Preparation method and application of vanadium tetrasulfide-based lithium-sulfur battery positive electrode

By mixing vanadium tetrasulfide with carbon-based material to form a nanorod structure and used for the positive electrode of lithium-sulfur battery, the problems of poor conductivity and multi-step conversion reaction of lithium-sulfur battery are solved, and higher rate performance and cycle stability are achieved. Reduced preparation costs.

CN118943305AActive Publication Date: 2024-11-12HEFEI UNIV OF TECH

Patent Information

Application Number
CN202411006337.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The poor electron conductivity and multi-step conversion reaction of the positive electrode of lithium-sulfur battery lead to insufficient electron transmission performance, limiting the high-rate performance of the battery, and the addition of catalytic materials in traditional methods increases costs and is difficult to effectively integrate.

Method used

Vanadium tetrasulfide (VS4) is used as the positive electrode material of lithium sulfur battery. By mixing with carbon-based materials and reacting in an autoclave, a nanorod structure is formed, which increases the reaction area and improves conductivity, and suppresses the shuttle effect of lithium polysulfide.

Benefits of technology

It improves the rate performance and cycle stability of lithium-sulfur batteries, reduces the production cost, and is simple in structure and easy to produce in quantified production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004963107130000011
    Figure HDA0004963107130000011
  • Figure HDA0004963107130000012
    Figure HDA0004963107130000012
  • Figure HDA0004963107130000021
    Figure HDA0004963107130000021
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a vanadium tetrasulfide-based lithium-sulfur battery positive electrode, which comprises the following steps: taking a vanadium tetrasulfide-based material as a sulfur source in the lithium-sulfur battery positive electrode, uniformly mixing the vanadium tetrasulfide-based material with conductive carbon black, and coating on a current collector to prepare the positive electrode for the lithium-sulfur battery. The positive electrode is simple and stable in structure, and compared with a traditional sulfur positive electrode, the positive electrode of the lithium-sulfur battery prepared by using the vanadium tetrasulfide-based material as the sulfur source has better conductivity and stronger lithium polysulfide adsorption and catalysis capability, has a good inhibition effect on a shuttle effect, provides more active sites, and has a good application prospect. The catalytic conversion reaction of lithium polysulfide is promoted, and excellent electrochemical characteristics are shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical energy storage, and in particular relates to a method for preparing a positive electrode of a vanadium tetrasulfide-based lithium-sulfur battery and an application thereof. Background Art

[0002] In the context of the rapid development of electric vehicles, people have gradually realized that lithium-ion batteries may not be able to meet the growing demand for high energy storage in the future. In contrast, lithium-sulfur batteries have a high theoretical specific capacity (1675mAh g -1 ) and energy density (2600Wh kg -1 ), good stability, abundant sulfur resources and environmental friendliness have attracted much attention. However, as a cathode material for lithium-sulfur batteries, sulfur (S) has poor electronic conductivity, resulting in insufficient electron transport performance of the sulfur cathode, which limits the high-rate performance of the battery. At the same time, there are multi-step conversion reactions in the sulfur cathode, and a variety of lithium polysulfide (LiPSs) intermediates will be produced during the reaction. These LiPSs have high solubility in the electrolyte, which will lead to a "shuttle effect" under the action of the electric field, leading to the loss of cathode sulfur substances and slow electrochemical kinetics. At the same time, it also causes volume changes in the cathode material, which will destroy the battery electrode structure and seriously affect the cycle life and stability of the battery. In order to overcome these problems, researchers have carried out a lot of research on the cathode of lithium-sulfur batteries. Among them, by introducing polar material catalysts to modify the sulfur cathode, the adsorption and conversion process of lithium ions can be effectively promoted, thereby inhibiting the shuttle effect. Transition metal sulfides have important potential in sulfur cathode modification due to their strong sulfur ion capture ability and excellent binding properties with lithium ions. However, the addition of a large amount of catalytic materials to the positive electrode in addition to the sulfur source not only increases the cost, but also poses a challenge in how to effectively integrate the catalytic materials into the electrode structure. Vanadium tetrasulfide (VS4) not only has the characteristics of strong adsorption and high catalytic activity of transition metal sulfides, but also has a high sulfur content, making it possible to directly serve as a sulfur source in the positive electrode of lithium-sulfur batteries. VS4 has a unique one-dimensional linear chain structure consisting of S2 2- The dimer is composed of two adjacent V atoms, and there is a weak van der Waals force between its parallel one-dimensional chains, which not only provides a larger open channel for lithium ion diffusion, but also enhances the adsorption and catalytic ability of LiPSs, and better inhibits the "shuttle effect" of LiPSs. Therefore, it is of great significance to develop VS4 as a new type of lithium-sulfur battery positive electrode material. Summary of the invention

[0003] In order to solve the problems of poor conductivity of sulfur in the positive electrode of traditional lithium-sulfur batteries and large volume changes during the reaction, the present invention aims to develop a method for preparing a vanadium tetrasulfide-based lithium-sulfur battery positive electrode with low cost, simple preparation process, simple structure and suitable for mass production, and its application in lithium-sulfur batteries, which can effectively reduce the LiPSs shuttle effect, accelerate redox kinetics, improve coulombic efficiency, and increase sulfur utilization, ultimately achieving the purpose of improving the rate performance of lithium-sulfur batteries and enhancing cycle stability.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] A method for preparing a vanadium tetrasulfide-based lithium-sulfur battery positive electrode comprises the following steps:

[0006] Step 1, ultrasonically disperse 0-50 mg of carbon-based material in 15-20 mL of deionized water, then add 2-3 mmol of vanadium source, seal and place in a 50-70° C. water bath and stir for 0.5-1 h to obtain solution A;

[0007] Step 2, add 8-12 mmol of sulfur source to 15-30 mL of ethylene glycol, stir for 10-30 min, and obtain solution B;

[0008] Step 3, after mixing solution A and solution B, stirring at room temperature for 0.5-1h, pouring the obtained mixed solution into a high-pressure reactor, and reacting at a temperature of 150-200°C for 20-30h to obtain an initial product;

[0009] Step 4, centrifugally washing the initial product and then drying it in a vacuum drying oven to obtain an intermediate product;

[0010] Step 5: Evenly mix the intermediate product, carbon black, polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP), and evenly coat the resulting slurry on one side of the current collector, and then dry it in a vacuum drying oven to obtain the target product, vanadium tetrasulfide-based lithium-sulfur battery positive electrode.

[0011] Preferably, in step 1, the carbon-based material is one of graphene oxide (GO), carbon nanotubes (CNT) and carbon spheres (HCS).

[0012] Preferably, in step 1, the vanadium source is ammonium metavanadate.

[0013] Preferably, in step 2, the sulfur source is at least one of thioacetamide, thiourea and sodium thiosulfate.

[0014] Preferably, in step 4, the cleaning is performed using deionized water and anhydrous ethanol in sequence.

[0015] Preferably, in step 5, the carbon black material is at least one of acetylene black (AB) and Ketjen black (KB).

[0016] Preferably, in step 5, the current collector is one of aluminum foil, carbon fiber paper (CFP) and carbon fiber cloth (CFC).

[0017] Preferably, in step 5, the mass ratio of the intermediate product, carbon black and PVDF is 6-7:2-3:1.

[0018] The vanadium tetrasulfide-based lithium-sulfur battery positive electrode prepared by the present invention can be used as a positive electrode in a lithium-sulfur battery.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] 1. The vanadium tetrasulfide-based lithium-sulfur battery positive electrode prepared by the preparation method of the present invention has a simple structure, stable electrode properties and excellent electrochemical characteristics.

[0021] 2. The preparation method of the vanadium tetrasulfide-based lithium-sulfur battery positive electrode provided by the present invention is to use the vanadium tetrasulfide-based material as the sulfur source in the lithium-sulfur battery positive electrode, evenly mix it with conductive carbon black, and then coat it on the current collector to prepare the positive electrode for the lithium-sulfur battery. The lithium-sulfur battery positive electrode prepared using the vanadium tetrasulfide-based material as the sulfur source has better conductivity, stronger lithium polysulfide adsorption and catalytic ability than the traditional positive electrode, has a good inhibitory effect on the "shuttle effect", promotes the conversion of LiPSs, and provides more active sites, showing excellent electrochemical properties.

[0022] 3. When preparing VS4, the present invention adds carbon-based materials to disperse the originally agglomerated VS4 nanospheres into VS4 nanorods, thereby increasing the reaction area and providing more active sites. At the same time, the introduction of carbon-based materials can also improve the conductivity of the VS4 positive electrode and greatly accelerate the diffusion rate of lithium ions.

[0023] 4. The lithium-sulfur battery assembled with the vanadium tetrasulfide-based lithium-sulfur battery positive electrode prepared by the present invention exhibits excellent rate performance and excellent long-term cycle life at high current density.

[0024] 5. The preparation process of the present invention is simple, the preparation cost is low, and it is easy to synthesize in large quantities and promote. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The SEM images of the intermediate products obtained in Examples 1 and 2 of the present invention are as follows: Figure 1 a and b in the figure correspond to VS4 and VS4@rGO, respectively.

[0026] Figure 2TEM images of the intermediate products obtained in Examples 1 and 2 of the present invention, Figure 2 a and b in the figure correspond to VS4 and VS4@rGO, respectively.

[0027] Figure 3 The XPS diagram of the intermediate products obtained in Example 1 and Example 2 of the present invention is shown in FIG. Figure 3 a and b in the figure correspond to the V2p spectrum and S2p spectrum, respectively.

[0028] Figure 4 The XRD diagrams of the intermediate products obtained in Examples 1 and 2 of the present invention are shown in FIG.

[0029] Figure 5 The Raman spectra of the intermediate products obtained in Examples 1 and 2 of the present invention are shown.

[0030] Figure 6 The variable rate performance curves of button batteries assembled from samples 1 to 4 prepared in Examples 1 to 4 of the present invention.

[0031] Figure 7 Long cycle test curves of button batteries assembled from samples 1 to 4 prepared in Examples 1 to 4 of the present invention at a current density of 2C.

[0032] Figure 8 Long cycle test curve of the button battery assembled with Sample 4 prepared in Example 4 of the present invention at a current density of 4C.

[0033] Fig. 9 The charge and discharge curves of the button battery assembled from Sample 4 prepared in Example 4 of the present invention at a current density of 4C. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0035] In the following process steps of the embodiments, unless otherwise specified, all are carried out at room temperature.

[0036] Example 1

[0037] In this embodiment, the VS4 / Al positive electrode is prepared according to the following steps:

[0038] Step 1: Add 2 mmol of ammonium metavanadate into 15 mL of deionized water, seal the beaker with tin foil, place it in a 60° C. water bath and stir for 45 min to obtain solution A.

[0039] Step 2: Add 10 mmol of thioacetamide to 20 mL of ethylene glycol and stir for 20 min to obtain solution B.

[0040] Step 3: After mixing solution A and solution B, stir at room temperature for 1 hour, pour the obtained mixed solution into a high-pressure reactor, and react at a temperature of 160° C. for 24 hours to obtain an initial product.

[0041] Step 4: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 50° C. and dried for 12 h to obtain an intermediate product VS4.

[0042] Step 5: grind the intermediate product and acetylene black in an agate mortar, then add PVDF and NMP and mix and stir evenly, wherein the mass ratio of the intermediate product, acetylene black and PVDF is 6:3:1. Then, coat the obtained slurry evenly on aluminum foil with an automatic coating machine and dry it in a vacuum drying oven at 60°C for 12 hours to obtain the target product VS4 / Al positive electrode, which is recorded as sample 1.

[0043] Example 2

[0044] In this example, the VS4@rGO / Al cathode was prepared according to the following steps:

[0045] Step 1: Ultrasonic disperse 45 mg of GO in 15 mL of deionized water, then add 2 mmol of ammonium metavanadate, seal the beaker with tin foil, place it in a 60°C water bath and stir for 45 min to obtain solution A.

[0046] Step 2: Add 10 mmol of thioacetamide to 20 mL of ethylene glycol and stir for 20 min to obtain solution B.

[0047] Step 3: After mixing solution A and solution B, stir at room temperature for 1 hour, pour the obtained mixed solution into a high-pressure reactor, and react at a temperature of 160° C. for 24 hours to obtain an initial product.

[0048] Step 4: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 50°C and dried for 12 hours to obtain the intermediate product VS4@rGO.

[0049] Step 5: Grind the intermediate product and acetylene black in an agate mortar, then add PVDF and NMP and mix well, wherein the mass ratio of the intermediate product, acetylene black and PVDF is 6:3:1. Then, the obtained slurry is evenly coated on aluminum foil with an automatic coating machine and dried in a vacuum drying oven at 60°C for 12 hours to obtain the target product VS4@rGO / Al positive electrode, which is recorded as sample 2.

[0050] Example 3

[0051] In this embodiment, the S / Al positive electrode is prepared according to the following steps:

[0052] Step 1: add sublimated sulfur (S) and acetylene black into an agate mortar for grinding, wherein the mass ratio of S to acetylene black is 6:3, then add into a small glass bottle, seal it in a glove box and place it in a reactor.

[0053] Step 2: Place it in an oven at 155.5°C and heat for 12 hours to obtain the intermediate product S / C.

[0054] Step 3: grind the intermediate product in an agate mortar, then add PVDF and NMP and mix and stir evenly, wherein the mass ratio of the intermediate product to PVDF is 9:1. Then, coat the obtained slurry evenly on aluminum foil with an automatic coating machine and dry it in a vacuum drying oven at 60°C for 12 hours to obtain the target product S / Al positive electrode, which is recorded as sample 3.

[0055] Example 4

[0056] In this example, the VS4@rGO / CFP cathode was prepared according to the following steps:

[0057] Step 1: Ultrasonic disperse 45 mg of GO in 15 mL of deionized water, then add 2 mmol of ammonium metavanadate, seal the beaker with tin foil, place it in a 60°C water bath and stir for 45 min to obtain solution A.

[0058] Step 2: Add 10 mmol of thioacetamide to 20 mL of ethylene glycol and stir for 20 min to obtain solution B.

[0059] Step 3: After mixing solution A and solution B, stir at room temperature for 1 hour, pour the obtained mixed solution into a high-pressure reactor, and react at a temperature of 160° C. for 24 hours to obtain an initial product.

[0060] Step 4: After the initial product is washed by centrifugation, it is placed in a vacuum drying oven at 50°C and dried for 12 hours to obtain the intermediate product VS4@rGO.

[0061] Step 5: Grind the intermediate product and acetylene black in an agate mortar, then add PVDF and NMP and mix well, wherein the mass ratio of the intermediate product, acetylene black and PVDF is 6:3:1. Then, the obtained slurry is evenly coated on the carbon fiber paper CFP with an automatic coating machine and dried in a vacuum drying oven at 60°C for 12 hours to obtain the target product VS4@rGO / CFP positive electrode, which is recorded as sample 4.

[0062] Figure 1 The following are SEM images of the intermediate products obtained in Example 1 and Example 2. Figure 1 a and b in correspond to VS4 material, Figure 1Figures c and d in the figure correspond to VS4@rGO materials. As shown in Figures a and b, the VS4 material presents a nanosphere morphology. However, as shown in Figures c and d, after the introduction of rGO, VS4 did not form a nanosphere morphology, but showed nanorods with a length of 200-400nm and a diameter of 50-100nm, and were uniformly attached to the rGO surface, indicating that these nanospheres are formed by stacking nanorods.

[0063] Figure 2 TEM images of the intermediate products obtained in Example 1 and Example 2, Figure 2 The a in corresponds to VS4 material, Figure 2 Figure b corresponds to VS4@rGO material. Figures a and b show similar results to those obtained by SEM. After adding rGO, VS4 is dispersed from nanospheres to nanorods and is evenly distributed on rGO.

[0064] Figure 3 The XPS diagram of the intermediate products obtained in Example 1 and Example 2, Figure 3 a and b correspond to the V 2p spectrum and S2p spectrum of the sample, respectively. As shown in Figure a, the number and position of the two peaks are basically the same. In addition, it can be clearly seen that the V 4+ The pair of prominent double peaks at higher binding energies of 524.2 eV and 516.5 eV are the same as those of VS4 in the valence state of vanadium, and there are two more peaks at 521.5 eV and 513.9 eV corresponding to V 2+ The peak value, V 2+ The presence of indicates the presence of sulfur vacancies in the sample. Figure b shows the S2p spectra of the VS4 sample and VS4@rGO sample. There are two (S2) 2- 2p 3 / 2 and 2p 1 / 2 The peak is caused by spin-orbit, which is also consistent with the valence state of sulfur in VS4.

[0065] Figure 4The XRD diagram of the intermediate product obtained in Example 1 and Example 2. The characteristic peaks of the VS4 and VS4@rGO samples obtained by the test correspond to the peaks of the standard single crystal oblique VS4 (JCPDS 87-0603), which indicates that the obtained sample is a VS4 with a pure phase monoclinic structure. The two very sharp main diffraction peaks at 15.7° and 17° correspond to the (110) and (020) crystal planes of the monoclinic phase VS4. The sharp main diffraction peaks also indicate that the sample has good crystallinity. The peaks at 28.1°, 30°, 36.3°, 40.6° and 44.1° correspond to the (-202), (004), (114), (-224) and (134) crystal planes of VS4, respectively. In addition, a broad diffraction peak at about 24° can be seen in the VS4@rGO sample, which comes from rGO and corresponds to the (002) plane of carbon.

[0066] Figure 5 The Raman spectra of the intermediate products obtained in Example 1 and Example 2 are shown in Figure 1. It can be clearly seen that the peaks at 197, 220, 276, 293, 351 and 560 cm -1 There are six Raman peaks. Among them, the peaks at 197 and 220 cm -1 The two peaks at 276 cm-1 are derived from the vibration of VS bond stretching. -1 The peaks at 293 and 560 cm-1 are from the vibration of the VS bond bending mode. -1 The two peaks at 351cm come from the vibration of SS bond deformation and stretching. -1 There is also a more obvious peak caused by the symmetrical vibration of VS4.

[0067] In order to characterize the electrochemical performance of the positive electrode obtained in the above example, the following test was performed.

[0068] Step 1: Take the positive electrode prepared in each embodiment as the positive electrode of the lithium-sulfur battery.

[0069] Step 2: Use metallic lithium as the negative electrode of the battery, glass fiber separator (Celgard 2400) as the separator, 1M LITFSI (bis(trifluoromethanesulfonyl)imide) dissolved in a DOL / DME mixed solution with a volume ratio of 1:1 and add 1wt% LiNO3 as the electrolyte, and assemble a CR2032 button battery in an inflatable glove box (Etelux Lab 2000, O2<0.1ppm, H2O<0.1ppm).

[0070] Step 3: Use Neware's BTS2300 charge and discharge tester to perform a battery charge and discharge test on the assembled button battery in a voltage window of 1.7-2.8V.

[0071] Figure 6The variable rate performance curves of button cells assembled from sample 1 (VS4 / Al), sample 2 (VS4@rGO / Al), sample 3 (S / Al) and sample 4 (VS4@rGO / CFP). It can be seen that at the current density of 0.2C-4C, the battery assembled from sample 4 has 1643, 1281, 1059, 835, 672, 547 mAh g -1 The specific capacity can also be restored to 1430 mAh g when gradually restored to 0.2C. -1 The high stable specific capacity and excellent cycle reversibility far exceed those of other samples.

[0072] Figure 7 Long cycle test curves of button cells assembled from sample 1 (VS4 / Al), sample 2 (VS4@rGO / Al), sample 3 (S / Al) and sample 4 (VS4@rGO / CFP) at 2C current density. The initial capacity of the battery assembled from sample 4 is 797 mAh g -1 After 300 cycles, it can still maintain 512mAh g -1 The high specific capacity is much higher than that of batteries with other types of positive electrodes.

[0073] Figure 8 This is the long cycle test curve of the button battery assembled with sample 4 (VS4@rGO / CFP) at a current density of 4C. The battery assembled with sample 4 can be cycled continuously for 1000 cycles at 4C and can still maintain 281mAh g after the cycle. -1 High specific capacity.

[0074] Fig. 9 The charge and discharge curves of the button cell assembled with sample 4 (VS4@rGO / CFP) at a current density of 4C. The charge and discharge curves of the battery assembled with sample 4 at the 1st, 10th, 100th and 1000th cycles at 4C show that the charge and discharge curves of the first 100 cycles are basically the same and have high stability, while the discharge specific capacity of the battery gradually begins to decrease from the 100th to the 1000th cycle. This may be due to the continuous change in the volume of the positive electrode under long-term high-current charge and discharge cycles, and the deposition of a small amount of lithium polysulfide on the surface of the positive electrode, which weakens the activity of the surface of the positive electrode material and thus affects the performance of the battery.

[0075] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a vanadium tetrasulfide-based lithium-sulfur battery positive electrode, characterized in that: The steps include: Step 1, ultrasonically disperse 0-50 mg of carbon-based material in 15-20 mL of deionized water, then add 2-3 mmol of vanadium source, seal and place in a 50-70° C. water bath and stir for 0.5-1 h to obtain solution A; Step 2, add 8-12 mmol of sulfur source to 15-30 mL of ethylene glycol, stir for 10-30 min, and obtain solution B; Step 3, after mixing solution A and solution B, stirring at room temperature for 0.5-1h, pouring the obtained mixed solution into a high-pressure reactor, and reacting at a temperature of 150-200°C for 20-30h to obtain an initial product; Step 4, centrifugally washing the initial product and then drying it in a vacuum drying oven to obtain an intermediate product; Step 5: Evenly mix the intermediate product, carbon black, polyvinylidene fluoride and N-methylpyrrolidone, and evenly coat the obtained slurry on one side of the current collector, and then dry it in a vacuum drying oven to obtain the target product, vanadium tetrasulfide-based lithium-sulfur battery positive electrode.

2. The preparation method according to claim 1, characterized in that: In step 1, the carbon-based material is one of graphene oxide, carbon nanotubes and carbon spheres.

3. The preparation method according to claim 1, characterized in that: In step 1, the vanadium source is ammonium metavanadate.

4. The preparation method according to claim 1, characterized in that: In step 2, the sulfur source is at least one of thioacetamide, thiourea and sodium thiosulfate.

5. The preparation method according to claim 1, characterized in that: In step 4, the cleaning is performed by sequentially using deionized water and anhydrous ethanol.

6. The preparation method according to claim 1, characterized in that: In step 5, the carbon black material is at least one of acetylene black and Ketjen black.

7. The preparation method according to claim 1, characterized in that: In step 5, the current collector is one of aluminum foil, carbon fiber paper and carbon fiber cloth.

8. The preparation method according to claim 1, characterized in that: In step 5, the mass ratio of the intermediate product, carbon black and polyvinylidene fluoride is 6-7:2-3:

1.

9. A vanadium tetrasulfide-based lithium-sulfur battery positive electrode prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the vanadium tetrasulfide-based lithium-sulfur battery positive electrode according to claim 9 in a lithium-sulfur battery.

Citation Information

Patent Citations

  • One-step in-situ preparation method of rGO / VS4 / S compound as lithium sulfur battery cathode material

    CN109585828A

  • Lithium-sulfur battery positive electrode composite material with high active substance content as well as preparation method and application thereof

    CN111354931A

  • VS4 / hierarchical pore graphitized carbon composite material and preparation method thereof, positive electrode material, positive plate, lithium-sulfur battery cell and lithium-sulfur battery pack

    CN112786845A

  • VS4-graphene aerogel composite material, preparation method and application

    CN113611830A

  • AU2020101299A4

Cited By

  • MnIn2S4atVS4 heterojunction photocatalyst as well as preparation method and application thereof

    CN121016791A