Halogen-oxygen compound multi-element solid solution type positive electrode material as well as preparation method and application thereof

Through the ball milling and solution reaction of halides and a variety of positive electrode materials, a halide-oxygen compound multi-solution positive electrode material is formed, which solves the problem of difficult to balance the high capacity and circulation performance of the positive electrode materials of lithium-ion batteries, and achieves high capacity , cycle stability and safety battery performance.

CN118943329AActive Publication Date: 2024-11-12NINGBO EASTERN INSTITUTE FOR ADVANCED STUDY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411017601.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing lithium-ion battery positive electrode materials are difficult to meet high capacity and good cycling performance at the same time, and the commonly used lithium insulator coating materials hinder lithium ions transmission, resulting in poor rate performance.

Method used

The solid solution reaction between halide and a variety of positive electrode materials is carried out through ball milling to form a halogen-oxygen compound multi-solution positive electrode material, delaying the decomposition process, inhibiting oxygen release, improving circulation performance, and solid solution of different layered positive electrode materials Improve the thermal stability and electrochemical properties of the battery.

Benefits of technology

It realizes maintaining the lithium ion diffusion coefficient and low interface resistance at high current density, significantly improving the reversible cycle capacity and cycle stability of the battery, and providing a lithium ion battery positive electrode material with high specific energy and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943329A_ABST
    Figure CN118943329A_ABST
Patent Text Reader

Abstract

The invention discloses a halogen-oxygen compound multi-element solid solution type positive electrode material and a preparation method and application thereof, and the preparation method of the halogen-oxygen compound multi-element solid solution type positive electrode material comprises the following steps: carrying out ball milling treatment on a halide MXa and at least two positive electrode material lithium composite oxides LixNO2, carrying out solid solution reaction in the ball milling process to obtain the multi-element solid solution type positive electrode material; wherein M comprises at least one selected from metal elements except Li and semi-metal elements, and X comprises at least one selected from F, Cl, Br and I; a is 1 to 5; n is at least one of transition metals; x is more than 0.5 and less than 1.10. The positive electrode material prepared by the preparation method provided by the invention simultaneously meets high capacity and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrode materials, and in particular to a halogen-oxygen compound multinary solid solution type positive electrode material and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy vehicles, higher requirements are placed on lithium-ion batteries that provide energy for them, especially the power performance and cycle performance requirements are more stringent. Capacity performance and cycle performance are key indicators for evaluating the quality of battery positive electrode materials. In current research, these two indicators are often difficult to meet at the same time. Therefore, finding lithium-ion battery positive electrode materials that meet both high capacity and good cycle performance has become the main goal of researchers.

[0003] Lithium iron phosphate has higher safety and cycle life, but relatively low energy density; lithium cobalt oxide has higher energy density, but shorter cycle life; ternary materials have better comprehensive performance, but the material price is higher; and lithium manganese oxide is a low-cost material, but has lower energy density.

[0004] At present, it is very important to modify the positive electrode materials of lithium batteries and further improve the battery performance of positive electrode materials, in order to maintain its high specific energy while taking into account cycle life and safety. Surface coating is a commonly used modification method, but most of the current coating materials are lithium "insulators", which hinder the migration and diffusion of lithium ions. Therefore, the lithium ion transmission rate and stability of the materials are poor at high rates, resulting in poor rate performance. Therefore, how to design lithium battery positive electrode materials with high specific energy, cycle life and safety has become one of the problems that need to be solved in the industry. Summary of the invention

[0005] The technical problem to be solved by the present invention is: how to prepare a lithium ion battery positive electrode material that meets both high capacity and good cycle performance. The present invention provides a halogen-oxygen compound multi-solid solution positive electrode material and its preparation method and application to solve the above problem.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a halogen-oxygen compound multinary solid solution positive electrode material comprises the following steps:

[0008] A halide MX a and at least two positive electrode materials lithium composite oxide Li x NO2 is ball-milled, and a multi-component solid solution positive electrode material is obtained through a solid solution reaction during the ball milling process; wherein:

[0009] M includes at least one selected from metal elements and semi-metal elements other than Li, X includes at least one selected from F, Cl, Br, I; a is 1 to 5;

[0010] N includes at least one of transition metals; 0.5<x<1.10.

[0011] The present invention adopts a halide and a plurality of positive electrode materials to solid-dissolve to prepare a composite positive electrode material. On the one hand: 1) The halide can delay the decomposition process of the layered positive electrode material, and at the same time slow down the release of oxygen in the positive electrode material through the oxidative decomposition of the halide. 2) The halide can also promote the phase change of oxidized chloride to oxide to capture oxygen species, thereby inhibiting the release of flammable oxygen gas and improving the thermal stability of the positive electrode material. On the other hand: 1) By solid-dissolving different layered positive electrode materials, the cycle performance of the layered positive electrode material is improved. For example, lithium cobalt oxide and lithium iron phosphate are ball-milled for solid solution, wherein the lithium iron phosphate layer is used as both an active material and a resistive barrier layer for overcharge and thermal runaway protection. The solid-solution electrode is not only resistant to overcharge current, but also can significantly reduce the surface temperature during overcharge, thereby significantly improving the cycle stability of lithium cobalt oxide. 2) For another example, although lithium iron phosphate has the advantages of high specific capacity, high safety and low cost, the discharge platform voltage is not high. By ball-milling it with lithium manganese oxide to form a solid solution, submicron-sized lithium iron phosphate particles can fill the gaps between the micron-sized particles of lithium manganese oxide, effectively blocking the direct contact between the electrolyte and lithium manganese oxide, inhibiting the dissolution of manganese, improving the electron transmission between the particles, reducing the internal resistance of the battery, and increasing the average operating voltage of the battery.

[0012] More specifically, the preparation method comprises:

[0013] Mixing halide material powder and positive electrode material powder in a specific ratio to obtain mixed fixed powder;

[0014] The mixed solid powder is transferred to a high-energy ball milling tank and then ball milled to obtain a ball-milled composite product.

[0015] Further optionally,

[0016] At least one halide MX a and at least two positive electrode materials lithium composite oxide Li x NO2 is ball-milled, and a multi-component solid solution positive electrode material is obtained through a solid solution reaction during the ball-milling process.

[0017] Further alternatively, the lithium composite oxide includes a compound having a layered rock salt structure, a compound having a spinel structure, or a compound having an olivine structure.

[0018] Further optionally, the compound having a layered rock salt structure comprises: Li x CoO2 (lithium cobalt oxide), Lix NiO2 (lithium nickel oxide), Li x MnO2 (lithium manganate), Li x NiMnO2 (nickel manganese oxide), Li x NiCoO2 (nickel cobalt oxide), Li x CoNiMnO2 (lithium cobalt nickel manganese oxide), Li x At least one of CoMnO2 (lithium cobalt manganese oxide) and Li2MnO3;

[0019] Alternatively, materials with a spinel structure include: LiMn2O4-based materials or LiNi 0.5 Mn 1.5 O4 series materials;

[0020] Alternatively, the compound having an olivine structure includes: LiNPO4, wherein N is at least one selected from Fe, Co, Mn, and Ni.

[0021] Further optionally, the mass ratio between the halide and the lithium composite oxide is:

[0022] There is one type of halide and two types of lithium composite oxides, and the corresponding mass ratio is 2:1:1 to 2:19:19;

[0023] And / or, there is one type of halide and three types of lithium composite oxides, and the corresponding mass ratio is 3:1:1:1 to 1:33:33:33;

[0024] And / or, there are two types of halides and two types of lithium composite oxides, and the corresponding mass ratio is 1:1:1:1 to 1:1:99:99;

[0025] And / or, there are two types of halides and three types of lithium composite oxides, and the corresponding mass ratios are 3:3:2:2:2 to 1:1:66:66:66.

[0026] When the halide ratio in the solid solution positive electrode material is too high, most of the capacity of the solid solution positive electrode comes from the halide, which results in significantly insufficient battery capacity and less than ideal electrochemical performance. When the halide ratio in the solid solution positive electrode is too low, the difficulty of solid solution between different positive electrodes increases significantly, the synergistic effect between different positive electrodes cannot be fully exerted, and the cycle stability decreases.

[0027] Further optionally, the mass ratio between the halide and the lithium composite oxide is:

[0028] And / or, there is one type of halide and three types of lithium composite oxides, and the corresponding mass ratio is 1:3:3:3 to 3:4:4:4;

[0029] And / or, there are two types of halides and two types of lithium composite oxides, and the corresponding mass ratio is 1:1:9:9 to 1:1:4:4;

[0030] And / or, there are two types of halides and three types of lithium composite oxides, and the corresponding mass ratios are 1:1:6:6:6 to 3:3:8:8:8.

[0031] Further optionally, the ball milling processing speed is 100 rpm to 700 rpm, and the ball milling time is 0.1 h to 22 h.

[0032] More preferably, the ball milling process speed is 300 rpm to 600 rpm, and the ball milling time is 0.1 h to 6 h.

[0033] A halogen-oxygen compound multinary solid solution type positive electrode material is prepared by adopting the above-mentioned method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material.

[0034] The invention discloses an application of a halogen-oxygen compound multi-component solid solution positive electrode material in the battery field.

[0035] A positive electrode plate comprises a halogen-oxygen compound multinary solid solution type positive electrode material prepared by the above-mentioned method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material.

[0036] The present invention has the following advantages and beneficial effects:

[0037] The present invention provides a halogen-oxygen compound multinary solid solution type positive electrode material, and a preparation method and application thereof. Due to the presence of an amorphous matrix, the positive electrode material enables the solid solution type positive electrode to maintain a high lithium ion diffusion coefficient and a low interface resistance during the entire charge and discharge process, thereby achieving reversible cycling at a high current density. In addition, the all-solid-state battery using the positive electrode material shows a high reversible capacity, which is due to the cumulative charge compensation of oxygen and halogen elements, showing a unique charge and discharge mechanism between cationic ordered rock salt crystals and amorphous parts. The introduction of an amorphous matrix and a halide provides a good ion conduction pathway and favorable ductility for the formation of a dense electrode layer, so that the solid solution type material has good ductility and high ionic conductivity. Solventizing lithium composite oxides with halides is an effective strategy for designing high-capacity electrode active materials.

[0038] The multi-component solid solution positive electrode provided by the present invention, after ball milling the halide and different positive electrodes, controls the appropriate ball milling speed and ball milling time, the materials all maintain good regular spherical particle morphology, and maintain the good crystallinity of the halide and the positive electrode material itself. Different from the amorphous halogen oxide positive electrode material, the multi-component solid solution positive electrode material has no obvious amorphous region and no obvious defect disordered structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0040] Figure 1 This is the SEM lattice image of the halogen-oxygen compound multinary solid solution type positive electrode material prepared in Example 1.

[0041] Figure 2 This is the SEM morphology of the halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 3.

[0042] Figure 3 This is the SEM morphology of the halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 4.

[0043] Figure 4 This is the SEM morphology of the halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 5.

[0044] Figure 5 This is the SEM morphology of the halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 6.

[0045] Figure 6 The halogen-oxygen compound multi-solid solution positive electrode material prepared in Example 1 was -1 Cyclic performance diagram under 24-hour conditions.

[0046] Figure 7 The halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 1 was -1 Cycle performance diagram.

[0047] Figure 8 The halogen-oxygen compound multi-solid solution positive electrode material prepared in Comparative Example 2 was -1 Cycle performance diagram. DETAILED DESCRIPTION

[0048] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0049] Example 1

[0050] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0051] Step 1: Add 0.4 g aluminum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganate is 1:2:2.

[0052] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0053] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0054] Comparative Example 1

[0055] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0056] Step 1: Add 1.2 g aluminum chloride, 0.4 g lithium cobalt oxide, and 0.4 g lithium manganese oxide into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium nickel manganese oxide is 3:1:1.

[0057] Step 2: After each 10-min ball milling, pause for 5 min and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to 0.5 h, and the ball milling speed is maintained at 500 rpm.

[0058] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0059] Comparative Example 2

[0060] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0061] Step 1: Add 0.04 g aluminum chloride, 0.98 g lithium cobalt oxide, and 0.98 g lithium manganese oxide into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium nickel manganese oxide is 2:49:49.

[0062] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0063] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0064] Comparative Example 3

[0065] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0066] Step 1: Add 0.4 g aluminum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganate is 1:2:2.

[0067] Step 2: After ball milling for 1 min, the ball milling speed was maintained at 500 rpm.

[0068] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0069] Comparative Example 4

[0070] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0071] Step 1: Add 0.4 g aluminum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganate is 1:2:2.

[0072] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to 24 hours, and the ball milling speed is maintained at 500 rpm.

[0073] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0074] Comparative Example 5

[0075] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0076] Step 1: Add 0.4 g aluminum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganate is 1:2:2.

[0077] Step 2: After each 10 minutes of ball milling, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to 0.5 hours, and the ball milling speed is maintained at 50 rpm.

[0078] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0079] Comparative Example 6

[0080] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0081] Step 1: Add 0.4 g aluminum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganate is 1:2:2.

[0082] Step 2: After each 10-min ball milling, pause for 5 min and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to 0.5 h, and the ball milling speed is maintained at 800 rpm.

[0083] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0084] Example 2

[0085] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0086] Step 1: Add 0.4 g aluminum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium manganese oxide, and 0.53 g lithium iron phosphate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide and lithium manganese oxide is 3:4:4:4.

[0087] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0088] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0089] Example 3

[0090] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0091] Step 1: Add 0.4 g tantalum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium manganese oxide, and 0.53 g lithium iron phosphate into a 500 mL high energy ball mill; wherein the mass ratio of tantalum chloride to lithium cobalt oxide and lithium manganese oxide is 3:4:4:4.

[0092] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0093] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0094] Example 4

[0095] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0096] Step 1: Add 0.4 g aluminum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium iron manganese phosphate, and 0.53 g lithium iron phosphate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide, lithium iron manganese phosphate, and lithium iron phosphate is 3:4:4:4.

[0097] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0098] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0099] Example 5

[0100] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0101] Step 1: Add 0.4 g aluminum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium iron manganese phosphate, and 0.53 g lithium iron phosphate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide, lithium iron manganese phosphate, and lithium iron phosphate is 3:4:4:4.

[0102] Step 2: After each 10-min ball milling, pause for 5 min and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to 2 h, and the ball milling speed is maintained at 500 rpm.

[0103] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0104] Example 6

[0105] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0106] Step 1: Add 0.4 g aluminum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium iron manganese phosphate, and 0.53 g lithium iron phosphate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lithium cobalt oxide, lithium iron manganese phosphate, and lithium iron phosphate is 3:4:4:4.

[0107] Step 2: After each ball milling for 10 minutes, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to be 2 hours, and the ball milling speed is maintained at 600 rpm.

[0108] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0109] Example 7

[0110] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0111] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 1:1:4:4.

[0112] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0113] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0114] Example 8

[0115] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0116] Step 1: Add 0.2 g aluminum chloride, 0.2 g zirconium chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to zirconium chloride, lithium cobalt oxide, and lithium manganate is 1:1:4:4.

[0117] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0118] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0119] Example 9

[0120] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0121] Step 1: Add 0.2g aluminum chloride, 0.2g zirconium chloride, 0.8g lithium cobalt oxide, and 0.8g lithium iron phosphate into a 500mL high-energy ball mill; wherein the mass ratio of aluminum chloride to zirconium chloride, lithium cobalt oxide, and lithium iron phosphate is 1:1:4:4.

[0122] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0123] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0124] Example 10

[0125] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0126] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 1:1:4:4.

[0127] Step 2: After each 10 minutes of ball milling, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to be 4 hours, and the ball milling speed is maintained at 500 rpm.

[0128] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0129] Embodiment 11

[0130] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0131] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.8 g lithium cobalt oxide, and 0.8 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 1:1:4:4.

[0132] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 600 rpm.

[0133] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0134] Example 12

[0135] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0136] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium manganate, and 0.53 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 3:3:8:8:8.

[0137] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0138] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0139] Embodiment 13

[0140] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0141] Step 1: Add 0.2 g aluminum chloride, 0.2 g zirconium chloride, 0.53 g lithium cobaltate, 0.53 g lithium manganate, and 0.53 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to zirconium chloride, lithium cobaltate, and lithium manganate is 3:3:8:8:8.

[0142] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0143] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0144] Embodiment 14

[0145] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0146] Step 1: Add 0.2g aluminum chloride, 0.2g lanthanum chloride, 0.53g lithium cobalt oxide, 0.53g lithium manganese oxide, and 0.53g lithium iron phosphate into a 500mL high-energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium iron phosphate is 3:3:8:8:8.

[0147] Step 2: After each 10-minute ball milling, pause for 5 minutes and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to be 0.5 hours, and the ball milling speed is maintained at 500 rpm.

[0148] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0149] Embodiment 15

[0150] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0151] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium manganate, and 0.53 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 3:3:8:8:8.

[0152] Step 2: After each 10-min ball milling, pause for 5 min and then continue the ball milling; then repeat the above steps, the total ball milling time is controlled to 2 h, and the ball milling speed is maintained at 500 rpm.

[0153] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0154] Example 16

[0155] This embodiment provides a halogen-oxygen compound multi-solution positive electrode material, and the specific preparation method is as follows:

[0156] Step 1: Add 0.2 g aluminum chloride, 0.2 g lanthanum chloride, 0.53 g lithium cobalt oxide, 0.53 g lithium manganate, and 0.53 g lithium manganate into a 500 mL high energy ball mill; wherein the mass ratio of aluminum chloride to lanthanum chloride, lithium cobalt oxide, and lithium manganate is 3:3:8:8:8.

[0157] Step 2: After each 10 minutes of ball milling, pause for 5 minutes and then continue ball milling; then repeat the above steps, the total ball milling time is controlled to 0.5 hours, and the ball milling speed is maintained at 600 rpm.

[0158] Except for the ball milling process, the loading and unloading processes were all carried out in a vacuum glove box, and the oxygen and water contents were controlled to be less than 0.1 ppm.

[0159] 1. Characterization and Analysis

[0160] The halogen-oxygen compound multi-solid solution cathode material prepared in Example 1 was photographed by scanning electron microscopy, and the effects of different ball milling speeds and ball milling times on the morphology of the solid solution cathode material were compared. The results are as follows: Figure 1-Figure 5 shown.

[0161] In Example 1, by controlling the appropriate ball milling speed and ball milling time, a solid solution positive electrode with regular spherical particles was prepared, and the morphology and structure remained relatively intact.

[0162] In Comparative Examples 3 and 5, it was found that when the ball milling time was too short or the ball milling speed was too low, the sample morphology was close to the initial positive electrode particles, and no obvious solid solution reaction occurred with the electrolyte.

[0163] In Comparative Examples 4 and 6, it was found that when the ball milling time was too long or the ball milling speed was too high, the sample morphology was severely damaged and the particles were of different sizes and shapes.

[0164] 2. Performance Test

[0165] 1. Battery preparation

[0166] The all-solid-state battery positive electrode active material and LiIn negative electrode of the multi-solid solution positive electrode combination prepared by Example 1, Comparative Example 1 and Comparative Example 2 were assembled in a glove box filled with argon. First, about 120 mg of Li6PS5Cl powder was pressed at 100 MPa for 1 min (diameter 10 mm). A composite positive electrode mixture was prepared by mixing the positive electrode active material, Li6PS5Cl and carbon black in a weight ratio of 70:30:1. On the Li6PS5Cl side of the solid electrolyte particle, about 10 mg of the composite positive electrode mixture was spread and pressed at 300 MPa for 2 min. On the other side of the particle, a thin indium foil (diameter 10 mg) was attached, and about 2 mg of lithium foil was pressed into a thin layer and placed on the indium foil. The mass loading of the composite positive electrode is 6 mg cm -2 .

[0167] 2. Test methods

[0168] The constant current charge / discharge voltage was set to 2.5V-4.3V relative to Li+ / Li. The charge and discharge curve test was performed at a current density of 0.1c. The cycle performance test was performed at a current density of 0.3c.

[0169] 3. Test results

[0170] The effects of different raw material ratios on the electrochemical performance of all-solid-state batteries were compared. In Example 1, the solid solution cathode synthesized by controlling the appropriate electrolyte and cathode mass ratio showed excellent cycling performance and high reversible capacity. After 50 cycles at 0.3C, the capacity remained at 218 mAh g -1 .

[0171] When the halide mass ratio is too high, the battery capacity decays to 100.5 mAh g -1 .

[0172] When the halide mass ratio is too low, the performance of the all-solid-state battery with halogen-oxygen compound multi-solid solution positive electrode deteriorates sharply, the capacity decay phenomenon is serious, the cycle stability decreases, and the capacity is only 124.9 mAh g after 50 cycles. -1 .

[0173] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a halogen-oxygen compound multi-solution positive electrode material, characterized in that: Includes steps: The halide MX a and at least two positive electrode materials lithium composite oxide Li x NO2 is ball-milled, and a multi-component solid solution positive electrode material is obtained through a solid solution reaction during the ball milling process; wherein: M includes at least one of a metal element and a semi-metal element other than Li, X includes at least one of F, Cl, Br, and I; a is 1 to 5; N includes at least one of transition metals; 0.5<x<1.

10.

2. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 1, characterized in that: At least one halide MX a and at least two positive electrode materials lithium composite oxide Li x NO2 is ball-milled, and a multi-component solid solution positive electrode material is obtained through a solid solution reaction during the ball-milling process.

3. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 1, characterized in that: The lithium composite oxide includes a compound having a layered rock salt structure, a compound having a spinel structure, or a compound having an olivine structure.

4. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 3, characterized in that: The compound having a layered rock salt structure includes: Li x CoO2、Li x NiO2、Li x MnO2、Li x NiMnO2、Li x NiCoO2、Li x CoNiMnO2、Li x At least one of CoMnO2 and Li2MnO3; Alternatively, materials with a spinel structure include: LiMn2O4-based materials or LiNi 0.5 Mn 1.5 At least one of O4 series materials; Alternatively, the compound having an olivine structure includes: LiNPO4, wherein N is at least one selected from Fe, Co, Mn, and Ni.

5. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 1, characterized in that: There is one type of halide and two types of lithium composite oxides, and the corresponding mass ratio is 2:1:1 to 2:19:19; And / or, there is one type of halide and three types of lithium composite oxides, and the corresponding mass ratio is 3:1:1:1 to 1:33:33:33; And / or, there are two types of halides and two types of lithium composite oxides, and the corresponding mass ratio is 1:1:1:1 to 1:1:99:99; And / or, there are two types of halides and three types of lithium composite oxides, and the corresponding mass ratios are 3:3:2:2:2 to 1:1:66:66:

66.

6. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 5, characterized in that: And / or, there is one type of halide and three types of lithium composite oxides, and the corresponding mass ratio is 1:3:3:3 to 3:4:4:4; And / or, there are two types of halides and two types of lithium composite oxides, and the corresponding mass ratio is 1:1:9:9 to 1:1:4:4; And / or, there are two types of halides and three types of lithium composite oxides, and the corresponding mass ratios are 1:1:6:6:6 to 3:3:8:8:

8.

7. The method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material according to claim 1, characterized in that: The ball milling process has a rotation speed of 100 rpm to 700 rpm, and a ball milling time of 0.1 h to 22 h.

8. A halogen-oxygen compound multi-solid solution positive electrode material, characterized in that: The positive electrode material is prepared by the method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material as described in any one of claims 1 to 7.

9. Application of a halogen-oxygen compound multi-solid solution positive electrode material in the battery field.

10. A positive electrode sheet, characterized in that: A halogen-oxygen compound multinary solid solution type positive electrode material prepared by the method for preparing a halogen-oxygen compound multinary solid solution type positive electrode material as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Cathode active material, cathode, and non-aqueous electrolyte secondary battery

    CN101414680A

  • Two-step high-energy ball milling method for preparation of lithium manganate solid solution anode material rich in lithium

    CN104157870A

  • High-capacity all-solid-state lithium-sulfur battery

    CN109449383A

  • Ball milling-heat treatment activation method of Li2MnO3 positive electrode material

    CN113443653A

  • Positive electrode material coated and modified by halide solid electrolyte and preparation method of positive electrode material