Ultrahigh-nickel polycrystalline ternary positive electrode material and preparation method thereof

By doping Ca and Mg elements into ultra-high nickel polycrystalline ternary positive electrode material and forming a porous structure, the volume expansion problem of the material during high current charging and discharging is solved, the structural stability and lithium ion transmission efficiency are improved, and the material is extended life.

CN118943318APending Publication Date: 2024-11-12NANTONG JINTONG ENERGY STORAGE POWER NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410918870.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Ultra-high nickel polycrystalline ternary cathode material will expand volumetrically during charging and discharging of high current, resulting in increased internal stress, structural collapse and rapid capacity attenuation.

Method used

Ultra-high nickel polycrystalline ternary cathode material doped with Ca and Mg elements is used to form a porous structure of the cathode material through co-precipitation reaction and the formation of nickel-cobalt-manganese precursor, and precise control of the core and shell, combined with lithium salt The molten state enters the porous structure, forming a stable structure to alleviate volume expansion.

Benefits of technology

It improves the structural stability of the material, adapts to high current charging and discharging, prevents structure collapse, enhances the transmission efficiency of lithium ions, and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943318A_ABST
    Figure CN118943318A_ABST
Patent Text Reader

Abstract

A preparation method of the ultrahigh-nickel polycrystalline ternary positive electrode material comprises the following steps: preparing a first mixed solution, a second mixed solution and a precipitator; keeping stirring, introducing nitrogen, and respectively adding the first mixed solution and a precipitator into the kettle for reaction; when the particle size of the material grows to 12.5-15.3 [mu] m, stopping feeding the first mixed solution, improving the second mixed solution, continuously growing the particle size of the material to 16-18 [mu] m, and stopping the reaction when the particle size pitch reaches 0.75 < (D90-D10) / D50 < 0.95; and centrifuging, washing and drying to obtain the ultrahigh-nickel polycrystalline ternary precursor, wherein the chemical formula of the ultrahigh-nickel polycrystalline ternary precursor is aNi < x > Co < y > Mn < z > M < 1-x-y-z > C < 2 > O < 2 >. BNi < x > Co < y > Mn < z > M < k > Sr < 1-x-y-z-k > C < 2 > O < 2 >, and mixing with a lithium salt, heating, and treating to obtain the ultrahigh-nickel polycrystalline ternary positive electrode material. The material is stable in structure and can adapt to large-current charging and discharging, and the preparation method is simple, easy to operate and convenient to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to an ultra-high nickel polycrystalline ternary positive electrode material and a preparation method thereof. Background Art

[0002] Ultra-high nickel polycrystalline ternary positive electrode materials are highly sought after for their high energy density and good cycle performance. However, when charged and discharged at high currents, their volume expands, causing internal stress to increase, leading to secondary ball rupture, structural collapse and rapid capacity decay.

[0003] Therefore, in order to alleviate the volume expansion of the ultra-high nickel polycrystalline ternary positive electrode material during high current charging and discharging, the ultra-high nickel polycrystalline ternary positive electrode material needs to be modified. Summary of the invention

[0004] The purpose of the present invention is to provide an ultra-high nickel polycrystalline ternary positive electrode material and a preparation method thereof.

[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention at the material level is:

[0006] An ultra-high nickel polycrystalline ternary positive electrode material with the chemical formula of aLiNi x Co y Mn z M 1-x-y-z O 2 ·bLiNi x Co y Mn z M k Sr 1-x-y-z-k O 2 , M element is one or more of Ca and Mg; wherein, 0.9<x<1.0, 0<y<0.05, 0<z<0.05, 0.002<1-xyz<0.004, 0.001<k<0.003, 0<1-xyzk<0.002, 4≤b / a≤6.

[0007] A further technical solution is that the particles of the material are spherical and have a porous structure in cross section, and the porous structure is divided into a core and a shell according to the pore size; wherein the pore size of the core is 200-500nm, the porosity is 18-22%, and the diameter accounts for 78-85% of the entire sphere; the pore size of the shell is 20-40nm, the porosity is 8-12%, and the thickness of the shell accounts for 15-22% of the entire sphere;

[0008] The core is composed of LiNi x Co y Mn z M k Sr 1-x-y-z-kO 2 The shell is composed of LiNi x Co y Mn z M 1-x-y-z O 2 ;

[0009] The material’s D50 is 16-18um, the particle size distance is 0.75<(D90-D10) / D50<0.95, and the tap density is 2.2-2.6g / cm 3 , the specific surface area is 0.50~0.70m 2 / g.

[0010] In order to achieve the above object, the technical solution adopted by the present invention at the method level is:

[0011] A method for preparing an ultra-high nickel polycrystalline ternary positive electrode material, comprising:

[0012] Step 1, preparing a first mixed solution of Ni, Co, Mn, a strontium salt and a salt containing an M element, wherein the strontium salt is one or more of strontium acetate, strontium nitrate and strontium chloride;

[0013] Preparing a second mixed solution of Ni, Co, Mn and a salt containing the M element;

[0014] An oxalic acid solution with a molar concentration of 1 to 5 mol / L is prepared as a precipitant, and the temperature of the precipitant solution is 50° C.;

[0015] Step 2: Keep stirring the reactor on, introduce nitrogen, and add the first mixed solution and the precipitant in step 1 into the reactor for coprecipitation reaction; nitrogen is continuously introduced during the reaction, the reaction temperature is maintained at 50-70° C., and the speed of the reactor is 400-600 r / min;

[0016] When the particle size D50 of the material in the reactor 1 When the particle size grows to 12.5-15.3um, the first mixed solution is stopped, the second mixed solution is improved, and the particle size of the material continues to grow to 16-18um. When the particle size distance reaches 0.75<(D90-D10) / D50<0.95, the reaction is stopped;

[0017] After centrifugation, washing and drying, the ultra-high nickel polycrystalline ternary precursor is obtained, and its chemical formula is aNi x Co y Mn z M 1-x-y- z C 2 O 2 ·bNi x Co y Mn zM k Sr 1-x-y-z-k C 2 O 2 ;

[0018] Step three: mix the ultra-high nickel polycrystalline ternary precursor prepared in step two with lithium salt, heat and react in a muffle furnace with oxygen, cool to room temperature after the reaction, and obtain the ultra-high nickel polycrystalline ternary positive electrode material through crushing and screening.

[0019] According to a further technical solution, in step 1, the total molar concentration of Ni, Co and Mn in the first mixed solution and the second mixed solution is 1.8 to 2.4 mol / L.

[0020] According to a further technical solution, in step three, the purity of the oxygen is greater than 99.99%.

[0021] According to a further technical solution, in step three, the molar ratio of the lithium salt to the ultra-high nickel polycrystalline ternary precursor is 1.02 to 1.04.

[0022] A further technical solution is that in step three, the mixture of the ultra-high nickel polycrystalline ternary precursor and the lithium salt is placed in a muffle furnace, heated to 390-430°C at a heating rate of 10°C / min, reacted for 5 hours, then heated to 780-840°C at a heating rate of 3°C / min, reacted for 18-22 hours, and then cooled to room temperature at a cooling rate of 1.5°C / min.

[0023] In a further technical solution, the M element is one or more of Ca and Mg, and the M element-containing salt is one or a combination of calcium chloride and magnesium chloride.

[0024] According to a further technical solution, in step three, the lithium salt is lithium hydroxide.

[0025] In a further technical solution, in step 1, the Ni salt is nickel sulfate, the Co salt is cobalt sulfate, and the Mn salt is manganese sulfate.

[0026] The terms “include,” “including,” “have,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0027] The terms used herein generally have the ordinary meanings of each term used in the art, in the context of the present invention, and in the specific context, unless otherwise noted. Certain terms used to describe the present invention will be discussed below or elsewhere in this specification to provide additional guidance to those skilled in the art regarding the description of the present invention.

[0028] The working principle and advantages of the present invention are as follows:

[0029] 1. The present invention achieves uniform distribution of the doped elements at the atomic level by doping one or more of the Ca and Mg elements in the process of preparing the ultra-high nickel polycrystalline ternary precursor, increases the holes in the ternary positive electrode material, improves the conductivity, and is conducive to the rapid transmission of lithium ions during high current charging and discharging. In addition, the incorporation of the Ca and Mg elements plays a certain role in fluxing, which is conducive to accelerating the fusion of the lithium source and the precursor, and the structure of the formed positive electrode material is more stable.

[0030] 2. When preparing the ultra-high nickel polycrystalline ternary precursor, the present invention achieves the goal of controlling the core (bNi x Co y Mn z M k Sr 1-x-y-z-k C 2 O 2 ) and shell (aNi x Co y Mn z M 1-x-y-z C 2 O 2 ) and the diameter of the core shell. In addition, the present invention can use oxalic acid as a precipitant to generate a ternary precursor of nickel-cobalt-manganese oxalate. During the sintering process of the positive electrode material, oxalate decomposes to produce a large amount of CO 2 Gas, forming a porous structure. The core (bNi x Co y Mn z M k Sr 1-x-y-z-k C 2 O 2 ) is grown from the first metal liquid, and is uniformly distributed with Sr elements. The Sr element acts as a flux, which can reduce the melting point of the positive electrode material during sintering, and is conducive to further cross-linking and melting of the porous structure to form larger pores, which can alleviate the volume expansion during high current charging and discharging and prevent structural collapse; the outer shell (aNi x Co y Mn z M 1-x-y-z C 2 O 2 ) does not contain Sr element, and its pores are smaller than the core, which helps to provide a relatively stable structure. At the same time, the right amount of pores helps to increase the contact area with the electrolyte, improve the transmission efficiency of lithium ions, and facilitate large current charging and discharging.

[0031] 3. When preparing the ternary positive electrode material, the ultra-high nickel polycrystalline ternary precursor and the lithium salt mixture are placed in a muffle furnace, heated to 390-430°C at a heating rate of 10°C / min, and then reacted for 5 hours. In this process, the ultra-high nickel polycrystalline ternary precursor is rapidly decomposed to form oxides. The CO generated in the process 2 The gas is quickly released from the inside of the precursor, forming a porous structure in the cross-section of the precursor, while the lithium salt changes from a solid state to a molten state, slowly entering into the porous structure inside the ultra-high nickel polycrystalline ternary precursor; it is then heated to 780-840°C at a heating rate of 3°C / min and reacted for 18-22 hours. The lithium that has entered into the porous structure inside the ultra-high nickel polycrystalline ternary precursor fuses with the precursor during the slow heating process, and then reacts to obtain a ternary positive electrode material. Since the flux Sr element is evenly distributed in the core of the precursor, it quickly cross-links and melts at 780-840°C, forming a porous structure with a larger pore size in the core; then it is cooled to room temperature at a cooling rate of 1.5°C / min. Slow cooling can ensure further stabilization of the porous structure of the core, and prevent rapid shrinkage of the core pores due to excessively rapid cooling, which in turn causes primary particle breakage.

[0032] 4. The cross-section of the ternary cathode material prepared by the present invention is a porous structure, which is divided into a core (component is LiNi x Co y Mn z M k Sr 1-x-y-z-k O 2 ) and shell (component is LiNi x Co y Mn z M 1-x-y-z O 2 ), the core pore size is 200-500nm, the porosity is 18%-22%, the core diameter accounts for 78%-85% of the entire sphere, the shell pore size is 20-40nm, the porosity is 8%-12%, the shell thickness accounts for 15%-22% of the entire sphere, D50 is 16-18um, and the particle size distance is 0.75<

[0033] (D90-D10) / D50<0.95, tap density is 2.2~2.6g / cm 3 , the specific surface area is 0.50~0.70m 2 / g. The large pore size structure of the core helps to alleviate the volume expansion during high current charging and discharging and prevent the collapse of the structure. The small pore size of the shell helps to stabilize the structure and increase the contact area with the electrolyte, providing more lithium ion transmission channels and improving the transmission efficiency of lithium ions.

[0034] In summary, the present invention provides an ultra-high nickel polycrystalline ternary positive electrode material and a preparation method. Compared with the prior art, the ultra-high nickel polycrystalline ternary positive electrode material of the present invention has a stable structure, can adapt to large current charging and discharging, and the corresponding preparation method is simple and easy to operate, which is convenient for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Attached Figure 1 This is a cross-sectional electron microscope image of the ultra-high nickel polycrystalline ternary positive electrode material prepared in Example 1 of the present invention;

[0036] Attached Figure 2 This is a cross-sectional electron microscope image of the ultra-high nickel polycrystalline ternary positive electrode material prepared in Comparative Example 1 of the present invention;

[0037] Attached Figure 3 This is a rate performance diagram of the battery prepared in Example 1 of the present invention and Comparative Example 1 at 25° C. and a voltage window of 3.0 to 4.3 V under the conditions of discharge current densities of 0.1, 0.2, 0.5, 1, 2 and 5 C, respectively. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0039] The present invention will be clearly described below with drawings and detailed descriptions. After understanding the embodiments of the present invention, any person skilled in the art can make changes and modifications based on the techniques taught by the present invention without departing from the spirit and scope of the present invention.

[0040] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the present disclosure.

[0041] Embodiment 1: A method for preparing an ultra-high nickel polycrystalline ternary positive electrode material, comprising the following steps in sequence:

[0042] Step 1, preparing a first mixed solution of Ni, Co, Mn, strontium acetate and calcium sulfate, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn, Sr and Ca elements is 92:4:3.6:0.1:0.3;

[0043] A second mixed solution of Ni, Co, Mn and calcium sulfate is prepared, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn and Ca elements is 92:4:3.6:0.4;

[0044] Prepare oxalic acid solution with a molar concentration of 4 mol / L as a precipitant, and the precipitant temperature is 50°C;

[0045] Step 2: Keep stirring the reactor on, introduce nitrogen, and add the first mixed solution and the precipitant into the reactor for co-precipitation reaction; nitrogen is continuously introduced during the reaction, the reaction temperature is maintained at 65° C., and the speed of the reactor is 500 r / min;

[0046] When the particle size D50 of the material in the reactor 1 When the particle size grows to 14 μm, the first mixed solution is stopped, and the second mixed solution is improved to continue growing to 17 μm, with a particle size spacing of 0.81, and the reaction is stopped; centrifugation, washing, and drying are performed to obtain an ultra-high nickel polycrystalline ternary precursor, whose chemical formula is Ni 0.92 Co 0.04 Mn 0.036 Ca 0.004 C 2 O 2 ·6Ni 0.92 Co 0.04 Mn 0.036 Ca 0.003 Sr 0.001 C 2 O 2 ;

[0047] Step 3: Mix the ultra-high nickel polycrystalline ternary precursor prepared in step 2 with lithium hydroxide, wherein the molar ratio of lithium salt to ultra-high nickel polycrystalline ternary precursor is 1.03, and introduce 99.99% oxygen into a muffle furnace for heating reaction, and heat to 420°C at a heating rate of 10°C / min and react for 5 hours, and then heat to 820°C at a heating rate of 3°C / min and react for 20 hours, and then cool to room temperature at a cooling rate of 1.5°C / min, and after crushing and screening, obtain an ultra-high nickel polycrystalline ternary positive electrode material, the chemical formula of the product is LiNi 0.92 Co 0.04 Mn 0.036 Ca 0.004 O 2 6LiNi 0.92 Co 0.04 Mn 0.036 Ca 0.003 Sr 0.00 1 O 2 The cross section of the ultra-high nickel polycrystalline ternary cathode material is a porous structure, which is divided into a core (component is LiNi 0.92 Co 0.04 Mn 0.036 Ca 0.003 Sr 0.001 O 2 ) and shell (component is LiNi 0.92 Co 0.04 Mn 0.036 Ca0.004 O 2 ), the core pore size is 200-500nm, the porosity is 20%, the core diameter accounts for 82% of the entire sphere, the shell pore size is 20-40nm, the porosity is 10%, the shell thickness accounts for 18% of the entire sphere, D50 is 17.2um, the particle size spacing is 0.82, and the tap density is 2.4g / cm 3 , with a specific surface area of ​​0.58m 2 / g, relevant data can be seen in Table 1.

[0048] Embodiment 2: A method for preparing an ultra-high nickel polycrystalline ternary positive electrode material, comprising the following steps in sequence:

[0049] Step 1, preparing a first mixed solution of Ni, Co, Mn, strontium acetate and calcium sulfate, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn, Sr and Ca elements is 93:2:4.6:0.1:0.3;

[0050] A second mixed solution of Ni, Co, Mn and calcium sulfate is prepared, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn and Ca elements is 93:2:4.6:0.4;

[0051] Prepare oxalic acid solution with a molar concentration of 4 mol / L as a precipitant, and the precipitant temperature is 50°C;

[0052] Step 2: Keep stirring the reactor on, introduce nitrogen, and add the first mixed solution and the precipitant into the reactor for co-precipitation reaction; nitrogen is continuously introduced during the reaction, the reaction temperature is maintained at 65° C., and the speed of the reactor is 500 r / min;

[0053] When the particle size D50 of the material in the reactor 1 When the particle size grows to 14 μm, the first mixed solution is stopped, and the second mixed solution is improved to continue growing to 17 μm, with a particle size spacing of 0.81, and the reaction is stopped; centrifugation, washing, and drying are performed to obtain an ultra-high nickel polycrystalline ternary precursor, whose chemical formula is Ni 0.93 Co 0.02 Mn 0.046 Ca 0.004 C 2 O 2 ·6Ni 0.93 Co 0.02 Mn 0.046 Ca 0.003 Sr 0.001 C 2 O 2 ;

[0054] Step 3: Mix the ultra-high nickel polycrystalline ternary precursor prepared in step 2 with lithium hydroxide, wherein the molar ratio of lithium salt to ultra-high nickel polycrystalline ternary precursor is 1.03, and introduce 99.99% oxygen into a muffle furnace for heating reaction, and heat to 420°C at a heating rate of 10°C / min and react for 5 hours, and then heat to 820°C at a heating rate of 3°C / min and react for 20 hours, and then cool to room temperature at a cooling rate of 1.5°C / min, and after crushing and screening, obtain an ultra-high nickel polycrystalline ternary positive electrode material, the chemical formula of the product is LiNi 0.93 Co 0.02 Mn 0.046 Ca 0.004 O 2 6LiNi 0.93 Co 0.02 Mn 0.046 Ca 0.003 Sr 0.00 1 O 2 The cross section of the ultra-high nickel polycrystalline ternary cathode material is a porous structure, which is divided into a core (component is LiNi 0.93 Co 0.02 Mn 0.046 Ca 0.003 Sr 0.001 O 2 ) and shell (component is LiNi 0.93 Co 0.02 Mn 0.046 Ca 0.004 O 2 ), the core pore size is 200-500nm, the porosity is 21%, the core diameter accounts for 82% of the entire sphere, the shell pore size is 20-40nm, the porosity is 10%, the shell thickness accounts for 18% of the entire sphere, D50 is 17.3um, the particle size spacing is 0.85, and the tap density is 2.3g / cm 3 , with a specific surface area of ​​0.63m 2 / g, relevant data can be seen in Table 1.

[0055] Embodiment 3: A method for preparing an ultra-high nickel polycrystalline ternary positive electrode material, comprising the following steps in sequence:

[0056] Step 1, preparing a first mixed solution of Ni, Co, Mn, strontium acetate and calcium sulfate, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn, Sr and Ca elements is 94:2:3.6:0.1:0.3;

[0057] A second mixed solution of Ni, Co, Mn and calcium sulfate is prepared, wherein the total molar concentration of Ni, Co and Mn in the mixed solution is 2.0 mol / L, and the molar ratio of Ni, Co, Mn and Ca elements is 94:2:3.6:0.4;

[0058] Prepare oxalic acid solution with a molar concentration of 4 mol / L as a precipitant, and the precipitant temperature is 50°C;

[0059] Step 2: Keep stirring the reactor on, introduce nitrogen, and add the first mixed solution and the precipitant into the reactor for co-precipitation reaction; nitrogen is continuously introduced during the reaction, the reaction temperature is maintained at 65° C., and the speed of the reactor is 500 r / min;

[0060] When the particle size D50 of the material in the reactor 1 When the particle size grows to 14 μm, the first mixed solution is stopped, and the second mixed solution is improved to continue growing to 17 μm, with a particle size spacing of 0.81, and the reaction is stopped; centrifugation, washing, and drying are performed to obtain an ultra-high nickel polycrystalline ternary precursor, whose chemical formula is Ni 0.94 Co 0.02 Mn 0.036 Ca 0.004 C 2 O 2 ·6Ni 0.94 Co 0.02 Mn 0.036 Ca 0.003 Sr 0.001 C 2 O 2 ;

[0061] Step 3: Mix the ultra-high nickel polycrystalline ternary precursor prepared in step 2 with lithium hydroxide, wherein the molar ratio of lithium salt to ultra-high nickel polycrystalline ternary precursor is 1.03, and introduce 99.99% oxygen into a muffle furnace for heating reaction, and heat to 420°C at a heating rate of 10°C / min and react for 5 hours, and then heat to 820°C at a heating rate of 3°C / min and react for 20 hours, and then cool to room temperature at a cooling rate of 1.5°C / min, and after crushing and screening, obtain an ultra-high nickel polycrystalline ternary positive electrode material, the chemical formula of the product is LiNi 0.94 Co 0.02 Mn 0.036 Ca 0.004 O 2 6LiNi 0.94 Co 0.02 Mn 0.036 Ca 0.003 Sr 0.00 1 O 2The cross section of the ultra-high nickel polycrystalline ternary cathode material is a porous structure, which is divided into a core (component is LiNi 0.94 Co 0.02 Mn 0.036 Ca 0.003 Sr 0.001 O 2 ) and shell (component is LiNi 0.94 Co 0.02 Mn 0.036 Ca 0.004 O 2 ), the core pore size is 200-500nm, the porosity is 22%, the core diameter accounts for 82% of the entire sphere, the shell pore size is 20-40nm, the porosity is 11%, the shell thickness accounts for 18% of the entire sphere, D50 is 17.2um, the particle size spacing is 0.82, and the tap density is 2.3g / cm 3 , with a specific surface area of ​​0.68m 2 / g, relevant data can be seen in Table 1.

[0062] Comparative Example 1:

[0063] The difference from the embodiments is that the precipitant used in step 1 is different. In this comparative example 1, sodium hydroxide is used as the precipitant and ammonia water is used as the complexing agent. The rest is exactly the same as the embodiments. The relevant data are shown in Table 1.

[0064] Table 1 shows the particle size data of samples in each embodiment and comparative example 1.

[0065]

[0066] By comparing the data of each embodiment in Table 1 above with that of Comparative Example 1, it can be seen that:

[0067] Under the same other conditions, the type of precipitant has no effect on the particle size D50 and particle size distribution of the ultra-high nickel polycrystalline ternary precursor and the positive electrode material. In addition, after the precursor is prepared into the corresponding positive electrode material, its D50 tends to increase, which is mainly related to the increase in the primary particles after the precursor is calcined. In Comparative Example 1, sodium hydroxide is used as the precipitant. Compared with the embodiment, the cross-section of the positive electrode material prepared in Comparative Example 1 ( Figure 2 ) is much lower than that of the embodiments.

[0068] Figure 1 This is a cross-sectional electron microscope image of the ultra-high nickel polycrystalline ternary positive electrode material prepared in Example 1 of the present invention. It can be seen from the figure that the cross-section is divided into two layers, an inner core and an outer shell. The inner core is a porous structure with a pore size larger than that of the outer shell. This structure is beneficial to alleviating the volume expansion effect during high current charging and discharging. The outer shell is also a porous structure with a small pore size, which is convenient for stabilizing the structure. At the same time, it can increase the contact area with the electrolyte and improve the transmission efficiency of lithium ions.

[0069] Figure 3 The rate performance of Example 1 and Comparative Example 1 after being prepared as positive electrode materials is compared. The rate performance of the embodiment is the best, which is consistent with the morphology analysis. As can be seen from the figure, under the conditions of charge and discharge current density of 0.1, 1, 5, 10 and 0.1C, the discharge capacity of the embodiment is 218, 200, 186, 161 and 218 mAh / g respectively. With the increase of charge and discharge current density, its discharge capacity decreases. When the charge and discharge current density returns to the initial 0.1C, its discharge capacity returns to the initial level, showing the good reversible performance of the ultra-high nickel polycrystalline ternary positive electrode material, indicating that its structure has good stability.

[0070] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. An ultra-high nickel polycrystalline ternary positive electrode material, characterized in that: The chemical formula is aLiNi x Co y Mn z M 1-x-y-z O2·bLiNi x Co y Mn z M k Sr 1-x-y-z-k O2, M element is one or more of Ca and Mg; wherein, 0.9<x<1.0, 0<y<0.05, 0<z<0.05, 0.002<1-xyz<0.004, 0.001<k<0.003, 0<1-xyzk<0.002, 4≤b / a≤6.

2. The ultra-high nickel polycrystalline ternary positive electrode material according to claim 1, characterized in that: The particles of the material are spherical, and the cross section is a porous structure, which is divided into a core and a shell; wherein the pore size of the core is 200-500nm, the porosity is 18-22%, and the diameter accounts for 78-85% of the entire sphere; the pore size of the shell is 20-40nm, the porosity is 8-12%, and the thickness of the shell accounts for 15-22% of the entire sphere; The core component is LiNi x Co y Mn z M k Sr 1-x-y-z-k O2, the shell component is LiNi x Co y Mn z M 1-x-y-z O2; The D50 of the material is 16~18um, the particle size distance is 0.75<(D90-D10) / D50<0.95, and the tap density is 2.2~2.6g / cm 3 , with a specific surface area of ​​0.50~0.70m 2 / g.

3. A method for preparing an ultra-high nickel polycrystalline ternary positive electrode material, characterized in that: For preparing the ternary positive electrode material in claim 1 or 2, the preparation method comprises: Step 1, preparing a first mixed solution of Ni, Co, Mn, a strontium salt and a salt containing an M element, wherein the strontium salt is one or more of strontium acetate, strontium nitrate and strontium chloride; Preparing a second mixed solution of Ni, Co, Mn and a salt containing the M element; Prepare an oxalic acid solution with a molar concentration of 1-5 mol / L as a precipitant, and the temperature of the precipitant solution is 50°C; Step 2: Keep stirring the reactor on, introduce nitrogen, and add the first mixed solution and the precipitant in step 1 into the reactor for coprecipitation reaction; nitrogen is continuously introduced during the reaction, the reaction temperature is maintained at 50-70° C., and the speed of the reactor is 400-600 r / min; When the particle size D501 of the material in the reactor grows to 12.5-15.3 um, stop feeding the first mixed solution, improve the second mixed solution, and continue to grow the particle size of the material to 16-18 um. When the particle size distance reaches 0.75<(D90-D10) / D50<0.95, stop the reaction; After centrifugation, washing and drying, the ultra-high nickel polycrystalline ternary precursor is obtained, and its chemical formula is aNi x Co y Mn z M 1-x-y-z C2O2·bNi x Co y Mn z M k Sr 1-x-y-z-k C2O2; Step three: mix the ultra-high nickel polycrystalline ternary precursor prepared in step two with lithium salt, heat and react in a muffle furnace with oxygen, cool to room temperature after the reaction, and obtain the ultra-high nickel polycrystalline ternary positive electrode material through crushing and screening.

4. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step 1, the total molar concentration of Ni, Co, and Mn in the first mixed solution and the second mixed solution is 1.8-2.4 mol / L.

5. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step three, the purity of the oxygen is greater than 99.99%.

6. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step three, the molar ratio of the lithium salt to the ultra-high nickel polycrystalline ternary precursor is 1.02-1.

04.

7. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step three, the mixture of the ultra-high nickel polycrystalline ternary precursor and the lithium salt is placed in a muffle furnace, heated to 390-430°C at a heating rate of 10°C / min, reacted for 5 hours, then heated to 780-840°C at a heating rate of 3°C / min, reacted for 18-22 hours, and then cooled to room temperature at a cooling rate of 1.5°C / min.

8. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: The M element is one or more of Ca and Mg, and the M element-containing salt is one or a combination of calcium chloride and magnesium chloride.

9. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step three, the lithium salt is lithium hydroxide.

10. The method for preparing an ultra-high nickel polycrystalline ternary positive electrode material according to claim 3, characterized in that: In step 1, the Ni salt is nickel sulfate, the Co salt is cobalt sulfate, and the Mn salt is manganese sulfate.

Citation Information

Cited By

  • Porous high-nickel ternary positive electrode material and preparation method and application thereof

    CN120998961A