Negative active material and rechargeable lithium battery including same

By using agglomerated natural graphite and artificial graphite negative electrode active materials in rechargeable lithium batteries, combined with amorphous carbon coating, the stability and expansion problems of lithium batteries during high-rate charging and discharging are solved, and their circulation is significantly improved Lifespan and efficiency.

CN118943315APending Publication Date: 2024-11-12SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410560617.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-05-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing rechargeable lithium batteries exhibit unstable cycle life and volume expansion characteristics during high-rate charging and discharging, affecting their application performance.

Method used

The negative electrode active material composed of tripartite particles of natural graphite, artificial graphite and amorphous carbon coating layer is used to increase the lithium ion embedding site through agglomeration and spheroidization processes, and combine the amorphous carbon coating layer to reduce resistance and volume expansion.

Benefits of technology

It significantly improves the cycle life, charging and discharging efficiency and high-speed magnification capabilities of lithium batteries, reduces volume expansion and resistance, and improves overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943315A_ABST
    Figure CN118943315A_ABST
Patent Text Reader

Abstract

A negative active material for a rechargeable lithium battery and a rechargeable lithium battery including the same are provided. The negative active material includes a first active material including tertiary particles of natural graphite in which the secondary particles agglomerate. The primary particles are agglomerated and spheroidized in the secondary particles. The artificial graphite is positioned on the surfaces of the primary particles and the surfaces of the secondary particles. The amorphous carbon coating layer surrounds the tertiary particles of natural graphite. Further, the negative electrode active material includes a second active material including a carbon-based material having an aspect ratio of about 2 to about 100.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure relate to a negative active material and a rechargeable lithium battery including the negative active material. Background Art

[0002] Recently, the rapid development of electronic devices (such as mobile phones, laptop computers, and electric vehicles) using batteries has led to a dramatic increase in demand for rechargeable batteries with relatively high capacity and light weight. For example, because rechargeable lithium batteries have light weight and high energy density, rechargeable lithium batteries have recently attracted attention as driving power sources for portable devices. Therefore, research to improve the performance of rechargeable lithium batteries is being actively conducted. Summary of the invention

[0003] The embodiments relate to negative electrode active materials exhibiting improved high-rate characteristics.

[0004] Some embodiments relate to a rechargeable lithium battery including the negative active material.

[0005] An embodiment can be implemented by providing a negative electrode active material including a first active material, the first active material including tertiary particles of natural graphite, and the secondary particles agglomerated in the tertiary particles of natural graphite. The primary particles agglomerated and spheroidized in the secondary particles. Artificial graphite is positioned on the surface of the primary particles and the surface of the secondary particles. An amorphous carbon coating layer surrounds the tertiary particles of natural graphite. The negative electrode active material also includes a second active material, and the second active material includes a carbon-based material having an aspect ratio of about 2 to about 100.

[0006] Embodiments may be implemented by providing a rechargeable lithium battery including a negative electrode including a negative active material, a positive electrode, and an electrolyte.

[0007] In some embodiments, the second active material may have an aspect ratio of about 2 to about 50.

[0008] In some embodiments, the amount of the second active material may be about 10 weight percent (wt %) to about 30 wt % based on the total 100 wt % of the negative active material.

[0009] In some embodiments, the second active material may include artificial graphite.

[0010] In some embodiments, the second active material may have an average length of a major axis of about 40 μm to about 120 μm.

[0011] In some embodiments, in the negative electrode active material, an area ratio of the second active material may be about 10% to about 40% based on 100% of the total area of ​​the negative electrode active material.

[0012] In some embodiments, the natural graphite may be flake natural graphite.

[0013] In some embodiments, the negative active material has an orientation index of about 40 to about 90.

[0014] In some embodiments, the negative active material may have a mercury cumulative pore volume of about 1.5 mL / g to about 3 mL / g.

[0015] In some embodiments, the second active material may have a rod shape.

[0016] In some embodiments, in the first active material, an amount of the amorphous carbon coating layer may be about 0.01 wt % to about 5 wt % based on the total 100 wt % of the first active material.

[0017] In some embodiments, in the first active material, an amount of the artificial graphite may be about 9 wt % to about 16.5 wt % of the total 100 wt % of the first active material.

[0018] In some embodiments, in the first active material, an amount of the natural graphite may be about 78.5 wt % to about 89 wt % based on the total 100 wt % of the first active material.

[0019] In some embodiments, the first active material may have a tap density of about 0.8 g / cc to about 1.1 g / cc.

[0020] In some embodiments, the amorphous carbon coating layer may include at least one of soft carbon, hard carbon, mesophase pitch carbide, burned coke, baked coke, and mixtures thereof.

[0021] The negative active material according to some embodiments may exhibit excellent cycle-life characteristics and reduced volume expansion characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Features will become apparent to those skilled in the art by describing in detail exemplary embodiments with reference to the accompanying drawings, in which:

[0023] Figure 1 is a schematic diagram showing the structure of a second active material according to some embodiments;

[0024] Figure 2A shows the structure of a first active material according to some embodiments;

[0025] Figure 2B The tertiary particles of natural graphite are shown. Figure 2A The structure of the first active substance shown in ;

[0026] Figure 3is a schematic perspective view showing a rechargeable lithium battery according to some embodiments;

[0027] Figure 4 is a SEM (scanning electron microscope) image of the negative electrode active material according to Example 1;

[0028] Figure 5 is a SEM image of the negative electrode active material according to Comparative Example 1; and

[0029] Figure 6 is a graph showing resistances of different densities of active materials according to Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0030] Hereinafter, example embodiments will now be described more fully with reference to the accompanying drawings; however, they may be implemented in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the exemplary implementation scheme to those skilled in the art.

[0031] In the drawings, the dimensions of layers and regions may be exaggerated for clarity. It will also be understood that if a layer or element is referred to as being "on" another layer or substrate, it can be directly on the other layer or substrate, or there may be intervening layers or elements. Additionally, it will be understood that if a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or there may be one or more intervening layers. Like reference numerals refer to like elements throughout.

[0032] In the present disclosure, unless the context clearly indicates otherwise, if no definition is otherwise provided, expressions in the singular include expressions in the plural. Unless otherwise defined, "A or B" may mean "including A or B", or "including both A and B".

[0033] In the present disclosure, unless otherwise defined in the specification, particle diameter can be an average particle diameter. Particle diameter represents an average particle diameter or average particle size (D50) with a cumulative volume of about 50 volume % in a particle size distribution. Average particle size (D50) can be measured by methods well known to those skilled in the art (e.g., by a particle size analyzer or by a transmission electron microscope image or a scanning electron microscope image). Alternatively, a dynamic light scattering measuring device is used for data analysis, and the number of particles is counted for each size range, thereby the average particle diameter (D50) value can be easily obtained by calculation. Average length and average thickness can be measured by using the same method as measuring "particle diameter".

[0034] The “aspect ratio” used herein may refer to a maximum aspect ratio or an average aspect ratio, and may be determined through a SEM image.

[0035] As used herein, the term "soft carbon" refers to a graphitizable carbon material and is easily graphitized by heat treatment at high temperature (e.g., 2800° C.), and "hard carbon" refers to a non-graphitizable carbon material and is slightly graphitized by heat treatment.

[0036] Crystalline carbon and amorphous carbon can be distinguished by XRD measurement. Natural graphite, which is a type of crystalline carbon, can be produced by reprocessing a mineral made by growing crystals under long-term heating and pressure. If measured by XRD (for example, when measured by XRD), the interplanar spacing (d 002) of the (002) plane can be to Artificial graphite, which is another type of crystalline carbon, can be produced by graphitization, and if measured by XRD (for example, when measured by XRD), the interplanar spacing (d 002) of the (002) plane can be to On the other hand, amorphous carbon may be a material made of carbon excluding natural graphite and artificial graphite, and if measured by XRD (for example, when measured by XRD), the interplanar spacing (d002) of the (002) plane may be or smaller.

[0037] XRD can be measured using an apparatus using CuKα radiation as a target line (e.g., product name: X'Pert, manufacturer: Malvern Panalytical). XRD measurement conditions can be: 2θ is 10° to 80°, the scanning speed (° / S) is 0.044 to 0.089, and the step length (° / step) is 0.013 to 0.039. For peak intensity resolution (peak intensity), the monochromator device can be removed to improve resolution.

[0038] The negative active material according to some embodiments includes a first active material 1 and a second active material.

[0039] The first active material 1 may include, for example, tertiary particles 7 of natural graphite, in which secondary particles 5 are agglomerated. The secondary particles 5 may be prepared by agglomerating and spheroidizing the primary particles 3. The artificial graphite 9 may be positioned on the surfaces of the primary particles 3 and the secondary particles 5. The amorphous carbon coating layer 11 may surround the tertiary particles 7 of natural graphite.

[0040] The second active material may be a carbon-based material having an aspect ratio of about 2 to about 100 (eg, a maximum aspect ratio of about 2 to about 100).

[0041] Thus, in some embodiments, the negative electrode active material may include a first active material 1 agglomerated from natural graphite and artificial graphite, and may have a substantially spherical shape. The second active material may have an aspect ratio of about 2 to about 100 (e.g., a maximum aspect ratio of about 2 to about 100) and an elongated shape.

[0042] Embodiments using negative active materials can exhibit and enjoy fast charging and long cycle life characteristics due to including the first active material 1, while also exhibiting and benefiting from reduced volume expansion during charging and discharging, reduced resistance, and improved high rate capability by including the second active material.

[0043] Based on the total 100wt% of the negative electrode active material, the amount of the second active material may be about 10 weight percent (wt%) to about 30wt% or about 20wt% to about 30wt% (e.g., based on the total 100wt% of the negative electrode active material, the amount of the second active material may be about 10wt% to about 20wt%, about 12wt% to about 18wt% or about 14wt% to about 16wt%). If the amount of the second active material in the negative electrode active material is within this range, increased positive effects and results may be obtained due to the inclusion of the second active material.

[0044] The second active material may be artificial graphite. If artificial graphite is included as the second active material, the artificial graphite may further improve charging and discharging efficiency and cycle life characteristics compared to natural graphite.

[0045] In one embodiment, the second active material is rod-shaped crystalline carbon. Rod-shaped refers to a shape that is long in one direction. Figure 1 As shown in , it represents a rod shape having a major axis A and a minor axis B. The rod type refers to a rod shape whose interior is substantially filled, and is different from a hollow or fiber shape having a major axis and a minor axis but being empty inside.

[0046] The rod type has an aspect ratio greater than 1, and the aspect ratio is the ratio of the length of the major axis / the length of the minor axis. The second active material according to some embodiments may be a carbon-based material having an aspect ratio (e.g., a maximum aspect ratio) of about 2 to about 100, about 2 to about 50, about 2 to about 20, about 2 to about 15, or about 5 to about 10. If the aspect ratio of the second active material is within this range, the resistance and volume expansion of the negative electrode 20 during charge and discharge can be further reduced, and the high rate characteristics can be further improved.

[0047] The long diameter of the second active material may be about 40 μm to about 120 μm or about 50 μm to about 120 μm (e.g., about 50 μm to about 100 μm, about 50 μm to about 90 μm, about 50 μm to about 80 μm, about 50 μm to about 70 μm; about 60 μm to about 100 μm, about 60 μm to about 90 μm, about 60 μm to about 80 μm, or about 60 μm to about 70 μm). If the long diameter of the second active material is within this range, the resistance and volume expansion of the negative electrode 20 during charge and discharge can be further reduced, and the high rate characteristics can be further improved.

[0048] The major diameter is the average length of the major axis, for example, Figure 1 The dimension of the major axis A of the rod (rod) carbon shown in FIG.

[0049] In the negative active material according to some embodiments, the area ratio of the second active material may be about 10% to about 40% or about 20% to about 30% based on 100% of the total area of ​​the negative active material (for example, the area ratio of the second active material may be about 15% to about 30%, about 16% to about 25%, or about 17% to about 23% based on 100% of the total area of ​​the negative active material). The area ratio may be measured by using a particle size analyzer and represents the ratio of the area occupied by the second active material per unit area of ​​the negative active material.

[0050] According to some embodiments, the structure of the first active material 1 is Figure 2A Shown in. Figure 2A The right part of shows an enlarged view of the secondary particle 5 corresponding to the dotted line. The first active material 1 according to some embodiments includes secondary particles 5 and tertiary particles 7 of natural graphite, a plurality of primary particles 3 are agglomerated and spheroidized in the secondary particles 5, and the secondary particles 5 are agglomerated in the tertiary particles 7 of natural graphite. An amorphous carbon coating layer 11 is included around the tertiary particles 7 of natural graphite. Artificial graphite 9 is positioned on the surface of the primary particles 3 and the surface of the secondary particles 5.

[0051] Figure 2B More clearly shown Figure 2A Tertiary particles of natural graphite7.

[0052] Crystalline carbon (specifically, natural graphite) used as a negative electrode active material has a higher capacity than artificial graphite, so it can achieve an ideal capacity close to the theoretical capacity. However, natural graphite includes large-sized particles with a particle size of about 40 μm to about 120 μm, so it is subjected to a spheroidization process for use as a negative electrode active material. This negative electrode active material includes limited sites where intercalation and deintercalation can occur, and therefore may exhibit inappropriate charge and discharge characteristics (e.g., inappropriate high-rate charge and discharge characteristics).

[0053] The first active material 1 according to some embodiments includes secondary particles 5, tertiary particles 7, and artificial graphite 9, the primary particles 3 of crushed natural graphite are agglomerated and spheroidized in the secondary particles 5, the secondary particles 5 are agglomerated in the tertiary particles 7, and the artificial graphite 9 is positioned on the surface of the primary particles 3 and the surface of the secondary particles 5. Therefore, the sites for lithium ion insertion and extraction can be increased, and therefore, the movement of lithium ions can be promoted. In this way, the negative active material according to some embodiments can exhibit improved fast charging and discharging characteristics.

[0054] In some embodiments, the natural graphite may be a flake natural graphite that can facilitate lithium ion insertion. According to another embodiment, the flake natural graphite may be a small-sized flake natural graphite. If the natural graphite is a small-sized flake natural graphite, the sites where lithium ions can be inserted and removed in the same area increase, and the channels through which lithium ions can transfer become shorter, making it more suitable for fast charging and discharging.

[0055] The first active material 1 according to some embodiments is prepared by spheroidizing and bending the small-sized primary particles 3, so that lithium ions can be embedded in the negative electrode active material, for example, not only in both ends of the flaky natural graphite, but also in the bent portion. In this way, the negative electrode active material according to some embodiments includes increased lithium ion embedding sites. Therefore, improved charging capability (particularly, high rate charging capability) can be exhibited.

[0056] The primary particles 3 may have a particle size of about 4 μm to about 8 μm. The particle size of the primary particles 3 may be, for example, about 4 μm to about 8 μm, about 4 μm to about 7 μm, or about 4 μm to about 6 μm. The particle size of the primary particles 3 (e.g., an average particle size such as D50) may be, for example, about 4 μm to about 6 μm, about 4.5 μm to about 5.5 μm, or about 4.5 μm to about 5 μm.

[0057] The secondary particles 5 may have a particle size of about 5 to about 10 μm. The particle size of the secondary particles 5 may be, for example, about 6 to about 10 μm, about 6 to about 8 μm, or about 7 to about 8 μm (eg, about 6 to about 7 μm).

[0058] The tertiary particles 7 may have a particle size of about 9 to about 15 μm, for example, about 9.2 to about 15 μm or about 9.5 to about 15 μm (eg, about 10 to about 12 μm or about 10 to about 11 μm).

[0059] If the particle size of the primary particle 3 is in the range of about 4 μm to about 8 μm, the secondary particle 5 can be easily prepared, the cycle life characteristics can be further improved, and the primary particle 3 can be easily used in the rechargeable lithium battery 100. If the particle size of the secondary particle 5 is about 5 μm to about 10 μm, the secondary particle 5 can easily form the tertiary particle 7 and can be easily used in the rechargeable lithium battery 100. If the particle size of the tertiary particle 7 is about 9 μm to about 15 μm, excellent initial efficiency can be exhibited, and excellent charge and discharge characteristics of the negative electrode 20 can be exhibited, which can be easily applied to the rechargeable lithium battery 100.

[0060] In the negative active material according to some embodiments, the thickness (e.g., average thickness) of the amorphous carbon coating layer 11 may be about 5 nm to about 50 nm (e.g., about 10 nm to about 50 nm or about 20 nm to about 50 nm). The amorphous carbon coating layer 11 having a thickness within this range may more effectively suppress side reactions with the electrolyte and may improve charge and discharge rate capability.

[0061] The first active material 1 including the primary particles 3, the secondary particles 5, and the tertiary particles 7 having a particle size within a specified range and the amorphous carbon coating layer 11 having a thickness within a specified range may have a particle size of about 9.05 μm to about 16 μm. The particle size of the first active material 1 may be, for example, about 9.05 μm to about 16 μm, about 9.2 μm to about 15.5 μm, or about 9.5 μm to about 15 μm (e.g., about 10 μm to about 12 μm or about 10 μm to about 11 μm). If the particle size of the first active material 1 is within this range, the volume expansion of the negative electrode 20 during charge and discharge can be more effectively suppressed, and the high rate characteristics can be further improved.

[0062] In some embodiments, the secondary particles 5 are formed by agglomerating a plurality of primary particles 3. The secondary particles 5 can be formed by agglomerating, for example, about 2 to about 30, about 2 to about 20, about 2 to about 10, or about 2 to about 4 primary particles 3. In some embodiments, the tertiary particles 7 are formed by agglomerating the secondary particles 5. The tertiary particles 7 can be formed by agglomerating, for example, about 2 to about 20, about 2 to about 10, or about 2 to about 4 secondary particles 5.

[0063] In some embodiments, the amount of artificial graphite 9 may be about 9 wt% to about 16.5 wt%, about 9 wt% to about 15 wt%, or about 10 wt% to about 14.5 wt% based on the total 100 wt% of the first active material (e.g., the amount of artificial graphite 9 may be about 10 wt% to about 14 wt%, about 10 wt% to about 13 wt%, or about 10 wt% to about 12 wt% based on the total 100 wt% of the first active material). In some embodiments, because the artificial graphite 9 is positioned on the surface of the primary particles 3 and the surface of the secondary particles 5, the artificial graphite 9 in the above range may increase the density of the interior of the negative active material. Since the first active material 1 according to some embodiments includes the secondary particles 5 and the tertiary particles 7, the primary particles 3 are agglomerated and spheroidized in the secondary particles 5, and the secondary particles 5 are agglomerated in the tertiary particles 7, the artificial graphite 9 (e.g., the artificial graphite 9 in the above specified range) filled into the space that may be formed between the particles may fill the space more fully. This enables the interior of the negative active material to be dense.

[0064] In some embodiments, based on the total 100 wt % of the first active material 1, the amount of natural graphite can be about 78.5 wt % to about 89 wt %, about 80 wt % to about 88.5 wt % or about 80.5 wt % to about 88 wt % (for example, based on the total 100 wt % of the first active material 1, the amount of natural graphite can be about 81 wt % to about 88 wt %, about 82 wt % to about 88 wt %, about 83 wt % to about 88 wt %, about 84 wt % to about 88 wt % or about 85 wt % to about 88 wt %).

[0065] The first active material 1 according to one embodiment may have an orientation index (OI) of about 40 to about 90, about 45 to about 90, or about 50 to about 90 (e.g., about 60 to about 90, about 70 to about 90, or about 80 to about 90). The first active material 1 may have an orientation index within a specified range, which indicates that it is randomly oriented similarly to artificial graphite. Therefore, the first active material 1 according to some embodiments may exhibit an excellent charging ability similar to that of artificial graphite.

[0066] In one or more embodiments, the orientation index can be obtained by X-ray diffraction analysis using CuKα rays, for example, as the ratio of the peak intensity at the (002) plane to the peak intensity at the (110) plane (I 002 / I 110 )get.

[0067] The negative active material of some embodiments may have a mercury cumulative pore volume (Hg cumulative pore volume) of about 1.5 mL / g to about 3 mL / g, about 2 mL / g to about 3 mL / g, or about 2 mL / g to about 2.8 mL / g (e.g., about 2.1 mL / g to about 2.5 mL / g or about 2.2 mL / g to about 2.4 mL / g). The mercury cumulative pore volume within this range indicates that the pores (e.g., empty spaces) inside the negative active material are small. The pores measured in the pore volume may have a pore size of about 0.01 μm to about 1 μm.

[0068] If the mercury cumulative pore volume is within a specified range, the electrolyte may be sufficiently impregnated to promote charge and discharge reactions, and a side reaction between the negative electrode active material and the electrolyte may not increase.

[0069] In some embodiments, mercury cumulative pore volume can be obtained by adding mercury to the negative active material, applying a pressure of about 0.1 psi to about 60,000 psi to inject mercury into the negative active material, and measuring the volume change of mercury according to the pressure change. The pressure change can be obtained by adjusting the pressure from about 0.1 psi to about 0.2 psi to about 50,000 psi to 60,000 psi.

[0070] Therefore, the first active material 1 according to some embodiments can have the following advantages: high capacity, good compression properties, and excellent pellet density from using natural graphite; improved high-rate charging capability from providing increased lithium ion insertion sites by including the secondary particles 5 in which the small-sized primary particles 3 are agglomerated; and high-rate charging capability of the artificial graphite 9. The effect of improving the charge and discharge rate characteristics by including the amorphous carbon coating layer 11 can also be obtained.

[0071] The amorphous carbon coating layer may be at least one of soft carbon, hard carbon, mesophase pitch carbide, burnt coke, baked coke, and mixtures thereof. In some embodiments, the amount of the amorphous carbon coating layer may be about 0.01 wt % to about 5 wt % based on the total 100 wt % of the first active material 1 (e.g., the amount of the amorphous carbon coating layer may be about 0.1 wt % to about 4 wt %, about 1 wt % to about 4 wt %, or about 2 wt % to about 3 wt % based on the total 100 wt % of the first active material 1).

[0072] The first active material 1 may have a tap density of about 0.8 g / cc to about 1.1 g / cc (e.g., about 0.9 g / cc to about 1.1 g / cc). If the first active material 1 has a tap density within a specified range, the internal pore volume of the first active material 1 and the side reaction with the electrolyte may be reduced, thereby improving the cycle life characteristics of the battery.

[0073] In one or more embodiments, a pressure of about 108 N is applied by using a GeoPyc 1360 pycnometer available from Micromeritics Instruments Corporation (inserting a GeoPyc 1360 pycnometer having a diameter of about 19.1 mm and having a diameter of 0.2907 cm 3 / mm of the cavity), the tap density can be obtained by averaging the values ​​obtained by three measurements.

[0074] Based on the total 100wt% of the negative electrode active material, the amount of the first active material can be about 70 weight percent (wt%) to about 90wt% or about 70wt% to about 80wt% (for example, based on the total 100wt% of the negative electrode active material, the amount of the first active material can be about 80wt% to about 90wt%, about 82wt% to about 88wt% or about 84wt% to about 86wt%).

[0075] The first active material 1 can be prepared through the following steps.

[0076] The size can be reduced by pulverizing a natural graphite raw material having a particle size of about 80 μm or more into primary particles 3. The natural graphite raw material can be pulverized into primary particles 3 by a jet milling method. 2 About 20kg / cm 2 Air flow grinding is carried out by using air flow grinding natural graphite under conditions of .

[0077] The natural graphite raw material may be flake natural graphite.

[0078] The pulverization and size reduction may be performed so that the particle diameter of the primary particles 3 is about 4 μm to about 8 μm (eg, about 4 μm to about 7 μm or about 4 μm to about 6 μm or about 5 μm to about 7 μm).

[0079] The primary particles 3 are subjected to spheroidization and agglomeration using a spheroidizing device to prepare secondary particles 5. Spheroidization and agglomeration may be performed so that the particle size of the secondary particles 5 is about 5 μm to about 10 μm (e.g., about 6 μm to about 10 μm, about 6 μm to about 8 μm, or about 7 μm to about 8 μm (e.g., about 6 μm to about 7 μm)).

[0080] The secondary particles 5 are mixed with the first amorphous carbon precursor to prepare a mixed product. Through this process, the inside of the secondary particles 5 can be dense.

[0081] The second amorphous carbon precursor is added to the resulting mixed product to agglomerate the tertiary particles 7. The agglomeration can be performed by using a general agglomeration device.

[0082] The first amorphous carbon precursor and the second amorphous carbon precursor may be one selected from phenolic resin, furan resin, epoxy resin, polyacrylonitrile, polyamide resin, polyimide resin, polyamideimide resin, synthetic asphalt, petroleum asphalt, coal asphalt, tar and combinations thereof.

[0083] The first amorphous carbon precursor and the second amorphous carbon precursor can be converted into crystalline carbon (e.g., artificial graphite 9) during subsequent heat treatment, and therefore, the mixing ratio of the secondary particles 5 to the first amorphous carbon precursor and the second amorphous carbon precursor can be adjusted so as to have approximately 9 wt% to approximately 16.5 wt% of artificial graphite 9 in the final product based on the total 100 wt% of the first active substance.

[0084] The process may include inserting the first amorphous carbon precursor and the second amorphous carbon precursor into the interior of the secondary particle 5 , resulting in the amorphous carbon precursor being positioned on the surface of the primary particle 3 and also on the surface of the secondary particle 5 .

[0085] The obtained tertiary particles 7 are subjected to a heat treatment. A heat treatment may be performed at a suitable high temperature (e.g., about 2,800°C to about 3,000°C) to graphitize the first amorphous carbon precursor and the second amorphous carbon precursor. The heat treatment may be performed for about 1 hour to about 5 hours (e.g., about 1 hour to about 4 hours or about 1 hour to about 3 hours). According to this process, the first amorphous carbon precursor and the second amorphous carbon precursor may be converted into artificial graphite 9. The first amorphous carbon precursor and the second amorphous carbon precursor positioned on the surface of the primary particle 3 and the surface of the secondary particle 5 are converted into artificial graphite 9. Therefore, the artificial graphite 9 may be positioned on these surfaces.

[0086] The first heat-treated product is coated with a third amorphous carbon precursor. The third amorphous carbon precursor may be one selected from phenolic resin, furan resin, epoxy resin, polyacrylonitrile, polyamide resin, polyimide resin, polyamideimide resin, synthetic asphalt, petroleum asphalt, coal asphalt, tar, and combinations thereof. The third amorphous carbon precursor may be the same as or different from the first amorphous carbon precursor and / or the second amorphous carbon precursor.

[0087] During coating, the amount of the third amorphous carbon precursor may be appropriately adjusted so that the thickness of the amorphous carbon coating layer 11 is about 5 nm to about 50 nm in the final product (first active material 1 ).

[0088] The coated product is subjected to a secondary heat treatment. The secondary heat treatment may be performed at about 800°C to about 2,000°C (e.g., about 800°C to about 1,800°C, about 800°C to about 1,600°C, about 800°C to about 1,400°C, or about 1,200°C to about 1,300°C). The secondary heat treatment may be performed for about 1 hour to about 5 hours, about 1 hour to about 4 hours, or about 1 hour to about 3 hours.

[0089] Some embodiments provide a negative electrode 20, a positive electrode 10, and a non-aqueous electrolyte.

[0090] The negative electrode 20 includes a negative active material layer and a current collector supporting the negative active material layer, the negative active material layer including a negative active material according to one embodiment, a binder, and optionally a conductive material.

[0091] In the negative active material layer, an amount of the negative active material may be about 95 wt % to about 99 wt % based on the total 100 wt % of the negative active material layer.

[0092] The binder may be included in an amount of about 1 wt % to about 5 wt % based on the total 100 wt % of the negative active material layer.

[0093] If a conductive material is also included, the amount of the negative active material may be about 90 wt % to about 98 wt % based on the total 100 wt % of the negative active material layer, and the amount of the binder and the conductive material may be about 1 wt % to about 5 wt % respectively based on the total 100 wt % of the negative active material layer.

[0094] The binder improves the binding properties between the negative electrode active material particles and between the negative electrode active material particles and the current collector. The binder may be a non-aqueous binder, an aqueous binder, or a combination thereof.

[0095] The non-aqueous binder may be ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0096] The aqueous binder can be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polymers containing ethylene oxide, polyvinyl pyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol or a combination thereof.

[0097] The binder may also include a cellulose compound. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose and their alkali metal salts. The alkali metal may be Na, K or Li. The cellulose compound may be used as a thickener, which may provide viscosity and may also be used as a binder. Based on 100 parts by weight of the negative electrode active material, the amount of the cellulose compound may be, for example, about 0.1 parts by weight to about 3 parts by weight.

[0098] A conductive material is included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes a chemical change. Examples of the conductive material may be: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials of metal powder or metal fiber including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0099] The current collector may include one selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0100] The positive electrode may include a current collector and a positive active material layer formed on the current collector.

[0101] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions. In some embodiments, one or more composite oxides of a metal selected from cobalt, manganese, nickel, and combinations thereof and lithium may be used. For example, a compound represented by one of the following chemical formulas may be used. Li a A 1-b X b D 1 2(0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 2-b X b O 4-c1 D 1 c1(0.90≤a≤1.8,0≤b≤0.5,0≤c1≤0.05);Li a Ni 1-b-c Co b X c D 1 α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c D 1 α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni b HAVE BEEN c G d O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Ni b Co c L 1 d G e O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0≤e≤0.1);Li a NiG bO2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2);Li a FePO4(0.90≤a≤1.8).

[0102] In the above chemical formula, A is selected from Ni, Co, Mn or a combination thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or a combination thereof; D 1 is selected from O, F, S, P or a combination thereof; E is selected from Co, Mn or a combination thereof; T is selected from F, S, P or a combination thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is selected from Ti, Mo, Mn or a combination thereof; Z is selected from Cr, V, Fe, Sc, Y or a combination thereof; J is selected from V, Cr, Mn, Co, Ni, Cu or a combination thereof; and L 1 Selected from Mn, Al or a combination thereof.

[0103] The compound may have a coating layer on the surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from the group consisting of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound for the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating layer may be applied by using these elements in the compound in a method that has no adverse effect on the properties of the positive active material, for example, the method may include any coating method (such as spraying, dipping, etc.), but since it is well known in the relevant art, it is not shown in more detail.

[0104] In the positive electrode, the amount of the positive active material may be about 90 wt % to about 98 wt % based on the total weight of the positive active material layer.

[0105] In some embodiments, the positive electrode active material layer may further include a binder and a conductive material, and may include the binder and the conductive material in an amount of about 1 wt % to about 5 wt % based on the total amount of the positive electrode active material layer.

[0106] The binder improves the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of the binder may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.

[0107] A conductive material is included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes a chemical change. Examples of the conductive material may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials of metal powder or metal fiber, including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.

[0108] The current collector may include Al.

[0109] The electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0110] The nonaqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.

[0111] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent, or an aprotic solvent.

[0112] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, mevalonolactone, caprolactone, etc. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. Examples of aprotic solvents include: nitriles, such as R-CN (wherein R is a C2 to C20 linear, branched or cyclic hydrocarbon, and may include a double bond, an aromatic ring or an ether bond); amides, such as dimethylformamide; dioxolanes, such as 1,3-dioxolane; cyclopentane sulfone, etc.

[0113] The organic solvent may be used alone or in a mixture. If the organic solvent is used in a mixture, the mixing ratio may be controlled according to the desired battery performance, and this may be well known to those skilled in the relevant art.

[0114] The carbonate-based solvent may include a mixture having a cyclic carbonate and a chain carbonate. The cyclic carbonate and the chain carbonate are mixed together in a volume ratio of about 1:1 to about 1:9, and if the mixture is used as an electrolyte, it may have enhanced performance.

[0115] The organic solvent may further include an aromatic hydrocarbon solvent and a carbonate solvent. The carbonate solvent and the aromatic hydrocarbon solvent may be mixed together in a volume ratio of about 1:1 to about 30:1.

[0116] The aromatic hydrocarbon organic solvent may be an aromatic hydrocarbon compound represented by Chemical Formula 1.

[0117] [Chemical formula 1]

[0118]

[0119] In Chemical Formula 1, R1 to R6 are the same or different and are selected from hydrogen, halogen, C1 to C10 alkyl, halogenated alkyl, and combinations thereof.

[0120] Examples of aromatic hydrocarbon organic solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, , 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene or a combination thereof.

[0121] The electrolyte may further include ethyl vinyl carbonate, vinylene carbonate, or an ethylene carbonate-based compound represented by Chemical Formula 2 as an additive for improving cycle life.

[0122] [Chemical formula 2]

[0123]

[0124] In Chemical Formula 2, R7 and R8 are the same or different and may be independently hydrogen, halogen, cyano (CN), nitro (NO2) or fluorinated C1 to C5 alkyl, provided that at least one of R7 and R8 is halogen, cyano (CN), nitro (NO2) or fluorinated C1 to C5 alkyl, and R7 and R8 are not hydrogen at the same time.

[0125] Examples of ethylene carbonate compounds may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, etc. The amount of the additive for improving cycle life characteristics may be used within an appropriate range.

[0126] The lithium salt dissolved in the organic solvent supplies lithium ions to the battery, enables the basic operation of the rechargeable lithium battery 100, and improves the transfer of lithium ions between the positive electrode 10 and the negative electrode 20. Examples of the lithium salt include at least one supporting salt selected from the following: LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+ 1SO2)(C y F 2y+1 SO2) (wherein, x and y are natural numbers, for example, integers from about 1 to about 20), lithium difluoro(bis(oxalato)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB), and lithium difluoro(oxalato)borate (LiDFOB). The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. If the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.

[0127] According to the type of the rechargeable lithium battery 100, the separator 30 may be located between the positive electrode 10 and the negative electrode 20. The separator 30 may use polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer thereof having two or more layers, and may be a mixed multilayer (such as a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, a polypropylene / polyethylene / polypropylene three-layer separator, etc.).

[0128] Figure 3 1 is an exploded perspective view of a rechargeable lithium battery 100 according to some embodiments. The rechargeable lithium battery 100 according to some embodiments is shown as a prismatic battery, but may include batteries of various shapes such as a cylindrical battery, a pouch battery, and the like.

[0129] Reference Figure 3 , the rechargeable lithium battery 100 according to the embodiment may include an electrode assembly 40 manufactured by winding a separator 30 between a positive electrode 10 and a negative electrode 20, and a case 50 accommodating the electrode assembly 40. An electrolyte (not shown) may be impregnated in the positive electrode 10, the negative electrode 20, and the separator 30.

[0130] The following examples and comparative examples are provided to highlight the features of one or more embodiments, but it will be understood that the examples and comparative examples will not be interpreted as limiting the scope of the embodiments, and the comparative examples will not be interpreted as being outside the scope of the embodiments. In addition, it will be understood that the embodiments are not limited to the specific details described in the examples and comparative examples.

[0131] (Example 1)

[0132] A flake natural graphite raw material having a particle size of 80 μm to 120 μm is air-milled to prepare small-sized primary particles having an average particle size (D50) of 4.9 μm. The small-sized primary particles are spheroidized and agglomerated by using a spheroidizing device to prepare secondary particles having an average particle size (D50) of 6.1 μm. The secondary particles are mixed with a first petroleum-based asphalt to prepare a mixed product.

[0133] Thereafter, a second petroleum-based asphalt was added to the mixed product and agglomerated to prepare tertiary particles having an average particle diameter (D50) of 10.4 μm.

[0134] The prepared tertiary particles were once heat-treated for 2 hours at 2,800° C. During the heat treatment, the first pitch carbon and the second pitch carbon were graphitized and existed as artificial graphite on the surfaces of the primary particles and the secondary particles.

[0135] The heat-treated product was coated with a third pitch and subjected to a secondary heat treatment at 1,200° C. for 2 hours to prepare a first active material having an average particle size (D50) of 10.5 μm and a tap density of 1.04 g / cc. The prepared first active material includes secondary particles and tertiary particles of natural graphite, artificial graphite positioned on the surfaces of the primary particles and the surfaces of the secondary particles, and a soft carbon coating layer surrounding the surfaces of the tertiary particles, the primary particles agglomerated and spheroidized in the secondary particles, and the secondary particles agglomerated in the tertiary particles of natural graphite.

[0136] During the preparation, the usage amounts of tertiary particles, first asphalt carbon, second asphalt carbon and third asphalt carbon are adjusted so that based on the total 100wt% of the first active material, the amount of natural graphite in the prepared first active material is 87wt%, the amount of artificial graphite is 10wt%, and the amount of the soft carbon coating layer is 3wt%.

[0137] As the second active material, rod-shaped artificial graphite having a major diameter (length of the major axis) of 60 μm and a maximum aspect ratio of 10 was used.

[0138] The first active material and the second active material were mixed at a weight ratio of 90:10 to prepare a negative electrode active material.

[0139] 97.5 wt % of a negative active material (a mixing ratio of the first active material: the second active material is 90:10 by weight), 1.5 wt % of a styrene-butadiene rubber binder, and 1.0 wt % of a carboxymethyl cellulose thickener were mixed in a water solvent to prepare a negative active material slurry.

[0140] The negative active material slurry was coated on a Cu foil current collector, dried and pressed under general procedures to prepare a negative electrode including the current collector and a negative active material layer formed on the current collector.

[0141] A coin-type half-cell was fabricated using a negative electrode, a lithium metal counter electrode, and an electrolyte, which was 1.5 M LiPF6 dissolved in a mixed solvent of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate (volume ratio 20:10:70).

[0142] (Example 2)

[0143] A negative electrode and a half-cell were manufactured through the same steps as those in Example 1, except that the mixing ratio of the first active material and the second active material was changed to a weight ratio of 80:20 to prepare a negative active material.

[0144] (Example 3)

[0145] A negative electrode and a half-cell were manufactured through the same steps as those in Example 1, except that the mixing ratio of the first active material and the second active material was changed to a weight ratio of 85:15 to prepare a negative active material.

[0146] (Comparative Example 1)

[0147] As the negative electrode active material, spherical natural graphite having a particle size of 10 μm to 15 μm was used.

[0148] A negative electrode and a half-cell were manufactured by the same steps as those in Example 1 using the negative electrode active material.

[0149] (Comparative Example 2)

[0150] The negative electrode active material of Comparative Example 1 was used as the first active material, and rod-type artificial graphite having a long diameter (length of the long axis) of 60 μm and a maximum aspect ratio of 10 was used as the second active material, and then the first active material and the second active material were mixed at a weight ratio of 90:10 to prepare a negative electrode active material.

[0151] A negative electrode and a half-cell were manufactured by the same steps as those in Example 1 using the negative electrode active material.

[0152] Experimental Example 1) SEM measurement

[0153] The SEM images of the negative electrode active materials of Example 1 and Comparative Example 1 are respectively Figure 4 and Figure 5 As shown in Figure 4 As shown in , the rod-shaped second active material and the agglomerated spherical first active material are distributed in the negative electrode active material of Example 1. In contrast, Figure 5 As shown in , the negative electrode active material of Comparative Example 1, which is natural graphite, has a spherical shape.

[0154] Experimental Example 2) Evaluation of Area Ratio

[0155] The area ratios occupied by the second active material in the negative active materials according to Examples 1 to 3 and Comparative Example 2 were measured by a particle size analyzer.

[0156] Experimental Example 3) Evaluation of Orientation Index

[0157] The peak intensity at the (002) plane relative to the peak intensity at the (110) plane was measured by X-ray diffraction analysis using CuKα rays. 002 / I 110 ) of the negative active materials according to Examples 1 to 3 and Comparative Examples 1 and 2. The results are shown in Table 1 as OI.

[0158] Experimental Example 4) Evaluation of Mercury Cumulative Pore Volume

[0159] The mercury cumulative pore volume of the negative electrodes according to Examples 1 to 3 and Comparative Examples 1 and 2 was measured by adding mercury to the negative active material, applying a pressure of 0.1 psi to inject mercury into the negative active material, and then increasing the pressure to 60,000 psi to measure the volume change of mercury. The results are shown in Table 1. The measured pores had a pore diameter of 0.01 μm to 1 μm.

[0160] Experimental Example 5) Evaluation of Charging Capacity

[0161] The half-cells according to Examples 1 to 3 and Comparative Examples 1 and 2 were charged and discharged once at 0.2C, and charged and discharged once at 2C.

[0162] The ratio of the charge capacity at 2 C to the charge capacity at 0.2 C was calculated. The results are shown in Table 1 as charge capacity.

[0163] Experimental Example 6) Evaluation of DC Internal Resistance (DC-IR)

[0164] The half-battery cells according to Examples 1 to 3 and Comparative Examples 1 and 2 were charged and discharged once under the following conditions: constant current / constant voltage charging at 0.2C, 4.25V, 0.05C cutoff at 25°C, paused for 10 minutes, constant current discharge at 0.33C, 2.80V cutoff, paused for 10 minutes. The DC internal resistance (DC-IR) was evaluated by measuring the voltage drop (V) when the current flows at 1C for 1 second at SOC50 (50% charging capacity based on 100% of the entire battery charging capacity, which is discharged 50% in the discharge state). The resistance value is obtained by the measured voltage and the applied current (1C). The results are shown as the DC internal resistance (DC-IR). The results are shown in Table 1. Figure 6 is a graph showing resistances of different densities of negative active materials according to Example 1 and Comparative Example 1.

[0165] Experimental Example 7) Evaluation of expansion characteristics

[0166] The half-cells according to Examples 1 to 3 and Comparative Examples 1 and 2 were charged and discharged at 3C for 19 cycles for 6000 minutes. The thickness before and after charging and discharging was measured, respectively. The thickness increase ratio was calculated by the following equation 1. The results are shown in Table 1 as expansion ratios.

[0167] [Equation 1]

[0168] Thickness increase ratio (%) = [(battery cell thickness after charging and discharging - battery cell thickness before charging and discharging) / (battery cell thickness before charging and discharging)] * 100

[0169] Table 1

[0170]

[0171] As shown in Table 1, Examples 1 to 3 using the agglomerated first active material and the second active material having a maximum aspect ratio of 10 to 100 exhibited excellent chargeability, low DC-IR of 6.0Ω to 6.3Ω, and low expansion ratio. Examples 1 to 3 had a mercury cumulative pore volume of the total negative electrode active material having the first active material and the second active material within 2.01 mL / g to 2.71 mL / g, so that easy impregnation of the electrolyte can be expected.

[0172] On the other hand, Comparative Example 2 using a mixture of spherical natural graphite and a second active material having a maximum aspect ratio of 10 exhibited similar charging capability, DC-IR, and expansion ratio to Comparative Example 1 using only spherical natural graphite, and therefore, it can be seen that the improvement effect is not significant.

[0173] According to these results, if the agglomerated first active material is used together with the second active material having an aspect ratio of 2 to 100, the effect by using the second active material having an aspect ratio of 2 to 100 can be maximized.

[0174] Example embodiments have been disclosed herein, and although specific terms are employed, they are used and interpreted in a general and descriptive sense only, and not for purposes of limitation. In some cases, as will be apparent to one of ordinary skill in the art upon filing this application, unless otherwise expressly noted, features, characteristics, and / or elements described in conjunction with a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described in conjunction with other embodiments. Therefore, it will be understood by those skilled in the art that various changes in form and detail may be made without departing from the spirit and scope of the invention as set forth in the appended claims.

Claims

1. A negative electrode active material, comprising: A first active material, comprising: tertiary particles of natural graphite, in which secondary particles are agglomerated, and in which primary particles are agglomerated and spheroidized; artificial graphite positioned on the surfaces of the primary particles and the secondary particles; and an amorphous carbon coating layer surrounding the tertiary particles of natural graphite; and The second active material includes a carbon-based material having an aspect ratio of 2 to 100.

2. The negative electrode active material according to claim 1, wherein The aspect ratio of the second active material is 2 to 50.

3. The negative electrode active material according to claim 1, wherein The amount of the second active material is 10 wt % to 30 wt % based on 100 wt % of the total negative active material.

4. The negative electrode active material according to claim 1, wherein The second active material includes artificial graphite.

5. The negative electrode active material according to claim 1, wherein The second active material has an average length of a major axis of 40 μm to 120 μm.

6. The negative electrode active material according to claim 1, wherein In the negative electrode active material, based on 100% of the total area of ​​the negative electrode active material, the area ratio of the second active material is 10% to 40%.

7. The negative electrode active material according to claim 1, wherein The natural graphite is flake natural graphite.

8. The negative electrode active material according to claim 1, wherein The negative electrode active material has an orientation index of 40 to 90.

9. The negative electrode active material according to claim 1, wherein The negative active material has a mercury cumulative pore volume of 1.5 mL / g to 3 mL / g.

10. The negative electrode active material according to claim 1, wherein The second active material has a rod shape.

11. The negative electrode active material according to claim 1, wherein In the first active material, an amount of the amorphous carbon coating layer is 0.01 wt % to 5 wt % based on 100 wt % of the total amount of the first active material.

12. The negative electrode active material according to claim 1, wherein In the first active material, an amount of the artificial graphite is 9 wt % to 16.5 wt % based on 100 wt % of the total of the first active material.

13. The negative electrode active material according to claim 1, wherein In the first active material, an amount of the natural graphite is 78.5 wt % to 89 wt % based on 100 wt % of the total of the first active material.

14. The negative electrode active material according to claim 1, wherein The first active material has a tap density of 0.8 g / cc to 1.1 g / cc.

15. The negative electrode active material according to claim 1, wherein The amorphous carbon coating layer includes at least one of soft carbon, hard carbon, mesophase pitch carbide, burned coke, and a mixture thereof.

16. A rechargeable lithium battery, comprising: A negative electrode, comprising a negative electrode active material according to any one of claims 1 to 15; Positive electrode; as well as Electrolytes.