and outside the hollow carbon fiber tube under a heating condition; and finally, injecting molten lithium into the carbonized cotton cloth current collector modified by the lithium-loving layers inside and outside the tube through a melting lithium infiltration method to obtain the composite metal lithium negative electrode. The preparation method has the advantages of simple operation, low cost and batch production, creatively prepares the three-dimensional carbon-based current collector constructed by the hollow fibers modified by the lithium-loving layers inside and outside the tube, can effectively promote uniform deposition of metal lithium inside and outside the fibers, avoids generation of lithium dendrites, relieves volume expansion, and improves the performance of the current collector. The coulombic efficiency and the cycle life of the lithium metal battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal lithium negative electrode preparation, in particular to a carbon-based composite metal lithium negative electrode with hollow carbon fibers modified with lithium-philic layers inside and outside the tube, and a preparation method and application thereof. Background Art

[0002] The development of electric vehicles and portable electronic devices has put forward higher requirements on the energy density and cycle performance of batteries. Metallic lithium has an ultra-high theoretical specific capacity and low electrode potential. It is considered to be the ideal negative electrode for the next generation of high energy density lithium secondary batteries and has received extensive attention and research in recent years.

[0003] However, the metal lithium anode has problems such as lithium dendrite growth, unstable SEI and volume expansion, which not only cause rapid degradation of battery performance, but also bring serious safety hazards. Inhibiting the growth of lithium dendrites, building a stable anode interface and buffering its volume effect are key issues to be solved in the development of the next generation of high-energy-density lithium batteries. Summary of the invention

[0004] The present invention provides a carbon-based composite metal lithium negative electrode with a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, and a preparation method and application thereof. Carbonized cotton cloth with hollow fibers is prepared by a high-temperature calcination method, and then a lithium-philic manganese dioxide nanosheet array is grown inside and outside the hollow fiber by a liquid phase reduction method. Then, molten lithium is infused into the hollow fiber and between the fiber skeleton by a molten lithium infiltration method to obtain a composite metal lithium negative electrode, which is used to overcome the defects of the metal lithium negative electrode in the prior art, such as poor cycle stability and short life caused by dendrite growth and volume expansion.

[0005] To achieve the above object, the present invention provides a method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, comprising the following steps:

[0006] S1: placing cotton cloth in an inert atmosphere and calcining it to obtain carbonized cotton cloth;

[0007] S2: Under heating conditions, immersing the carbonized cotton cloth in a potassium permanganate acid solution, then taking it out, rinsing it with deionized water and vacuum drying it to obtain a carbonized cotton cloth with a manganese dioxide nanosheet array grown thereon;

[0008] S3: Carbonized cotton with manganese dioxide nanosheet arrays is placed on the surface of molten lithium metal. Under the action of capillary action and chemical reaction, the molten lithium metal infiltrates the entire carbonized cotton cloth, which is then taken out and the carbon-based composite lithium metal negative electrode is obtained after the molten lithium metal is cooled and solidified.

[0009] To achieve the above-mentioned purpose, the present invention also proposes a carbon-based composite metal lithium negative electrode of hollow carbon fibers modified with lithium-philic layers inside and outside the tube, which is prepared by the above-mentioned preparation method; the carbon-based composite metal lithium negative electrode is a three-dimensional carbon-based current collector constructed of hollow fibers modified with lithium-philic layers inside and outside the tube, and metallic lithium is filled into the interior and fiber skeleton of the fibers modified with lithium-philic layers inside and outside the tube on the basis of maintaining the original structural morphology of the carbonized cotton cloth.

[0010] To achieve the above objectives, the present invention also proposes the application of a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, and the carbon-based composite metal lithium negative electrode prepared by the above-mentioned preparation method or the above-mentioned carbon-based composite metal lithium negative electrode is applied to a lithium metal battery.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] The method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube provided by the present invention prepares a three-dimensional carbon-based current collector constructed with a hollow fiber modified with a lithium-philic layer inside and outside the tube. The manganese dioxide nanosheet arrays grown inside and outside the fiber significantly increase the wetting speed of molten lithium during the process of molten lithium infiltration; the hollow structure can provide space for the deposition of lithium, effectively alleviating the volume expansion; the manganese dioxide nanosheet arrays grown inside and outside the fiber promote the uniform deposition of lithium, inhibit the growth of dendrites, and improve the cycle stability and cycle life of the battery. Therefore, the three-dimensional carbon-based current collector of the present invention has the characteristics of large specific surface area, light weight, good conductivity and high mechanical strength, can effectively reduce current density and inhibit dendrite growth, and the three-dimensional skeleton can significantly alleviate the volume expansion of the lithium negative electrode. At the same time, the lithium-philicity of the carbon-based material is improved by the lithium-philic surface modification layer, and the uniform deposition of lithium is promoted. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0014] Figure 1 The SEM images of the carbonized cotton cloth prepared in Example 1 at 500 μm and 4 μm;

[0015] Figure 2 This is a SEM image of the carbonized cotton hollow fiber prepared in Example 1 at 2 μm;

[0016] Figure 3The SEM images of the carbonized cotton cloth grown with manganese dioxide nanosheet arrays prepared in Example 1 at 4 μm and 500 nm;

[0017] Figure 4 This is a SEM image of the carbonized cotton cloth hollow fiber grown with manganese dioxide nanosheet arrays prepared in Example 1 at 2 μm;

[0018] Figure 5 This is an electron transmission image of the fiber grown with manganese dioxide nanosheet arrays prepared in Example 1;

[0019] Figure 6 This is the XRD image of the carbonized cotton cloth with the manganese dioxide nanosheet array grown in Example 1;

[0020] Figure 7 The SEM images of the composite metal lithium negative electrode prepared in Example 1 at 200 μm and 20 μm;

[0021] Figure 8 This is a SEM picture of the composite metal lithium negative electrode hollow fiber filled with molten lithium at 2 μm prepared in Example 1;

[0022] Fig. 9 This is the XRD image of the composite metal lithium negative electrode prepared in Example 1;

[0023] Fig.10 The figure is a comparison chart of the cycle performance of a button battery using the composite metal lithium negative electrode prepared in Example 1 as the negative electrode and a button battery using a lithium sheet as the negative electrode;

[0024] Fig.11 A comparison chart of the rate performance of a button cell using the composite metal lithium negative electrode prepared in Example 1 as the negative electrode and a button cell using a lithium sheet as the negative electrode;

[0025] Fig.12 Cycling performance diagram of a laminated soft-pack battery using the composite metal lithium negative electrode prepared in Example 1 as the negative electrode;

[0026] Fig.13 Surface and cross-sectional SEM images of the carbon fiber cloth grown with manganese dioxide nanosheet arrays prepared in Comparative Example 1 at 2 μm.

[0027] Fig.14 The cycle performance of the button battery with the composite metal lithium negative electrode prepared in Comparative Example 1 as the negative electrode.

[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0031] Unless otherwise specified, all drugs / reagents used were commercially available.

[0032] The present invention provides a method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, which is characterized by comprising the following steps:

[0033] S1: placing cotton cloth in an inert atmosphere and calcining it to obtain carbonized cotton cloth;

[0034] S2: Under heating conditions, immersing the carbonized cotton cloth in a potassium permanganate acid solution, then taking it out, rinsing it with deionized water and vacuum drying it to obtain a carbonized cotton cloth with a manganese dioxide nanosheet array grown thereon;

[0035] S3: Carbonized cotton with manganese dioxide nanosheet arrays is placed on the surface of molten lithium metal. Under the action of capillary action and chemical reaction, the molten lithium metal infiltrates the entire carbonized cotton cloth, which is then taken out and the carbon-based composite lithium metal negative electrode is obtained after the molten lithium metal is cooled and solidified.

[0036] Preferably, in step S1, the cotton cloth is a cloth woven from cotton yarn using various weaving structures.

[0037] Preferably, in step S1, the inert atmosphere is argon or nitrogen.

[0038] Preferably, in step S1, the calcination temperature is 600-1200°C and the time is 1-2 hours. Too high a calcination temperature will affect the mechanical properties of the carbonized cotton cloth, resulting in a decrease in strength; too low a temperature will result in incomplete carbonization and poor conductivity.

[0039] Preferably, in step S2, the heating temperature is 70-80°C and the heating time is 10-120 minutes. If the reaction time is too short, the manganese dioxide nanosheets grown on the fiber will be uneven; if the reaction time is too long, the nanosheets will grow too much and form agglomerates, which will increase the proportion of inactive substances in the composite lithium negative electrode and reduce the specific surface area.

[0040] Preferably, in step S2, the acid in the potassium permanganate acidic solution is hydrochloric acid, sulfuric acid or nitric acid.

[0041] Preferably, in step S2, the molar ratio of potassium permanganate to hydrogen ions in the potassium permanganate acidic solution is 1:1 to 1.2. Acidic conditions can promote the decomposition of potassium permanganate to generate manganese dioxide.

[0042] Preferably, in step S3, the mass ratio of the molten metal lithium to the carbonized cotton cloth is 5 to 25: 1. The lithium metal surface loading of the carbon-based composite metal lithium negative electrode is controlled by controlling the ratio of the two.

[0043] Preferably, in step S3, the lithium metal surface loading of the carbon-based composite metal lithium negative electrode is 5 to 25 mg cm -2 Too high a lithium metal loading will lead to failure of the three-dimensional current collector.

[0044] The present invention also proposes a carbon-based composite metal lithium negative electrode with hollow carbon fibers modified with lithium-philic layers inside and outside the tube, which is prepared by the above-mentioned preparation method; the carbon-based composite metal lithium negative electrode is a three-dimensional carbon-based current collector constructed of hollow fibers modified with lithium-philic layers inside and outside the tube, and metal lithium is filled into the interior and fiber skeleton of the fibers modified with lithium-philic layers inside and outside the tube on the basis of maintaining the original structural morphology of the carbonized cotton cloth.

[0045] The present invention also proposes an application of a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with lithium-philic layers inside and outside the tube, and the carbon-based composite metal lithium negative electrode prepared by the above-mentioned preparation method or the above-mentioned carbon-based composite metal lithium negative electrode is applied to a lithium metal battery.

[0046] Example 1

[0047] This embodiment provides a method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with inner and outer lithium-philic layers, comprising:

[0048] S1: Place the cut cotton pieces in a tubular furnace, sinter at 900° C. for 2 hours in an argon atmosphere, and obtain carbonized cotton cloth after cooling in the furnace.

[0049] S2: 0.395 g of potassium permanganate, 0.07 mL of concentrated sulfuric acid and 50 mL of deionized water were mixed and stirred to obtain a potassium permanganate acid solution, and then a carbonized cotton cloth was placed so that it was completely immersed in the solution, and then the carbonized cotton cloth was taken out and rinsed with deionized water after being kept at 75° C. for 20 minutes, and then placed in a vacuum oven at 100° C. for 3 hours to obtain a carbonized cotton cloth with a manganese dioxide nanoarray grown thereon;

[0050] S3: Heat to 300°C in a glove box to melt the lithium sheet, then place the carbonized cotton with manganese dioxide grown on it on the molten metallic lithium. Under the action of capillary action and chemical reaction, the molten lithium infiltrates the entire carbonized cotton cloth, and then take out the molten lithium to solidify to obtain a composite metallic lithium negative electrode.

[0051] Figure 1 The SEM images of the carbonized cotton cloth obtained in step S1 of this embodiment at 500 μm and 4 μm are shown. It can be seen from the figure that the surface of the carbonized cotton cloth fiber is smooth and the overall woven structure is retained.

[0052] Figure 2 This is a SEM picture of the carbonized cotton cloth hollow fiber obtained in step S1 of this embodiment at 2 μm. It can be seen from the figure that the fiber of the carbonized cotton cloth has a hollow structure.

[0053] Figure 3 The SEM images of the carbonized cotton cloth grown with manganese dioxide nanosheet arrays prepared in step S2 of this embodiment at 4 μm and 500 nm show that the nanosheets grow vertically and uniformly on the fibers.

[0054] Figure 4 This is a SEM picture of the carbonized cotton cloth hollow fiber grown with manganese dioxide nanosheet arrays prepared in step S2 of this embodiment at 2 μm. It can be seen from the picture that manganese dioxide nanosheet arrays are grown on both the inner and outer surfaces of the hollow fiber.

[0055] Figure 5 This is an electron transmission image of the fiber grown with manganese dioxide nanosheet arrays obtained in step S2 of this embodiment, which further illustrates the growth of manganese dioxide nanosheets inside and outside the hollow fiber.

[0056] Figure 6 This is the XRD picture of the carbonized cotton cloth with the manganese dioxide nanosheet array grown in step S2 of this embodiment. The comparison with the standard card shows that the grown substance is manganese dioxide.

[0057] Figure 7 The SEM images of the composite metal lithium negative electrode prepared in step S3 of this embodiment at 200 μm and 20 μm show that lithium is filled into the fiber skeletons.

[0058] Figure 8 This is a SEM picture taken at 2 μm of the composite metal lithium negative electrode hollow fiber filled with molten lithium obtained in step S3 of this embodiment.

[0059] Fig. 9 This is the XRD picture of the composite metal lithium negative electrode obtained in step S3 of this embodiment. Compared with the standard card, it shows that in the process of melt infiltration of lithium, molten lithium and manganese dioxide undergo a chemical reaction to generate manganese, and this reaction greatly promotes the infiltration rate of molten lithium.

[0060] Fig.10 The following is a comparison chart of the cycle performance of the button battery with the composite metal lithium negative electrode as the negative electrode and the button battery with the lithium sheet as the negative electrode. At a charge and discharge rate of 0.5C, the button battery assembled with the composite metal lithium negative electrode has a capacity retention rate of up to 85.7% after 400 cycles, and an average coulomb efficiency of up to 99.8%, while the button battery assembled with the lithium sheet negative electrode has a capacity retention rate of only 30.4% after 400 cycles. The excellent cycle performance of the composite metal lithium negative electrode is due to the fact that the hollow fiber modified with internal and external lithium affinity plays a good role in alleviating volume expansion and inhibiting dendrite growth.

[0061] Fig.11 The figure is a comparison of the rate performance of the button battery with the composite metal lithium negative electrode as the negative electrode and the button battery with the lithium sheet as the negative electrode. It can be seen from the figure that at a low rate, the performance of the two negative electrodes is equivalent, but when the rate is increased to 3C, the discharge capacity of the button battery composed of the lithium sheet negative electrode is less than 100mAhg -1 , while the button battery composed of composite metal lithium negative electrode still has 112mAhg -1 , this result shows that the composite metal anode has good rate performance.

[0062] Fig.12 The cycle performance diagram of the laminated soft-pack battery with the composite metal lithium negative electrode prepared in this embodiment as the negative electrode is shown in Figure 1. At a rate of 0.5C, the initial discharge specific capacity can reach 145 mAhg -1 After 100 cycles, the capacity retention rate can reach 64.5%, and the Coulomb efficiency remains above 99.8%, with excellent cycle stability.

[0063] Example 2

[0064] This embodiment provides a method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with inner and outer lithium-philic layers, comprising:

[0065] S1: Place the cut cotton pieces in a tubular furnace, sinter at 1200° C. for 1 hour in a nitrogen atmosphere, and obtain carbonized cotton cloth after cooling in the furnace.

[0066] S2: 0.395 g of potassium permanganate, 0.21 mL of concentrated hydrochloric acid and 50 mL of deionized water were mixed and stirred to obtain a potassium permanganate acid solution, and then a carbonized cotton cloth was placed so that it was completely immersed in the solution, and then the carbonized cotton cloth was taken out and rinsed with deionized water after being kept at 80° C. for 60 min, and then placed in a vacuum oven and kept at 100° C. for 3 h to obtain a carbonized cotton cloth with a manganese dioxide nanoarray grown thereon;

[0067] S3: Heat to 300°C in a glove box to melt the lithium sheet, then place the carbonized cotton with manganese dioxide grown on it on the molten metallic lithium. Under the action of capillary action and chemical reaction, the molten lithium infiltrates the entire carbonized cotton cloth, and then take out the molten lithium to solidify to obtain a composite metallic lithium negative electrode.

[0068] Example 3

[0069] This embodiment provides a method for preparing a carbon-based composite metal lithium negative electrode of a hollow carbon fiber modified with inner and outer lithium-philic layers, comprising:

[0070] S1: The cotton cut into pieces is placed in a tubular furnace, sintered at 600° C. for two hours in an argon atmosphere, and then cooled in the furnace to obtain carbonized cotton cloth.

[0071] S2: 0.395 g potassium permanganate, 0.16 mL concentrated nitric acid and 50 mL deionized water were mixed and stirred to obtain a potassium permanganate acid solution, and then a carbonized cotton cloth was placed so that it was completely immersed in the solution, and the carbonized cotton cloth was kept at 70° C. for 120 min, then taken out and rinsed with deionized water, and then placed in a vacuum oven at 100° C. for 3 h to obtain a carbonized cotton cloth with a manganese dioxide nanoarray grown thereon;

[0072] S3: Heat to 300°C in a glove box to melt the lithium sheet, then place the carbonized cotton with manganese dioxide grown on it on the molten metallic lithium. Under the action of capillary action and chemical reaction, the molten lithium infiltrates the entire carbonized cotton cloth, and then take out the molten lithium to solidify to obtain a composite metallic lithium negative electrode.

[0073] Comparative Example 1

[0074] This comparative example provides a carbon-based composite metal lithium negative electrode with a lithium-philic layer modified solid carbon fiber, comprising the following steps:

[0075] S1: cutting the commercial carbon fiber cloth into suitable sizes and shapes, ultrasonically cleaning and drying the carbon fiber cloth with anhydrous ethanol and deionized water respectively, and then adding the dried carbon fiber cloth into a sulfuric acid solution for hydrothermal reaction to obtain an acidified carbon fiber cloth;

[0076] S2: Potassium permanganate, concentrated sulfuric acid and deionized water are prepared into a mixed solution, heated and stirred in a water bath to completely dissolve the potassium permanganate, and then the acidified carbon fiber cloth is placed in the mixed solution, kept warm and stirred, ultrasonically cleaned, and vacuum dried to obtain a carbon fiber cloth loaded with manganese dioxide nanosheet arrays;

[0077] S3: Heat the metallic lithium to a molten state, immerse one end of the carbon fiber cloth loaded with the manganese dioxide nanosheet array into the molten metallic lithium, and obtain a composite metallic lithium negative electrode through capillary action.

[0078] Fig.13The surface and cross-sectional SEM images at 2 μm of the carbon fiber cloth grown with manganese dioxide nanosheet arrays prepared in Comparative Example 1. As can be seen from the figure, the fibers of the carbon fiber cloth are solid structures. Compared with the carbonized cotton cloth where the nanosheets are distributed on the inner and outer surfaces of the hollow fibers, the nanosheets are only distributed on the outer surface of the carbon fiber cloth fibers.

[0079] Fig.14 The cycle performance of the button cell with the composite metal lithium negative electrode as the negative electrode prepared in Comparative Example 1. After 150 cycles, the discharge capacity of the battery decayed rapidly. Fig.10 There is a huge gap in the cycle performance compared with Example 1. This result shows that hollow carbon fibers have a better ability to improve the performance of lithium metal negative electrodes than solid carbon fibers.

[0080] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a carbon-based composite metal lithium negative electrode with a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, characterized in that: The following steps are involved: S1: placing cotton cloth in an inert atmosphere and calcining it to obtain carbonized cotton cloth; S2: immersing the carbonized cotton cloth in a potassium permanganate acidic solution under heating conditions, then taking it out, rinsing it with deionized water, and vacuum drying it to obtain a carbonized cotton cloth with a manganese dioxide nanosheet array grown thereon; S3: Carbonized cotton with manganese dioxide nanosheet arrays is placed on the surface of molten lithium metal. Under the action of capillary action and chemical reaction, the molten lithium metal infiltrates the entire carbonized cotton cloth. It is then taken out and the molten lithium metal is cooled and solidified to obtain a carbon-based composite lithium metal negative electrode.

2. The preparation method according to claim 1, wherein In step S1 , the cotton cloth is a cloth woven from cotton yarn using various weaving structures.

3. The preparation method according to claim 1, wherein In step S1 , the inert atmosphere is argon or nitrogen.

4. The preparation method according to claim 1, wherein In step S1, the calcination temperature is 600-1200° C. and the calcination time is 1-2 hours.

5. The preparation method according to claim 1, wherein In step S2, the heating temperature is 70-80°C and the heating time is 10-120 minutes.

6. The preparation method according to claim 1, wherein In step S2, the acid in the potassium permanganate acidic solution is hydrochloric acid, sulfuric acid or nitric acid.

7. The preparation method according to claim 1, wherein In step S2, the molar ratio of potassium permanganate to hydrogen ions in the potassium permanganate acidic solution is 1:1 to 1.

2.

8. The preparation method according to claim 1, wherein In step S3, the lithium metal surface loading of the carbon-based composite metal lithium negative electrode is 5 to 25 mg cm -2 .

9. A carbon-based composite metal lithium negative electrode with a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8; the carbon-based composite metal lithium negative electrode is a three-dimensional carbon-based current collector constructed of hollow fibers modified with lithium-philic layers inside and outside the tube. On the basis of maintaining the original structural morphology of the carbonized cotton cloth, metallic lithium is filled into the interior and fiber skeleton of the fibers modified with lithium-philic layers inside and outside.

10. Application of a carbon-based composite metal lithium negative electrode with a hollow carbon fiber modified with a lithium-philic layer inside and outside the tube, characterized in that: The carbon-based composite metal lithium negative electrode prepared by the preparation method according to any one of claims 1 to 8 or the carbon-based composite metal lithium negative electrode according to claim 9 is applied to a lithium metal battery.

Citation Information

Patent Citations

  • Three-dimensional current collector for metal secondary battery anode and preparation and application thereof

    CN106898778A

  • Preparation method of composite lithium metal negative electrode and battery containing composite lithium metal negative electrode

    CN111106310A

  • Three-dimensional carbon-based composite metal lithium negative electrode and preparation method and application thereof

    CN116504928A

  • Composite carbon fibers for lithium battery and preparation thereof

    KR1019980059070A

Cited By

  • Femtosecond laser additive manufacturing method for lithium-loving microstructure on surface of copper foil current collector for metal lithium negative electrode