Three-dimensional graded reticular metal oxide / carbon composite material as well as preparation method and application thereof

By using three-dimensional graded mesh metal oxide/carbon composite materials in zinc ion batteries to form a conductive network, the problems of poor conductivity and short cycle life of vanadium-based positive electrode materials are solved, and high capacity and long life battery performance is achieved.

CN118943309AActive Publication Date: 2024-11-12SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI

Patent Information

Application Number
CN202310521928.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The existing vanadium-based positive electrode materials have problems such as poor conductivity, short cycle life and serious capacity attenuation in zinc-ion batteries. The increase in the surface area of ​​the composite material makes it difficult to suppress the dissolution of vanadium ions, and the thermal stability is unbalanced, which affects the battery life.

Method used

Using three-dimensional graded mesh metal oxide/carbon composite materials, the metal oxide active material covering the carbon shell is interwoven with the highly conductive carbon skeleton to form a conductive network, and is prepared by hydrothermal reaction and calcination to form multi-layer and multi-layer The conductive structure of the dimension inhibits the dissolution of vanadium ions and improves electrochemical properties.

Benefits of technology

It significantly improves the conductivity and ion diffusion rate of the battery, extends the cycle life, weakens the battery capacity attenuation, and achieves high-capacity and long-life zinc ion battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943309A_ABST
    Figure CN118943309A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional graded reticular metal oxide / carbon composite material as well as a preparation method and application thereof. The three-dimensional graded net-shaped metal oxide / carbon composite material comprises a metal oxide active material coated with a carbon shell layer and a high-conductivity carbon skeleton, and the metal oxide active material coated with the carbon shell layer and the high-conductivity carbon skeleton are interwoven to form a three-dimensional graded conductive net-shaped structure. The three-dimensional graded net-shaped metal oxide / carbon composite material provided by the invention is used as a positive electrode active material for the zinc ion battery, the battery performance can be remarkably improved, firstly, the conductivity of the whole material is improved and the reaction area of an electrolyte and an electrode is increased by forming a three-dimensional conductive network, and the material has a relatively high ion diffusion rate; the carbon layer wraps the metal oxide due to the layered structure, so that the dissolution of transition metal ions is inhibited, the capacity attenuation of the battery is greatly weakened, and the cycle life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a metal oxide / carbon composite material, in particular to a three-dimensional hierarchical mesh metal oxide / carbon composite material and a preparation method thereof, as well as an application thereof, belonging to the technical field of nanomaterials. Background Art

[0002] As people's demand for energy grows, low-cost and high-safety zinc-ion batteries have great development potential and are expected to be used in various large-scale energy storage facilities such as microgrids, solar energy and wind energy. With an ultra-high global average production of 502,000 tons and an extremely low metal price of $0.2 / kg, zinc metal has an undisputed cost advantage among various ion batteries. Therefore, it is urgent to find an ideal positive electrode material to match it with high-capacity and long-cycle zinc-ion batteries.

[0003] At present, the positive electrode materials for zinc-ion batteries on the market are divided into four categories: vanadium-based, manganese-based, Prussian blue analogs and organic positive electrodes. Among them, manganese-based and Prussian blue analogs are difficult to apply in the industry due to their poor rate performance and low specific capacity, while the research on organic positive electrodes is still in the early stages of development and the technology is not mature enough. However, vanadium-based has an ultra-high theoretical specific capacity of 589mAh / g, which has attracted widespread attention. Vanadium ions have multi-electron reactions in the charge and discharge cycle. 5+ / V 3+ The valence state changes, and no matter which valence state it is in, it has a stable crystal structure. However, some troubling problems were found in the subsequent research process, such as poor material conductivity, insufficient cycle life, and serious capacity attenuation. Therefore, domestic and foreign researchers have made a series of achievements in response to these problems, including improving the interlayer spacing of vanadium pentoxide by introducing metal ions to increase capacity, but because the crystal structure is changed, its thermal stability is also affected to a certain extent, and the battery life is difficult to meet people's satisfaction; the other is to compound with carbon materials to improve the conductivity of metal oxides, but because the surface area of ​​the composite material increases, the electrolyte and vanadium pentoxide have more contact area, and the dissolution of vanadium ions cannot be suppressed. Moreover, in current research, most vanadium-based positive electrode materials are modified by introducing metal cations, but they have a certain negative effect on the inherent crystal structure of vanadium oxygen bond formation. Even if the capacity is slightly increased, its thermal stability is in an unbalanced state, so that the life cannot be guaranteed, and the positive electrode dissolution phenomenon is not suppressed. Therefore, how to design a reasonable three-dimensional hierarchical conductive composite material is still a huge challenge. Summary of the invention

[0004] The main purpose of the present invention is to provide a three-dimensional hierarchical network metal oxide / carbon composite material and a preparation method thereof to overcome the deficiencies in the prior art.

[0005] Another object of the present invention is to provide an application of the three-dimensional hierarchical network metal oxide / carbon composite material in the preparation of electrode materials.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a three-dimensional hierarchical network metal oxide / carbon composite material, which includes: a metal oxide active material coated with a carbon shell layer and a highly conductive carbon skeleton, wherein the metal oxide active material coated with the carbon shell layer and the highly conductive carbon skeleton are interwoven to form a three-dimensional hierarchical conductive network structure.

[0008] The embodiment of the present invention also provides a method for preparing a three-dimensional hierarchical network metal oxide / carbon composite material, which comprises:

[0009] Providing a first solution comprising a highly conductive carbon framework material;

[0010] Providing a second solution comprising a transition metal oxide precursor, an organic solvent, and a carbon source (including a carbon skeleton and a carbon shell source);

[0011] The first solution and the second solution are mixed, subjected to a hydrothermal reaction, and freeze-dried to obtain a three-dimensional carbon skeleton framework to obtain a precursor material;

[0012] The precursor material is calcined to obtain a three-dimensional hierarchical network metal oxide / carbon composite material.

[0013] The embodiment of the present invention also provides the use of the aforementioned three-dimensional hierarchical network metal oxide / carbon composite material in the preparation of electrode materials.

[0014] Correspondingly, an embodiment of the present invention further provides a positive electrode for a zinc ion battery, comprising a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is the aforementioned three-dimensional hierarchical network metal oxide / carbon composite material.

[0015] The embodiment of the present invention further provides a zinc ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode adopts the above-mentioned positive electrode of the zinc ion battery.

[0016] Compared with the prior art, the beneficial effects of the present invention are at least:

[0017] The three-dimensional hierarchical network metal oxide / carbon composite material provided by the present invention is used as a positive electrode active material for zinc ion batteries, which can significantly improve the battery performance. First, the conductivity of the overall material is improved and the reaction area of ​​the electrolyte and the electrode is increased by forming a three-dimensional conductive network, and the ion diffusion rate is increased, so that the battery capacity is improved. Then, the layered structure allows the carbon layer to wrap the metal oxide, inhibiting the dissolution of transition metal ions, thereby greatly reducing the battery capacity attenuation and extending the cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1a and Figure 1b is a SEM image of vanadium pentoxide (V2O5) prepared in Comparative Example 1;

[0020] Figure 1c and Figure 1d is a SEM image of the three-dimensional hierarchical network structure of the vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) prepared in Example 1 of the present invention;

[0021] Figure 2a and Figure 2b is a TEM image of the carbon coating structure of the vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) prepared in Example 1 of the present invention;

[0022] Figure 3 is the XRD pattern of the materials obtained in Comparative Examples 1-3 and the vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) prepared in Example 1;

[0023] Figure 4a , Figure 4b They are respectively the diffusion coefficient of zinc ions and the cycle performance diagram of a battery composed of the vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) prepared in Example 1 of the present invention as the positive electrode active material of a zinc ion battery;

[0024] Figure 5 This is a cycle performance diagram of a battery using vanadium pentoxide (V2O5) prepared in Comparative Example 1 as a positive electrode active material for a zinc ion battery;

[0025] Figure 6 is a SEM image of the material prepared in Comparative Example 2;

[0026] Figure 7 This is a cycle performance diagram of a battery composed of the material prepared in Comparative Example 2 as the positive electrode active material of a zinc ion battery;

[0027] Figure 8 is a SEM image of the material prepared in Comparative Example 3;

[0028] Fig. 9 This is a cycle performance diagram of a battery composed of the material prepared in Comparative Example 3 as the positive electrode active material of a zinc ion battery. DETAILED DESCRIPTION

[0029] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice, which mainly studies the three-dimensional conductive carbon network and its composite to obtain a hierarchical mesh material to achieve efficient electron conduction and rapid ion diffusion, thereby improving its electrochemical performance. The technical solution, its implementation process and principle will be further explained as follows.

[0030] One aspect of an embodiment of the present invention provides a three-dimensional hierarchical network metal oxide / carbon composite material comprising: a metal oxide active material coated with a carbon shell layer and a highly conductive carbon skeleton material, wherein the metal oxide active material coated with a carbon shell layer and the highly conductive carbon skeleton material are interwoven to form a three-dimensional hierarchical conductive network structure.

[0031] As a preferred embodiment, the metal oxide active material includes a transition metal oxide, and the transition metal oxide includes any one or a combination of two of vanadium-based oxides, manganese-based oxides, niobium-based oxides, molybdenum oxides, etc., but is not limited thereto.

[0032] Furthermore, the vanadium-based oxides may include vanadium pentoxide (V2O5), vanadium trioxide (V2O3), vanadium dioxide (VO2), vanadium heptoxide (V3O7), vanadium trioxide (V6O 13 ), any one or a combination of two or more of metal ion intercalated vanadium oxide, wherein the metal ion intercalated vanadium oxide includes M-VO, Cs n V2O5、Al n V2O5、Fe n V2O5、Ca n Any one or a combination of two or more of V2O5, etc., M is selected from any one of metals such as Li, Na, K, Ag, Ca, Mn, Co, Zn, Fe, Cr, etc., but is not limited thereto.

[0033] Furthermore, the manganese-based oxide may include manganese dioxide MnO2 of different crystalline forms (α, β, γ, δ, λ, etc.), manganese monoxide (MnO), manganese trioxide (Mn2O3), and manganese oxides M-MO doped with metal ions, such as Na n MnO2, M can be any one or a combination of two or more metals such as Li, Na, K, V, Ag, Ca, Co, Pb, Zn, Fe, Cr, etc., but is not limited thereto.

[0034] Further, the niobium-based oxide includes niobium pentoxide (Nb2O5), but is not limited thereto.

[0035] As a preferred solution, the thickness of the carbon shell layer is 5 to 10 nm.

[0036] As a preferred embodiment, the highly conductive carbon skeleton material may include carbon nanotubes, graphene, graphene oxide, C 60 , graphyne, graphene quantum dots, heteroatom-doped graphene (doping elements include N, P, S, etc.), carbon nanofibers, carbon aerogels, carbon nanotube arrays, etc., or any one or a combination of two or more thereof, but not limited thereto.

[0037] Further, the carbon nanotubes may be at least one of multi-walled carbon nanotubes, single-walled carbon nanotubes, etc., and the graphene may be at least one of multi-layer graphene, single-layer graphene, etc., but are not limited thereto.

[0038] As a preferred solution, the content of the highly conductive carbon material in the three-dimensional hierarchical network metal oxide / carbon composite material is 10 to 60 wt %.

[0039] In summary, the present invention provides a hierarchical mesh conductive carbon network that facilitates electron conduction and ion diffusion. This structure can achieve multi-level and multi-dimensional coupling and synergistic effects, wherein the multi-level refers to a carbon shell structure coating the outside of the metal oxide active material, and the multi-dimensional refers to the three-dimensional network structure formed. The metal oxide active material coated with the carbon shell structure and the highly conductive carbon skeleton material (such as carbon nanotubes, graphene, etc.) are intertwined to form a three-dimensional conductive network, which ensures full contact between the electrode and the electrolyte while inhibiting the dissolution of vanadium ions, jointly promoting electron conduction and ion diffusion, so that the composite material exhibits extremely superior cycle stability and ultra-long life.

[0040] Another aspect of the embodiments of the present invention further provides a method for preparing a three-dimensional hierarchical network metal oxide / carbon composite material, which comprises:

[0041] Providing a first solution comprising a highly conductive carbon framework material;

[0042] Providing a second solution comprising a transition metal oxide precursor, an organic solvent, and a carbon source (including a carbon skeleton and a carbon shell source);

[0043] The first solution and the second solution are mixed, subjected to a hydrothermal reaction, and freeze-dried to obtain a three-dimensional carbon skeleton framework to obtain a precursor material;

[0044] The precursor material is calcined to obtain a three-dimensional hierarchical network metal oxide / carbon composite material.

[0045] Among them, the types of the highly conductive carbon materials are as described above and will not be repeated here.

[0046] In a specific embodiment, the preparation method comprises: dispersing the highly conductive carbon skeleton material in water to form the first solution.

[0047] Furthermore, the concentration of the highly conductive carbon skeleton material in the first solution is 0.8-2.0 mg / mL.

[0048] In a specific embodiment, the mass ratio of the transition metal oxide precursor to the carbon source is 1 to 5:1.

[0049] Furthermore, the mass ratio of the organic solvent to the combination of the transition metal oxide precursor and the carbon source (solute) is 20 to 60:1.

[0050] In a specific embodiment, the transition metal oxide precursor includes any one or a combination of two or more of a vanadium source, a manganese source, a niobium source, a molybdenum source, etc., but is not limited thereto.

[0051] Furthermore, the vanadium source includes any one or a combination of two or more of vanadate, metavanadate (such as ammonium metavanadate), pyrovanadate, orthovanadate, etc., but is not limited thereto.

[0052] Furthermore, the manganese source includes any one or a combination of two or more of potassium permanganate, manganese sulfate (such as hydrated manganese sulfate), manganese perchlorate (such as hydrated manganese perchlorate), manganese nitrate (such as hydrated manganese nitrate), etc., but is not limited thereto.

[0053] Furthermore, the niobium source includes any one or a combination of two or more of niobium pentachloride, ammonium niobate, niobium chlorate, etc., but is not limited thereto.

[0054] Furthermore, the molybdenum source includes any one or a combination of two or more of sodium molybdate, cobalt molybdate, molybdenum sulfide, molybdenum oxide, etc., but is not limited thereto.

[0055] In a specific embodiment, the carbon shell source includes any one or a combination of two or more of oxalic acid, glucose, melamine, dopamine, polydopamine, resorcinol-formaldehyde resin, polyvinyl pyrrolidone, tannic acid, citric acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, aniline, anthracene, etc., but is not limited thereto.

[0056] Furthermore, when the carbon shell source is oxalic acid, tannic acid, citric acid, etc., the pH value of the second solution can be adjusted to 2 to 6. These types of functions here are relatively special, which can not only adjust the pH value but also serve as a carbon shell coating layer.

[0057] Furthermore, the organic solvent includes any one or a combination of two or more of ethylene glycol, isopropanol, n-butanol, glycerol, propylene glycol, glycerol, polyethylene glycol, ethyl acetate, acetone, etc., but is not limited thereto.

[0058] Furthermore, the preparation method may also include: adding a surfactant to the first solution or the second solution to prevent the highly conductive carbon skeleton material or the carbon shell source material from agglomerating in the solution, wherein the surfactant includes any one or a combination of two or more of anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc., but is not limited thereto.

[0059] Among them, the anionic surfactant includes any one or a combination of two or more of linear alkylbenzene sulfonate, sodium α-olefin sulfonate, sodium dodecyl sulfate, etc., and the cationic surfactant includes any one or a combination of two or more of hexadecyldimethylammonium bromide, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, dodecyldimethylamine oxide, etc.; preferably, the nonionic surfactant includes alkyl alcohol amide, fatty alcohol polyvinyl ether, etc., and the amphoteric surfactant includes at least one of dodecyldimethyl betaine, carboxylate type imidazoline, etc., but is not limited thereto.

[0060] In a specific embodiment, the temperature of the hydrothermal reaction is 100-200°C, and the reaction time is 6-28h. The preparation mechanism of the hydrothermal reaction in the present invention is: first, under a high temperature and high pressure reducing atmosphere, the carbon-containing functional groups of the carbon shell source (such as oxalic acid substances) are preferentially adsorbed on the generated transition metal oxide (such as vanadium pentoxide nanoparticles), forming a pre-coated uncrystallized precursor, which is uniformly dispersed on the carbon skeleton in the solution. The present invention can obtain a three-dimensional structure by freeze drying.

[0061] In a specific embodiment, the preparation method comprises: heating the precursor material to 200-600°C at a heating rate of 1-10°C / min in an air atmosphere and calcining for 1-4 hours to obtain the three-dimensional hierarchical network metal oxide / carbon composite material. The calcination in the present invention has the following functions: 1. forming a complete carbon coating layer during the calcination process; 2. removing the remaining solvent of the precursor material and causing it to crystallize into a transition metal oxide.

[0062] In summary, the present invention obtains a metal oxide@carbon composite electrode with high conductivity and fast ion diffusion rate by synthesizing a three-dimensional hierarchical conductive network structure in situ by a simple one-step hydrothermal method. This hierarchical conductive network uses carbon materials as carriers, and then generates metal oxides in situ on them, so that the carbon materials are uniformly wrapped around the outside of the metal oxide active material. This multi-level and multi-dimensional hierarchical structure design achieves twice the result with half the effort. The metal oxide wrapped by the carbon layer has good conductivity, and at the same time, it also reduces its contact area with the weakly acidic electrolyte, inhibiting the dissolution of transition metal ions. The formed three-dimensional conductive network provides more reactive active sites, accelerating the diffusion rate of ions inside the electrode.

[0063] Another aspect of the embodiments of the present invention further provides a three-dimensional hierarchical network metal oxide / carbon composite material prepared by the aforementioned preparation method.

[0064] Another aspect of the embodiments of the present invention further provides the use of any of the aforementioned three-dimensional hierarchical network metal oxide / carbon composite materials in the preparation of electrode materials.

[0065] Specifically, another aspect of an embodiment of the present invention further provides a zinc ion battery positive electrode, including a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is the aforementioned three-dimensional hierarchical network metal oxide / carbon composite material.

[0066] Correspondingly, another aspect of an embodiment of the present invention further provides a zinc ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode adopts the aforementioned zinc ion battery positive electrode.

[0067] The zinc ion battery assembled by the present invention has a high ion diffusion rate (D Zn 2+ =10 -8 ~10 -10 ) and excellent rate performance, and has an ultra-high specific capacity of 480 mA h / g at a current density of 5 A / g, a capacity retention rate of 84% and a coulombic efficiency close to 100% after 1200 stable cycles.

[0068] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.

[0069] The following examples take vanadium pentoxide electrode material with high theoretical specific capacity (589 mAh / g) as an example, and all reagents used are analytically pure.

[0070] Comparative Example 1

[0071] Take 1.0g of ammonium metavanadate and dissolve it in 60mL of ethylene glycol. Stir magnetically for half an hour at a speed of rpm = 1600r / S, and add dilute hydrochloric acid to adjust the pH to about 2-3. Then pour the solution into a hydrothermal kettle and react at 180℃ for 24h, then filter it and wash it with deionized water until it is neutral, freeze-dry it overnight to obtain a loose precursor material. The precursor is transferred to a tube furnace, heated to 450℃ at a heating rate of 4℃ / min in an air atmosphere and calcined for 2h to obtain an electrode material. The material is mixed with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, and the slurry is evenly coated on the graphene film, vacuum dried at 60℃ for 24 hours, and punched into an electrode sheet with a diameter of 10mm. The zinc sheet is used as the negative electrode, and a 3mol / L zinc trifluoromethanesulfonate solution is used as the electrolyte. The button battery is assembled with a 2025 battery shell.

[0072] Example 1

[0073] First, 80 mg of carbon nanotube powder and 16 mL of graphene aqueous solution (5 mg / mL) were ultrasonically dispersed in 200 mL of deionized water using a cell crusher at 45% power to obtain solution 1. Ammonium metavanadate was dissolved in 40 mL of ethylene glycol, and oxalic acid was added to adjust the pH to about 2 to 6 to obtain solution 2, wherein the mass ratio of ammonium metavanadate to oxalic acid was 1:1, and the mass ratio of ethylene glycol to the combination of ammonium metavanadate and oxalic acid was 20:1. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 100°C for 28 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor was transferred to a tubular furnace, heated to 350°C at a heating rate of 4°C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0074] Example 2

[0075] First, 250 mg of carbon nanofiber powder, 50 mL of nitrogen-doped graphene aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 250 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.7 g of ammonium metavanadate was dissolved in 45 mL of ethylene glycol, and 1.35 g of oxalic acid and 0.5 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to obtain solution 2. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 200 ° C for 6 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 450 ° C at a heating rate of 4 ° C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0076] Example 3

[0077] First, 200 mg of carbon aerogel, 60 mL of graphene quantum dot aqueous solution (5 mg / mL) and 10 mg of sodium dodecyl sulfate were ultrasonically dispersed in 500 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.45 g of ammonium metavanadate was dissolved in 60 mL of propylene glycol, and 1.15 g of citric acid and 0.5 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to form solution 2, and solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal autoclave and reacted at 180 ° C for 24 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tubular furnace, heated to 200 ° C at a heating rate of 1 ° C / min in an air atmosphere, and calcined for 4 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0078] Example 4

[0079] First, 200 mg of carbon nanotube array powder, 60 mL of graphene quantum dot aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 500 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.0 g of ammonium metavanadate was dissolved in 60 mL of ethyl acetate, and 1.35 g of citric acid and 0.5 g of hexadecyltrimethylammonium bromide were added and magnetically stirred at rpm = 1600 r / S to form solution 2. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 100 ° C for 28 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 600 ° C at a heating rate of 10 ° C / min in an air atmosphere, and calcined for 1 hour to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0080] Example 5

[0081] First, 200 mg of gydne powder, 60 mL of nitrogen-doped graphene aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 500 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.0 g of ammonium metavanadate was dissolved in 60 mL of ethyl acetate, and 1.35 g of citric acid and 0.5 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to form solution 2, and solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal autoclave and reacted at 160 ° C for 18 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 400 ° C at a heating rate of 5 ° C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0082] Example 6

[0083] First, 80 mg of carbon nanotube powder, 16 mL of graphene oxide aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 200 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 0.732 g of hydrated manganese sulfate was dissolved in 40 mL of ethylene glycol, and 0.76 g of oxalic acid and 0.1 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to obtain solution 2. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal autoclave and reacted at 200°C for 18 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 400°C at a heating rate of 4°C / min in an air atmosphere, and calcined for 4 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. 2 mol / L zinc sulfate and 0.2 mol / L manganese sulfate solution were used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0084] Example 7

[0085] First, 80 mg of carbon nanotube powder, 16 mL of graphene oxide aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 200 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 0.886 g of niobium chloride was dissolved in 60 mL of n-butanol, and 0.89 g of oxalic acid and 0.1 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to obtain solution 2. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal autoclave and reacted at 120°C for 28 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 450°C at a heating rate of 5°C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 2mol / L zinc sulfate solution was used as the electrolyte. The button battery was assembled using a 2025 type battery shell.

[0086] Example 8

[0087] First, 80 mg of carbon nanotube powder, 16 mL of graphene oxide aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 200 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.36 g of molybdenum oxide was dissolved in 60 mL of glycerol, and 1.5 g of citric acid and 0.1 g of hexadecyltrimethylammonium bromide were added with magnetic stirring at rpm = 1600 r / S to obtain solution 2. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 180°C for 18 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 500°C at a heating rate of 5°C / min in an air atmosphere, and calcined for 4 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 2mol / L zinc sulfate solution was used as the electrolyte. The button battery was assembled using a 2025 type battery shell.

[0088] Example 9

[0089] First, 300 mg of carbon nanotube powder and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 200 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.0 g of ammonium metavanadate was dissolved in 80 mL of n-butanol, and 1.35 g of glucose and 0.5 g of hexadecyltrimethylammonium bromide were added and magnetically stirred at rpm = 1600 r / S for half an hour, and pH was adjusted to about 2-3 with dilute hydrochloric acid to obtain solution 2, and solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 160°C for 18 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tube furnace, heated to 450°C at a heating rate of 4°C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0090] Example 10

[0091] First, 60 mL of graphene aqueous solution (5 mg / mL) and 10 mg of N-vinyl pyrrolidone were ultrasonically dispersed in 200 mL of deionized water using a cell crusher with 45% power to obtain solution 1. 1.0 g of ammonium metavanadate was dissolved in n-butanol, and 5 g of glucose and 0.5 g of hexadecyltrimethylammonium bromide were added and magnetically stirred at rpm = 1600 r / S for half an hour, and pH was adjusted to about 2-3 with dilute hydrochloric acid to obtain solution 2. The mass ratio of n-butanol to ammonium metavanadate and glucose was 60:1. Solution 2 was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle at 200 ° C for 12 hours, and then it was filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor material was transferred to a tubular furnace, heated to 350 ° C at a heating rate of 4 ° C / min in an air atmosphere, and calcined for 4 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0092] Comparative Example 2

[0093] First, 200 mg of carbon nanotube powder and 40 mL of graphene aqueous solution (5 mg / mL) were ultrasonically dispersed in 300 mL of deionized water using a cell crusher at 45% power to obtain solution 1. 0.5 g of ammonium metavanadate was dissolved in 40 mL of ethylene glycol, and dilute hydrochloric acid was added to adjust the pH to about 2-3 to obtain solution 2, which was slowly added dropwise to the stirred solution 1, and then the mixed solution was poured into a hydrothermal kettle and reacted at 180°C for 24 hours, then filtered and washed with deionized water until neutral, and freeze-dried overnight to obtain a loose precursor material. The precursor was transferred to a tubular furnace, heated to 350°C at a heating rate of 4°C / min in an air atmosphere, and calcined for 2 hours to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0094] Comparative Example 3

[0095] Take 0.5g of ammonium metavanadate and dissolve it in 40mL of ethylene glycol, add 1.35g of oxalic acid and 0.5g of hexadecyltrimethylammonium bromide, stir magnetically at rpm = 1600r / S for half an hour, slowly drop solution 2 into the stirred solution 1, then pour the mixed solution into a hydrothermal kettle and react at 180℃ for 24h, then filter it and wash it with deionized water until it is neutral, freeze-dry it overnight to obtain a loose precursor material. Transfer the precursor to a tube furnace, heat it to 350℃ at a heating rate of 4℃ / min in an air atmosphere, and calcine it for 2h to obtain an electrode material. The material was mixed evenly with carbon black (Super P) and a binder (5% PVDF) in a mass ratio of 7:2:1 to prepare a slurry, which was evenly coated on the graphene film and vacuum dried at 60°C for 24 hours. The electrode sheets were punched into electrode sheets with a diameter of 10 mm. The zinc sheet was used as the negative electrode. A 3 mol / L zinc trifluoromethanesulfonate solution was used as the electrolyte. The button cells were assembled using a 2025 type battery shell.

[0096] The inventors of this case also took the vanadium pentoxide (V2O5) obtained in Comparative Example 1, the vanadium pentoxide without carbon layer obtained in Comparative Example 2, the material obtained in Comparative Example 3, and the vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CN Ts) obtained in Example 1 as examples, and conducted various characterization and performance tests, and the results are as follows:

[0097] See also Figure 1a and Figure 1b , is the SEM data of vanadium pentoxide (V2O5), Figure 1c and Figure 1dThe SEM data of the three-dimensional hierarchical network structure of vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) is shown. Figure 2a and Figure 2b , showing the TEM data of the carbon-coated structure of vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs).

[0098] See also Figure 3 , which are the XRD data of vanadium pentoxide (V2O5), vanadium pentoxide without carbon layer, the material obtained in Comparative Example 3, and vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs).

[0099] Figure 4a The diffusion coefficient of zinc ions in a battery composed of V2O5@G-CNTs as the positive electrode active material of a zinc ion battery is shown. Figure 4b The graph shows the cycling performance data of batteries composed of vanadium pentoxide (V2O5) and vanadium pentoxide@carbon nanotube / graphene composite (V2O5@G-CNTs) as positive electrode active materials for zinc ion batteries.

[0100] Figure 5 The graph shows the cycle performance of a battery composed of vanadium pentoxide (V2O5) prepared in Comparative Example 1 as the positive electrode active material of a zinc ion battery.

[0101] Figure 6 This is a SEM image of the vanadium pentoxide without carbon layer prepared in Comparative Example 2. This material is used as the positive electrode active material of a zinc ion battery to form a battery. The cycle performance of the battery is as follows: Figure 7 shown.

[0102] Figure 8 The SEM image of the material prepared in comparative example 3 (coated with a carbon layer but without cross-linking carbon nanotubes and graphene) is shown. The material is used as the positive electrode active material of a zinc ion battery to form a battery. The cycle performance of the battery is shown in FIG. Fig. 9 shown.

[0103] In addition, the inventors of this case also used other raw materials and process conditions listed in this specification, and prepared a series of three-dimensional hierarchical network metal oxide / carbon composite materials with reference to the aforementioned embodiments, all of which have the excellent properties described in this specification.

[0104] In summary, the three-dimensional hierarchical network metal oxide / carbon composite material provided by the present invention is used as a positive electrode active material for zinc ion batteries, which can significantly improve the battery performance. First, by forming a three-dimensional conductive network, the conductivity of the overall material is improved and the reaction area of ​​the electrolyte and the electrode is increased, and the battery capacity is improved by having a higher ion diffusion rate. Then, the layered structure allows the carbon layer to wrap the metal oxide, inhibiting the dissolution of vanadium ions, thereby greatly reducing the battery capacity attenuation and extending the cycle life.

[0105] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.

Claims

1. A three-dimensional hierarchical network metal oxide / carbon composite material, characterized in that: include: A metal oxide active material coated with a carbon shell layer and a highly conductive carbon skeleton, wherein the metal oxide active material coated with a carbon shell layer and the highly conductive carbon skeleton are interwoven with each other to form a three-dimensional hierarchical conductive network structure.

2. The three-dimensional hierarchical network metal oxide / carbon composite material according to claim 1, characterized in that: The metal oxide active material includes a transition metal oxide, and the transition metal oxide includes any one or a combination of two or more of vanadium-based oxide, manganese-based oxide, niobium-based oxide, and molybdenum oxide; Preferably, the vanadium-based oxide includes any one or a combination of two or more of vanadium pentoxide, vanadium trioxide, vanadium dioxide, vanadium heptoxide, vanadium trioxide, and metal ion intercalated vanadium oxide; Preferably, the manganese-based oxide includes any one or a combination of two or more of manganese dioxide, manganese monoxide, manganese trioxide, and metal ion-doped manganese oxide; Preferably, the niobium-based oxide comprises niobium pentoxide; And / or, the thickness of the carbon shell layer is 5-10 nm.

3. The three-dimensional hierarchical network metal oxide / carbon composite material according to claim 1, characterized in that: The highly conductive carbon skeleton comprises carbon nanotubes, graphene, graphene oxide, C 60 , graphyne, graphene quantum dots, heteroatom-doped graphene, carbon nanofibers, carbon aerogels, carbon nanotube arrays, any one or a combination of two or more thereof, wherein the doping element in the heteroatom-doped graphene includes at least one of N, P, and S; preferably, the carbon nanotubes include multi-walled carbon nanotubes and / or single-walled carbon nanotubes, and preferably, the graphene includes multi-layer graphene and / or single-layer graphene; And / or, the content of the highly conductive carbon material in the three-dimensional hierarchical network metal oxide / carbon composite material is 10 to 60 wt %.

4. The method for preparing the three-dimensional hierarchical network metal oxide / carbon composite material according to any one of claims 1 to 3, characterized in that: include: Providing a first solution comprising a highly conductive carbon framework material; Providing a second solution comprising a transition metal oxide precursor, an organic solvent, and a carbon source; The first solution and the second solution are mixed, subjected to a hydrothermal reaction, and freeze-dried to obtain a three-dimensional carbon skeleton framework to obtain a precursor material; The precursor material is calcined to obtain a three-dimensional hierarchical network metal oxide / carbon composite material.

5. The preparation method according to claim 4, characterized in that: include: The highly conductive carbon skeleton material is dispersed in water to form the first solution. Preferably, the concentration of the highly conductive carbon skeleton material in the first solution is 0.8-2.0 mg / mL.

6. The preparation method according to claim 4, characterized in that: The mass ratio of the transition metal oxide precursor to the carbon source is 1 to 5:1; and / or the mass ratio of the organic solvent to the combination of the transition metal oxide precursor and the carbon source is 20 to 60:1; And / or, the transition metal oxide precursor includes any one of a vanadium source, a manganese source, a niobium source, and a molybdenum source, or a combination of two or more thereof. Preferably, the vanadium source includes any one of vanadate, metavanadate, pyrovanadate, and orthovanadate, or a combination of two or more thereof; preferably, the manganese source includes any one of potassium permanganate, manganese sulfate, manganese perchlorate, and manganese nitrate, or a combination of two or more thereof; preferably, the niobium source includes any one of niobium pentachloride, ammonium niobate, and niobium chlorate, or a combination of two or more thereof; preferably, the molybdenum source includes any one of sodium molybdate, cobalt molybdate, molybdenum sulfide, and molybdenum oxide, or a combination of two or more thereof; And / or, the carbon source comprises any one or a combination of two or more of oxalic acid, glucose, melamine, dopamine, polydopamine, resorcinol-formaldehyde resin, polyvinyl pyrrolidone, tannic acid, citric acid, polyvinyl alcohol, polypyrrole, vitamin C, polyethylene glycol, aniline, and anthracene; Preferably, when the carbon source is oxalic acid, citric acid or tannic acid, the pH value of the second solution is adjusted to 2 to 6; And / or, the organic solvent includes any one or a combination of two or more of ethylene glycol, isopropanol, n-butanol, glycerol, propylene glycol, glycerol, polyethylene glycol, ethyl acetate, and acetone; And / or, the preparation method further comprises: adding a surfactant to the first solution or the second solution, wherein the surfactant comprises any one of anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants, or a combination of two or more thereof; preferably, the anionic surfactant comprises any one of linear alkylbenzene sulfonate, sodium α-olefin sulfonate, and sodium dodecyl sulfate, or a combination of two or more thereof; preferably, the cationic surfactant comprises any one of hexadecyldimethylammonium bromide, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, and dodecyldimethylamine oxide, or a combination of two or more thereof; preferably, the nonionic surfactant comprises alkyl alcohol amide and / or fatty alcohol polyethylene ether; preferably, the amphoteric surfactant comprises dodecyldimethylbetaine and / or carboxylate-type imidazoline.

7. The preparation method according to claim 4, characterized in that: The temperature of the hydrothermal reaction is 100-200°C, and the reaction time is 6-28h; and / or, the preparation method comprises: in an air atmosphere, heating the precursor material to 200-600°C at a heating rate of 1-10°C / min and calcining for 1-4h to obtain the three-dimensional hierarchical network metal oxide / carbon composite material.

8. Use of the three-dimensional hierarchical network metal oxide / carbon composite material according to any one of claims 1 to 3 in the preparation of electrode materials.

9. A positive electrode for a zinc ion battery, comprising a positive electrode active material, a conductive agent and a binder, characterized in that: The positive electrode active material is a three-dimensional hierarchical network metal oxide / carbon composite material according to any one of claims 1 to 3.

10. A zinc ion battery comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The positive electrode is the zinc ion battery positive electrode according to claim 9.

Citation Information

Patent Citations

  • Surface layer oxidized carbon nanotube array / graphene / manganese dioxide composite material electrode and preparation method and application thereof

    CN106548876A

  • Method for preparing high-capacity battery anode material

    CN108550824A

  • Carbon-coated vanadium pentoxide positive electrode material as well as preparation method thereof and application of carbon-coated vanadium pentoxide positive electrode material in lithium battery

    CN109817943A

  • Structure of multi-sphere carbon-coated manganese dioxide composite material and preparation method thereof

    CN110148716A

  • Preparation method of binder-free aqueous zinc ion battery positive electrode composite material

    CN112421017A

Cited By

  • Vanadium-based metal oxide (at) rGO composite aerogel as well as preparation method and application thereof

    CN120664589A