Carbon-silicon composite material with elastic nanostructure as well as preparation method and application of carbon-silicon composite material

By using elastic nanostructured carbon-silicon composite materials in lithium-ion batteries, using titanium dioxide and carbon nano-thin layers to wrap silicon particles, and combining functionalized carbon nanotube networks, the structural damage problem caused by volume expansion of silicon negative electrode materials is solved. High capacity and cycle stability of negative electrode materials are achieved, simplifying production processes and reducing costs.

CN118943310APending Publication Date: 2024-11-12MONTA VISTA ENERGY TECH CORP (ANHUI)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310526578.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the silicon negative electrode material has structural damage and electrolyte consumption due to volume expansion, making it difficult to achieve high capacity and cycle stability. The large-scale production of silicon nanowires is difficult, resulting in limited commercial applications.

Method used

Using carbon-silicon composite materials with elastic nanostructures, silicon particles are wrapped through titanium dioxide thin layer and carbon nano-thin layer, and functionalized carbon nanotubes form a continuous network structure to form carbon-carbon chemical bonds to limit the volume expansion of silicon particles and avoid Contact with the electrolyte to achieve electrochemical stability.

Benefits of technology

Effectively constrain the volume expansion of silicon particles, avoid damage to the electrode structure, improve the reversible capacity and cycle stability of the negative electrode material of lithium-ion batteries, and reduce production costs, achieving low-cost and efficient process production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943310A_ABST
    Figure CN118943310A_ABST
Patent Text Reader

Abstract

The invention provides a carbon-silicon composite material with an elastic nanostructure as well as a preparation method and application of the carbon-silicon composite material. The carbon-silicon composite material is provided with an elastic unit, and the elastic unit is of a continuous network structure formed by a titanium dioxide thin layer, a carbon nano thin layer and a carbon nano tube which are sequentially wrapped on the surface of a silicon-containing particle; the volume expansion of the silicon-containing particles is restrained in the elastic unit by the elastic unit. The preparation method comprises the following steps: carrying out heat treatment on a carbon nanotube to obtain a functionalized carbon nanotube, mixing silicon-containing particles with tetra-n-butyl titanate, carrying out high-temperature annealing, mixing the obtained product with the functionalized carbon nanotube and an organic carbon source, and finally carrying out high-temperature pyrolysis in inert gas. According to the carbon-silicon composite material with the elastic nanostructure, volume expansion of silicon-containing particles in the electrochemical charging and discharging process can be restrained in an elastic unit, macroscopic strain and stress accumulation is not generated, and the preparation method is simple, low in equipment requirement and easy to popularize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a carbon-silicon composite material with an elastic nanostructure, a preparation method and an application thereof. Background Art

[0002] Lithium-ion batteries are structurally divided into positive electrode, negative electrode, diaphragm, electrolyte and shell. Among the many negative electrode materials, silicon negative electrode has high theoretical capacity and is valued, but the volume expansion of silicon is huge. After full lithium embedding, the volume expansion is >300%, and the excessive volume expansion causes the silicon particles themselves to crack and break. This characteristic causes the contact between the active layer particles of the silicon negative electrode material to fail after repeated charge and discharge. As the cycle of charge and discharge progresses, the cracked silicon particles continue to produce new surfaces, which react with the electrolyte to form a new SEI film, resulting in the depletion of the electrolyte.

[0003] In order to overcome the stability problem caused by the volume expansion of silicon, in recent years, research on silicon materials has been the focus of breakthroughs in this field. Silicon nanowires as negative electrode materials have been proven to be extremely effective in exerting their high capacity characteristics. The silicon nanowires prepared by Cui Yi and others at Stanford University have the characteristics of highly reversible and non-ruptured volume expansion during charge and discharge, and can still maintain 83.6% of the reversible capacity after 1,000 cycles. However, due to the difficulty of the synthesis method and the extremely high cost, large-scale production of silicon nanowires is still not possible. At present, the more mature commercial silicon-based negative electrode materials are mainly based on silicon oxide composite materials, but the volume expansion of silicon oxide is still relatively severe.

[0004] Carbon materials have good electrical conductivity and can wrap silicon nanoparticles to avoid the uncontrolled growth of SEI films. Silicon particles are compounded in the carbon network to buffer the volume expansion of silicon to a certain extent, effectively inhibiting the structural damage of the electrode and making it have better cycle stability. For example, Chinese invention patent CN114590795A uses a dispersant solution to carry out a sol-gel reaction to synthesize mesoporous silica balls, and obtains a carbon-wrapped mesoporous silicon composite material by carbon source-assisted carbon thermal reduction. Chinese invention patent CN114566634A uses silicon nanoparticles and organic matter to composite spinning and pyrolysis carbonization to obtain silicon-carbon composite nanofibers, embeds silicon nanoparticles inside carbon nanofibers, and then attaches titanium dioxide to the surface of nanofibers to form an electrochemically stable layer with a certain elasticity, further stabilizes its spatial structure, and avoids contact between silicon and electrolyte, inhibits the rapid growth of SEI film, and the resulting composite material has good high-capacity charge and discharge stability.

[0005] However, although the above method proves that highly stable high-capacity silicon-based materials can be prepared through appropriate structural control, the technical method used can only be implemented in the laboratory, with high production costs and high equipment requirements, and cannot be mass-produced. Therefore, it is still an urgent problem to obtain a silicon-carbon composite material that is easy to produce at low cost and effectively exerts the high-capacity characteristics of silicon through appropriate structural design and taking into account the process requirements of large-scale production. Summary of the invention

[0006] In order to overcome the shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a carbon-silicon composite material with an elastic nanostructure and a preparation method thereof. The carbon-silicon composite material with an elastic nanostructure prepared by the method of the present invention can constrain the volume expansion of silicon-containing particles during the electrochemical charging and discharging lithium insertion process within the composite material powder without generating macroscopic strain and stress accumulation, and protect the silicon particles from contacting the electrolyte during the volume expansion of the silicon particles, thereby obtaining an electrochemically stable high-capacity negative electrode material.

[0007] In order to achieve the above technical effects, the technical solution adopted by the present invention is as follows:

[0008] The present invention provides a carbon-silicon composite material with an elastic nanostructure, wherein the carbon-silicon composite material has a first elastic unit and a second elastic unit;

[0009] The first elastic unit comprises a titanium dioxide thin layer and a carbon nano thin layer sequentially wrapped on the surface of the silicon-containing particles;

[0010] The second elastic unit is a continuous network structure formed by functionalized carbon nanotubes;

[0011] The first elastic unit constrains the volume expansion of the silicon-containing particles within the first elastic unit so as not to contact with the electrolyte; and the second elastic unit constrains the volume expansion of the first elastic unit within the second elastic unit.

[0012] Furthermore, a carbon-carbon chemical bond is formed between the carbon nanofilm and the functionalized carbon nanotube to constrain the first elastic unit inside the second elastic unit.

[0013] Furthermore, the functionalized carbon nanotubes are irregularly filled to form a continuous network structure, resulting in a large number of voids in the carbon silicon material, which is conducive to accommodating the volume expansion of the first elastic unit.

[0014] The present invention also provides a method for preparing the above-mentioned carbon-silicon composite material with elastic nanostructure, comprising the following steps:

[0015] Titanium dioxide is coated on the surface of silicon nanoparticles to form a titanium dioxide thin layer; an organic carbon source is coated and adhered to the surface of the titanium dioxide thin layer and the functionalized carbon nanotubes, and after pyrolysis, the organic carbon source forms a carbon nanolayer on the surface of the titanium dioxide thin layer, thereby forming the carbon nanoparticles coated with the titanium dioxide thin layer and the carbon nanolayer in sequence as the first elastic unit;

[0016] The functionalized carbon nanotubes form a continuous carbon nanotube network structure as the second elastic unit.

[0017] Furthermore, the preparation steps include:

[0018] S1. Preparation of functionalized carbon nanotubes: mixing carbon nanotubes with an oxidant and heat treating to obtain functionalized carbon nanotubes;

[0019] S2. Preparation of silicon / titanate coated material: dispersing silicon-containing nanoparticles in an organic solvent, adding an organic titanium source to dissolve, and adding deionized water to obtain a silicon / titanate coated material;

[0020] S3. Preparation of silicon / titanium dioxide coated material: The silicon / titanate coated material obtained in S2 was vacuum annealed to obtain a silicon / titanium dioxide coated material;

[0021] S4. Preparing a precursor; mixing the functionalized carbon nanotubes described in S1 and the silicon / titanium dioxide coating material described in S3 with an organic carbon source and spray drying the mixture so that the organic carbon source is wrapped and adhered to the silicon / titanium dioxide coating material and the surface of the carbon nanotubes to obtain a precursor;

[0022] S5. Making a carbon-silicon composite material: pyrolyzing the precursor obtained in S4 to obtain a carbon-silicon composite material.

[0023] Furthermore, the heat treatment temperature is 400-800° C., and the heat treatment time is 5-120 minutes.

[0024] Furthermore, the temperature during the vacuum annealing is 550-600° C., and the time of the vacuum annealing is 20-40 minutes.

[0025] Furthermore, the oxidant includes potassium permanganate, phosphorus pentoxide, and persulfate, preferably potassium permanganate.

[0026] Furthermore, the organic solvent includes small molecule alcohols and low molecule alkanes, and preferably, is anhydrous ethanol.

[0027] Furthermore, the organic titanium source includes Ti(OR)4, R is an alkyl chain, and preferably, is tetra-n-butyl titanate.

[0028] Furthermore, the organic carbon source includes any one of polyvinyl alcohol, glucose, fructose, polyvinyl pyrrolidone, chitosan, or a combination of two or more thereof.

[0029] Furthermore, in S4, the mass ratio of the silicon / titanium dioxide coating material to the functionalized carbon nanotubes is 0.3-0.5:1; and the mass of the organic carbon source accounts for 10%-20% of the mixed mass.

[0030] Furthermore, in S5, the pyrolysis temperature is 800-1400°C.

[0031] Furthermore, the diameter of the carbon nanotubes is 2-200 nanometers; and the particle size of the silicon-containing nanoparticles is in the range of 10-300 nanometers.

[0032] Furthermore, the mass ratio of the carbon nanotube powder to the potassium permanganate powder is 10:1.

[0033] Furthermore, the silicon-containing nanoparticles include: elemental silicon, silicon monoxide or SiOx, wherein 0<X<1.

[0034] Furthermore, the mass ratio of tetra-n-butyl titanate to silicon-containing nanoparticles is 0.02-0.1:1.

[0035] The above-mentioned carbon-silicon composite material with elastic nanostructure, or the carbon-silicon composite material with elastic nanostructure prepared by the preparation method provided by the present invention is used in the negative electrode of lithium-ion batteries.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The carbon-silicon composite material with elastic nanostructure provided by the present invention has an elastic unit, which constrains the volume expansion of silicon-containing particles inside the elastic unit, can avoid contact between the silicon-containing particles and the electrolyte, obtain a stable SEI film, and obtain highly reversible large-capacity negative electrode performance.

[0038] The method for preparing a carbon-silicon composite material with an elastic nanostructure provided by the present invention uses silicon-containing nanoparticles, carbon nanotubes and an organic carbon source as raw materials, and realizes the preparation of a high-silicon content and large-capacity negative electrode material under simple process conditions, thereby achieving both high performance and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 This is a schematic diagram of the preparation method of the carbon-silicon composite material according to Example 1 of the present invention.

[0041] Figure 2 This is a scanning electron microscope image of the pure carbon nanotubes used in Example 1 of the present invention.

[0042] Figure 3 This is a scanning electron microscope image of the silicon / titanium dioxide coating material prepared in Example 1 of the present invention.

[0043] Figure 4 This is a scanning electron microscope image (with logo) of the silicon / titanium dioxide coating material prepared in Example 1 of the present invention.

[0044] Figure 5 This is an electron microscope image of the nano-silicon used in Example 1 of the present invention.

[0045] Figure 6 This is a first cycle charge and discharge curve diagram of the carbon-silicon composite material prepared in Example 1 of the present invention.

[0046] Figure 7 This is a cycle curve diagram of the first 50 cycles of the carbon-silicon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0047] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.

[0048] Example 1

[0049] This embodiment provides a method for preparing a carbon-silicon composite material having an elastic nanostructure. Figure 1 The preparation process is as follows: carbon nanotubes are mixed with potassium permanganate to obtain functionalized carbon nanotubes; silicon-containing nanoparticles are mixed with tetra-n-butyl titanate and vacuum annealed to obtain silicon / titanium dioxide coating materials; finally, the functionalized carbon nanotubes are mixed with the silicon / titanium dioxide coating materials, polyvinyl alcohol is added and pyrolyzed to obtain carbon-silicon composite materials.

[0050] Specifically, the preparation steps are as follows:

[0051] (1) Preparation of functionalized carbon nanotubes

[0052] a. Use an electronic balance to take 10 g of carbon nanotubes (diameter: 30-50 nm; length: 10-20 μm; purity> 95wt%;) and 1 g of potassium permanganate, mix them evenly in a mortar, and place them together with the mortar into a closed crucible filled with argon.

[0053] b. Place the crucible in a tubular furnace, and in an argon atmosphere, heat it to 400°C at a heating rate of 1°C / min, and maintain the temperature at 400°C for 5 minutes to obtain a solid powder. After the furnace cools to room temperature, take out the solid powder.

[0054] c. Wash the solid powder with deionized water and centrifuge, repeat this process three times to remove excess salt components and obtain wet carbon nanotubes.

[0055] d. Dry the wet carbon nanotubes in a vacuum oven at 60°C to obtain functionalized carbon nanotubes.

[0056] (2) Synthesis of silicon / titanate coated materials

[0057] a. Weigh 10 g of nano-silicon powder (D50 is about 100 nm, the maximum is not more than 300 nm, and the minimum is not less than 10 nm) and disperse it evenly in 2 L of anhydrous ethanol by ultrasonication.

[0058] b. Add 0.5 g of tetra-n-butyl titanate to the anhydrous ethanol containing nano-silicon powder to form an ethanol dispersion with a mass ratio of nano-silicon powder to tetra-n-butyl titanate of 20:1.

[0059] c. Under stirring condition of 1000 rpm, slowly add 500 mL of ethanol-water solution with a volume ratio of 9:1 into the ethanol dispersion, continue stirring for 8 hours and then age overnight to obtain a precipitate.

[0060] d. The precipitate was dried in a vacuum oven at 60°C to obtain silicon / titanic acid coated particles.

[0061] (3) Preparation of silicon / titanium dioxide coating materials

[0062] The silicon / titanic acid coated particles prepared in step (2) are vacuum annealed in a vacuum furnace, the vacuum furnace is heated to 550°C at a heating rate of 2°C / min, and maintained at a constant temperature of 550°C for 20 minutes. The particles are cooled to room temperature and taken out to obtain a powdered silicon / titanium dioxide coated material.

[0063] (4) Preparation of pyrolysis precursor

[0064] 3 g of the silicon / titanium dioxide coating material obtained in step (3) was weighed and ultrasonically dispersed in 500 ml of deionized water, and 10 g of the functionalized carbon nanotubes obtained in step (1) were added to form a dispersion having a mass ratio of silicon / titanium dioxide coating material to functionalized carbon nanotubes of 3:10, and 1.5 g of polyvinyl alcohol having a mass fraction of 10% was added thereto. The dispersion was spray-dried so that the polyvinyl alcohol was wrapped and adhered to the surface of the silicon / titanium dioxide coating material and the functionalized carbon nanotubes to obtain a pyrolysis precursor. The spray drying conditions were as follows: an inlet temperature of 220°C, an outlet temperature of 120°C, and a feed rate of 10 mL / min.

[0065] (5) Preparation of carbon-silicon composite materials

[0066] The pyrolysis precursor in the above step (4) is placed in an argon atmosphere for pyrolysis, the temperature is raised to 800°C at a rate of 2°C / min, and the temperature is maintained at 800°C for 2 hours to fully pyrolyze the polyvinyl alcohol to obtain a black block-like carbon-silicon composite material. The black block-like carbon-silicon composite material is taken out and crushed through a 500-mesh sieve to obtain a powder-like carbon-silicon composite material.

[0067] In this embodiment, tetrabutyl titanate is controlled to hydrolyze and deposit on the surface of nano-silicon powder to form a silicon / titanic acid coating material through steps (2) and (3), and then a thin layer of titanium dioxide is formed on the surface of the nano-silicon powder by vacuum annealing. Then, through steps (4) and (5), polyvinyl alcohol is dispersed in the solution of silicon / titanium dioxide coating material and functionalized carbon nanotubes to form a uniform solution, which is then spray-dried and granulated. At the same time, the polyvinyl alcohol is wrapped and adhered to the surface of the silicon / titanium dioxide coating material and the functionalized carbon nanotubes. Through high-temperature pyrolysis, a carbon nanofilm and a continuous carbon nanotube network structure are formed on the titanium dioxide thin layer.

[0068] Example 2

[0069] The difference between this embodiment and embodiment 1 is that the heat treatment temperature in step (1) of embodiment 2 is 600° C., and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0070] Example 3

[0071] The difference between this embodiment and embodiment 1 is that the heat treatment temperature in step (1) of embodiment 3 is 800° C., and the other conditions are consistent with embodiment 1 to obtain a carbon-silicon composite material.

[0072] Example 4

[0073] The difference between this embodiment and embodiment 1 is that the heat treatment time in step (1) of embodiment 4 is 1 hour, and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0074] Example 5

[0075] The difference between this embodiment and embodiment 1 is that the heat treatment time in step (1) of embodiment 5 is 2 hours, and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0076] Example 6

[0077] The difference between this embodiment and embodiment 1 is that in step (3) of embodiment 6, the vacuum annealing temperature is 575° C., and the other conditions are the same as those of embodiment 1, to obtain a carbon-silicon composite material.

[0078] Example 7

[0079] The difference between this embodiment and embodiment 1 is that the vacuum annealing temperature in step (3) of embodiment 7 is 600° C., and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0080] Example 8

[0081] The difference between this embodiment and embodiment 1 is that the vacuum annealing time in step (3) of embodiment 8 is 30 minutes, and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0082] Example 9

[0083] The difference between this embodiment and embodiment 1 is that the vacuum annealing time in step (3) of embodiment 9 is 40 minutes, and the other conditions are the same as those of embodiment 1, thereby obtaining a carbon-silicon composite material.

[0084] Example 10

[0085] The difference between this embodiment and embodiment 1 is that in step (4) of embodiment 10, the hot organic carbon source is glucose, and the other conditions are the same as those of embodiment 1 to obtain a carbon-silicon composite material.

[0086] Embodiment 11

[0087] The difference between this embodiment and embodiment 1 is that in step (4) of embodiment 11, the hot organic carbon source is chitosan, and the other conditions are the same as those of embodiment 1 to obtain a carbon-silicon composite material.

[0088] Example 12

[0089] The difference between this embodiment and embodiment 1 is that in step (4) of embodiment 12, the hot organic carbon source is glucose and chitosan (the ratio of the two is 1:1), and the other conditions are consistent with embodiment 1 to obtain a carbon-silicon composite material.

[0090] Example 13

[0091] The difference between this embodiment and embodiment 1 is that in step (5) of embodiment 13, the pyrolysis temperature is 1000° C., and the other conditions are the same as those of embodiment 1, to obtain a carbon-silicon composite material.

[0092] Embodiment 14

[0093] The difference between this embodiment and embodiment 1 is that in step (5) of embodiment 14, the pyrolysis temperature is 1200° C., and the other conditions are the same as those of embodiment 1, to obtain a carbon-silicon composite material.

[0094] Embodiment 15

[0095] The difference between this embodiment and embodiment 1 is that in step (5) of embodiment 15, the pyrolysis temperature is 1400° C., and the other conditions are the same as those of embodiment 1, to obtain a carbon-silicon composite material.

[0096] Example 16

[0097] The difference between Example 16 and Example 1 is that in step (1) of Example 16, the silicon source is SiO, and the other conditions are consistent with Example 1, to obtain a carbon-silicon composite material.

[0098] Embodiment 17

[0099] The difference between Example 2 and Example 1 is that in step (1) of Example 17, the silicon source is a mixture of Si and SiO in a mass ratio of 1:1, and the other conditions remain the same as in Example 1 to obtain a carbon-silicon composite material.

[0100] Embodiment 18

[0101] The difference between Example 3 and Example 1 is that in step (1) of Example 18, the silicon source is SiO x (wherein 0<X<1), and the other conditions are consistent with those in Example 1 to obtain a carbon-silicon composite material.

[0102] Comparative Example 1

[0103] The difference between this comparative example and Example 1 is that the heat treatment temperature in step (1) is 300° C., and the other conditions are the same as those in Example 1, to obtain a carbon-silicon composite material.

[0104] Comparative Example 2

[0105] The difference between this comparative example and Example 1 is that the pyrolysis temperature in step (5) is 600° C., and the other conditions are the same as those in Example 1, to obtain a carbon-silicon composite material.

[0106] Performance Characterization and Data Analysis

[0107] The carbon-silicon composite material prepared in Example 1 was observed for its morphology using a scanning electron microscope (SEM). Figure 2 , Figure 3 Obviously, the titanium dioxide-coated silicon particles are attached to the functionalized carbon nanotubes, and the irregular filling of the continuous functionalized carbon nanotubes forms a network structure, resulting in a large number of voids in the material, which is conducive to adapting to the volume expansion effect of silicon-containing particles. At the same time, the size of the nanoparticles is between 50-200nm, which is consistent with the particle size of the raw silicon powder.

[0108] The elastic titanium dioxide thin layer and carbon nanolayer wrap the silicon-containing particles therein, and when the silicon-containing particles expand in volume, elastic deformation is generated to adapt to the expansion of the silicon-containing particles so that the silicon-containing particles are not in contact with the electrolyte. Carbon-carbon bonds are formed between the carbon nanolayer and the functionalized carbon nanotubes, so that the silicon-containing particles coated with the titanium dioxide thin layer are anchored on the functionalized carbon nanotubes. Combined with the high elasticity of the functionalized carbon nanotube network, the large volume expansion of the nanoparticles containing the silicon component is stabilized in the gaps of these elastic structures, thereby obtaining an electrochemically stable high-capacity negative electrode material.

[0109] The first cycle charge and discharge performance of the carbon-silicon composite material prepared in Example 1 was tested.

[0110] See also Figure 4 , is the first cycle charge and discharge curve of the carbon-silicon composite material prepared in Example 1 (under 0.2C delithiation / 0.2C lithium insertion conditions). The test shows that the first cycle charge and discharge capacities of the prepared carbon-silicon composite material are 740.4mAh / g and 959.8mAh / g, respectively, corresponding to a first cycle coulombic efficiency of 77.1%. When lithium is inserted, there is a weak peak at 1.2V corresponding to the beginning of SEI formation.

[0111] See also Figure 5 , which is the cycle curve of the carbon-silicon composite material prepared in Example 1 for the first 50 cycles, indicating that the carbon-silicon composite material still has a reversible capacity of 582 mAh / g and an irreversible capacity of 598 mAh / g after 50 cycles.

[0112] The carbon-silicon composite materials prepared in the examples and embodiments were assembled into CR2025 type button half-cells to test the electrochemical performance.

[0113] The specific assembly process is as follows: lithium metal sheet is used as the counter electrode; 1M Li PF6 / EC∶DEC∶DMC (1∶1∶1) + 1% FEC is used as the electrolyte; polypropylene microporous membrane is used as the separator; active material, CE-300j, sodium carboxymethyl cellulose (CMC), and styrene-butadiene latex (SBR) are prepared into slurry according to the mass ratio of 8∶1∶0.5∶0.5, evenly coated on carbon-coated copper foil and placed in a vacuum drying oven at 80℃ for 4h to make electrode sheets. The battery is assembled in a glove box filled with Ar gas. The model of the battery test system is LAND CT3002A, and the voltage range is 0.001~2V.

[0114] The mass fraction of Si and the lithium storage performance of the samples prepared in the above examples and embodiments are shown in Table 1.

[0115] Table 1. Mass fraction of silicon-carbon composite materials and lithium storage capacity implementation table

[0116]

[0117]

[0118] Referring to Table 1, it can be seen from the data of Examples 1-18 in Table 1 that the functionalized carbon nanotube composite titanium dioxide-coated nano-silicon improves the stability of the silicon-carbon composite material to a certain extent.

[0119] Specifically, the test results of Examples 1-5 show that carbon nanotubes treated with different oxidation conditions have different effects on the electrochemical properties of the final silicon-carbon material. Moderate oxidation increases the cycle stability of the negative electrode material. Too short or too long an oxidation time will cause a decrease in battery capacity, first efficiency and cycle stability. Too short an oxidation time results in too few oxygen-containing functional groups grafted onto the surface of the carbon nanotubes, and only a small number of silicon dioxide-coated silicon particles produce a "pinning" effect. At the same time, the bond force between the carbon nanotubes is insufficient, and an effective spatial network cannot be formed to inhibit the expansion effect of silicon. The SEI film formed by the battery cycle is unstable. These reasons lead to a decrease in cycle performance; too long an oxidation time causes the content of oxygen-containing functional groups on the surface of the carbon nanotubes to be too high, inducing the formation of a tighter interaction layer during pyrolysis, reducing the reserved expansion space, resulting in a decrease in the cyclability of the battery. At the same time, too high an oxygen content will also reduce the silicon content in the silicon-carbon composite material. The moderately oxidized functionalized carbon nanotubes avoid the above disadvantages to a certain extent, forming a continuous conductive network in space, reducing the contact resistance between the two, making the charge transfer more efficient, and at the same time, the reserved space provides a guarantee for the growth of a stable SEI film and the expansion of silicon-based materials. The 300°C heat treatment used in Comparative Example 1 cannot completely functionalize the carbon nanotubes, resulting in poor overall electrochemical performance.

[0120] Examples 1, 6-9 show the effect of the amount of deposited titanium dioxide on the electrochemical performance of the final battery. Titanium dioxide deposited on the silicon surface is not only conducive to separating nano-silicon from the electrolyte and forming a stable SEI film, but also slows down the oxidation of the nano-silicon surface to a certain extent, preventing the nano-silicon particles from catalyzing other side reactions due to their large specific surface area; on the other hand, the mechanical strength of titanium dioxide can alleviate the expansion effect caused by silicon nanoparticles when lithium is embedded.

[0121] The vacuum annealing temperature and time of titanium dioxide coated nano-silicon also have a certain effect on the electrochemical performance of the negative electrode material. Example 7 uses a higher temperature annealing, and the titanium dioxide precursor titanic acid loses water quickly, resulting in poor coating effect on nano-silicon, and ultimately reduces the electrochemical performance of the battery. The vacuum annealing time of Example 1 is relatively short, resulting in insufficient dehydration time of titanic acid, and its first effect and capacity retention rate are less than those of Example 8, but the annealing time of Example 9 is too long, resulting in its silicon-carbon material cycle performance being worse than that of Example 1.

[0122] The choice of organic carbon source also affects the electrochemical properties of the negative electrode material. The glucose used in Example 10 is more conducive to improving the cycle performance, but the capacity of the battery is small. The carbon-silicon composite materials prepared from other organic carbon sources have their own advantages and disadvantages. Taking all factors into consideration, polyvinyl alcohol is the best organic carbon source. Examples 13-14 show that a suitable sintering temperature is beneficial to improving the capacity and first efficiency of the half-cell. Too low or too high a temperature will result in poor electrochemical performance. In Comparative Example 2, the pyrolysis temperature is 600°C. Due to incomplete pyrolysis, the first efficiency of the prepared silicon-carbon composite material is low, and the capacity retention rate is lower than the performance of any silicon-carbon composite material prepared in Examples 1-18.

[0123] The examples explore the effects of different silicon sources on the performance of silicon-carbon materials. Example 16 has a low first efficiency of silicon-carbon negative electrode material due to the poor intrinsic first coulombic efficiency of silicon monoxide, but the cyclability is close to that of Example 1; Example 17 has improved capacity and first coulombic efficiency, but the cyclability decreases significantly; Example 3 has a slightly higher first coulombic efficiency and capacity than Example 18 because of the low oxygen content in the silicon source. In summary, the preferred raw material for the silicon-carbon material prepared by this method is pure silicon particles.

[0124] In summary, the present invention provides a carbon-silicon composite material with an elastic nanostructure. The structural design of the composite material utilizes the elastic properties of the ultra-thin titanium dioxide coating layer and the ultra-thin carbon coating layer. During the battery charging and discharging stage, the silicon particles are protected from contact with the electrolyte during the volume expansion process of the silicon particles. Combined with the high elasticity of the carbon nanotube network, the nanoparticles containing silicon components are expanded in large volumes and stabilized in the gaps of these elastic structures, thereby obtaining an electrochemically stable high-capacity negative electrode material. The preparation process is simple, the equipment requirements are low, and it is easy to promote.

Claims

1. A carbon-silicon composite material with an elastic nanostructure, characterized in that: The carbon-silicon composite material has a first elastic unit and a second elastic unit; The first elastic unit comprises a titanium dioxide thin layer and a carbon nano-thin layer sequentially wrapped on the surface of the silicon-containing particles; wherein the titanium dioxide thin layer and the carbon nano-thin layer are both elastic; The second elastic unit is a continuous carbon nanotube network structure formed by functionalized carbon nanotubes; In the first elastic unit, the elastic effect of the titanium dioxide thin layer and the carbon nano thin layer is utilized to constrain the silicon-containing particles after volume expansion inside the first elastic unit, so that the silicon-containing particles are not in contact with the electrolyte; at the same time, the second elastic unit constrains the first elastic unit within the network structure of the second elastic unit when the volume expands.

2. The carbon-silicon composite material with elastic nanostructure according to claim 1, characterized in that: A carbon-carbon chemical bond is formed between the carbon nanofilm and the functionalized carbon nanotubes, thereby constraining the first elastic unit within the network structure of the second elastic unit; The functionalized carbon nanotubes are irregularly filled to form a continuous network structure, resulting in a large number of voids in the carbon silicon material, which is conducive to accommodating the volume expansion of the first elastic unit.

3. The carbon-silicon composite material with elastic nanostructure according to claim 1 or 2, characterized in that: The preparation method of the first elastic unit includes coating titanium dioxide on the surface of silicon-containing particles to form a titanium dioxide thin layer; an organic carbon source is coated and adhered to the surface of the titanium dioxide thin layer and the functionalized carbon nanotubes, and after pyrolysis, the organic carbon source forms a carbon nano-thin layer on the surface of the titanium dioxide thin layer, thereby forming a titanium dioxide thin layer-carbon nano-thin layer sequentially coated on the surface of the silicon-containing particles from the inside to the outside; The functionalized carbon nanotubes form a continuous carbon nanotube network structure as the second elastic unit.

4. A method for preparing the carbon-silicon composite material with elastic nanostructure as claimed in claims 1 to 3, characterized in that: The following steps are involved: S1. Preparation of functionalized carbon nanotubes: mixing carbon nanotubes with an oxidant and then heat treating to obtain functionalized carbon nanotubes; S2. Preparation of silicon / titanate coated material: dispersing silicon-containing particles in an organic solvent, and then adding an organic titanium source to dissolve to obtain a silicon / titanate coated material; S3. Preparation of silicon / titanium dioxide coated material: vacuum annealing the silicon / titanate coated material in S2 to obtain a silicon / titanium dioxide coated material; S4. Preparing a precursor: mixing the functionalized carbon nanotubes described in S1 and the silicon / titanium dioxide coating material described in S3 with an organic carbon source and spray drying the mixture, so that the organic carbon source is wrapped and adhered to the silicon / titanium dioxide coating material and the surface of the functionalized carbon nanotubes to obtain a precursor; S5. Making a carbon-silicon composite material: pyrolyzing the precursor described in S4 to obtain a carbon-silicon composite material.

5. The method for preparing the carbon-silicon composite material with elastic nanostructure according to claim 4, characterized in that: The heat treatment temperature is 400-800°C, and the heat treatment time is 5-120 minutes; And / or, the temperature during the vacuum annealing is 550-600° C., and the time of the vacuum annealing is 20-40 minutes; and / or, the oxidant comprises potassium permanganate; And / or, the organic solvent comprises anhydrous ethanol; And / or, the organic titanium source includes tetra-n-butyl titanate.

6. The method for preparing the carbon-silicon composite material with elastic nanostructure according to claim 5, characterized in that: The organic carbon source includes any one of polyvinyl alcohol, glucose, fructose, polyvinyl pyrrolidone and chitosan, or a combination of two or more thereof.

7. The method for preparing the carbon-silicon composite material with elastic nanostructure according to claim 6, characterized in that: The mass ratio of the silicon / titanium dioxide coating material to the functionalized carbon nanotubes in S4 is 0.3-0.5:1; And / or, the mass of the organic carbon source in S4 accounts for 10%-20% of the mixed mass. And / or, in S5, the pyrolysis temperature is 800-1400°C.

8. The method for preparing the carbon-silicon composite material with elastic nanostructure according to claim 7, characterized in that: The diameter of the carbon nanotubes is 30-50 nanometers; And / or, the particle size of the silicon-containing nanoparticles ranges from 10 to 300 nanometers.

9. The method for preparing the carbon-silicon composite material with elastic nanostructure according to claim 8, characterized in that: The carbon nanotubes and the oxidant are mixed in a mass ratio of 10:1; And / or, the silicon-containing nanoparticles include: elemental silicon, silicon dioxide or SiOx, wherein 0<X<1; And / or, the mass ratio of the organic titanium source to the silicon-containing nanoparticles is 0.02-0.1:

1.

10. Use of the carbon-silicon composite material with elastic nanostructure as claimed in any one of claims 1 to 3, or the carbon-silicon composite material prepared by the preparation method as claimed in any one of claims 4 to 9 in the negative electrode of a lithium-ion battery.