In-situ polymerization coating modified ultra-high nickel ternary material and preparation method and application thereof

Through two-stage in-situ polymerization coating technology, the structural instability problem of high-nickel ternary layered oxide positive electrode material is solved, and optimized interface and mechanical properties are formed, which improves the fast charging and high-temperature cycle stability of lithium-ion batteries. .

CN118943338AActive Publication Date: 2024-11-12CENT SOUTH UNIV +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411249630.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The structural instability of high-nickel ternary layered oxide positive electrode materials in lithium-ion batteries due to the increase in nickel content, including irreversible structural phase change, microcrack formation and Li+/Ni2+ disorder, resulting in increased risk of surface structure degradation and thermal runaway. , and conventional metal oxide coatings hinder lithium ion transport and lack mechanical stability.

Method used

Using two-stage in-situ polymerization coating method, monomer A, monomer B and additive C with specific structures are used to form a layer of cladding on the surface of ultra-high nickel ternary material to optimize interface stability and mechanical properties. Improve lithium ion conduction capability.

Benefits of technology

It realizes tolerance and fast charging performance in the electrolyte, maintains the stability of the cladding layer and positive electrode structure, and improves the high-temperature cycle stability and fast charging capability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943338A_ABST
    Figure CN118943338A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of battery materials, and particularly relates to a preparation method of an in-situ polymerization coated modified ultrahigh nickel ternary material, which comprises the following steps: obtaining a coating solution containing a monomer A, a monomer B and an additive C; the preparation method comprises the following steps: putting an ultra-high nickel ternary material into coating liquid, then carrying out first-stage polymerization at a temperature T1 in advance, and then carrying out second-stage polymerization at a temperature T2, so as to prepare the in-situ polymerization coating modified ultra-high nickel ternary material, the monomer A is a monomer with a structure shown in a formula 1 # imgabs0 #; the monomer B is obtained by carrying out Michael addition reaction on polyether amine and a compound shown in a formula 2 # imgabs 1 #; the additive C is a lithium-containing compound which is difficult to dissolve in the electrolyte; wherein the weight ratio of the additive C to the total monomer is (0.003-0.02): 1; 40 DEG C < = T1 < T2 < = 100 DEG C. The invention further discloses the material prepared by the preparation method and application. The material disclosed by the invention has excellent quick charging and high-temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-energy battery materials, and specifically relates to an in-situ polymerization-coated modified ultra-high nickel ternary material and its preparation method and application Background Art

[0002] Lithium-ion batteries currently dominate the electric vehicle market. High nickel ternary layered oxides (LiNi x Co y Mn z O2, NCM) has the advantages of high discharge specific capacity, low cost and environmental friendliness, and is considered to be the most advanced positive electrode material for lithium-ion batteries. The ultra-high nickel positive electrode obtained by increasing the nickel content in the NCM positive electrode can have a higher energy density of lithium-ion batteries. However, the increase in nickel content exacerbates a series of serious problems of NCM cathodes, such as irreversible structural phase transition, microcrack generation and Li + / Ni 2 + The instability of the NCM cathode structure is mainly attributed to the The local stress generated by the rapid anisotropic lattice strain during the phase transition. The local stress released along the grain boundaries leads to mechanical fatigue and microcrack formation in the bulk structure. The electrolyte then penetrates into the cathode particles and reacts with the exposed fresh surface, triggering a continuous irreversible phase transition, which slows down the lithium ion intercalation kinetics. The oxygen vacancies formed by the lattice oxygen escape will eventually lead to Li + / Ni 2+ Disorder, transition metal dissolution, and formation of rock-salt phases.

[0003] Many NCM cathode modification strategies have been developed, such as element doping, surface coating, and core-shell structure design. Among them, surface coating is an effective optimization method to directly improve the surface chemical and structural stability of cathode materials. Surface coating is expected to reduce side reactions between cathode and electrolyte and alleviate the dissolution of transition metals (TM) by hydrofluoric acid (HF) corrosion. However, conventional metal oxide materials hinder the transmission of lithium ions and do not have strong mechanical properties to cope with the considerable volume change of the cathode during the H2-H3 transformation process and maintain the integrity of the coating layer and the cathode body. Therefore, it is of great significance to develop a coating layer that can effectively prevent electrolyte corrosion, accelerate lithium ion transmission, and have a certain mechanical stability to maintain the stability of the coating layer itself and the cathode structure in long cycles, which is of great significance to expand the application of ultra-high nickel ternary cathode materials. Summary of the invention

[0004] In order to overcome the interface and structural stability problems of ultra-high nickel positive electrodes, the purpose of the present invention is to provide a method for preparing an in-situ polymerization-coated modified ultra-high nickel ternary material, aiming to prepare a modified high nickel positive electrode active material with excellent interface stability, the ability to withstand electrolyte corrosion and taking into account excellent fast charging and stability.

[0005] The second purpose of the present invention is to provide an in-situ polymerization-coated modified ultra-high nickel ternary material obtained by the preparation method and its application.

[0006] The third object of the present invention is to provide a battery comprising the in-situ polymerization-coated modified ultra-high nickel ternary material.

[0007] Due to the surface Ni 4+ The content is too high, the surface chemical environment of the high nickel positive electrode is not stable, and the highly catalytically active Ni 4+ It can cause the organic electrolyte system to decompose and produce gases such as CO2, CO, and H2. At the same time, since the surface of the high-nickel positive electrode usually has more residual lithium, the residual lithium will react with the electrolyte to generate a thicker CEI, which increases the lithium ion transmission path and slows down the lithium ion transmission speed. In view of this problem, the present invention has conducted in-depth research and provided the following solution:

[0008] A method for preparing an in-situ polymerization-coated modified ultra-high nickel ternary material, comprising obtaining a coating liquid containing a monomer A, a monomer B and an additive C; placing the ultra-high nickel ternary material in the coating liquid, then preliminarily performing a first stage polymerization at a temperature T1, and then performing a second stage polymerization at a temperature T2, to obtain the in-situ polymerization-coated modified ultra-high nickel ternary material;

[0009] The monomer A is a monomer having a structure of formula 1;

[0010]

[0011] The R1 is a saturated carbon chain, a saturated carbon ring, an unsaturated carbon ring, a carbon chain with a carbon ring, or a carbon chain with an unsaturated carbon ring;

[0012] The monomer B is obtained by Michael addition reaction of polyetheramine and compound of formula 2;

[0013]

[0014] The R2 is a C1-C6 alkyl group;

[0015] Additive C is a lithium-containing compound that is difficult to dissolve in conventional electrolytes; wherein the weight ratio of the total monomer of additive C is 0.003-0.02:1;

[0016] 40℃≤T1<T2≤100℃.

[0017] The present invention innovatively uses monomer A, monomer B and additive C to perform two-stage in-situ polymerization on the ultra-high nickel ternary material, so that a coating layer with stable interface and excellent mechanical properties and ion conductivity can be formed in situ on the surface of the ultra-high nickel ternary material. The present invention's research shows that the material prepared by the preparation method has a stable electrolyte / positive electrode interface and can exhibit excellent fast charging and high temperature cycle stability.

[0018] In the present invention, in Formula 1, R1 is a C1-C10 saturated carbon chain, a cyclohexyl ring, a cyclohexyl ring with a carbon chain, or a benzene ring;

[0019] Preferably, the monomer A is at least one of formula 1-a, formula 1-b, and formula 1-c;

[0020]

[0021] Preferably, monomer A is a composite monomer of formula 1-a and formula 1-c; further, the weight ratio of the two is 0.5 to 2: 1. The present invention shows that the preferred monomer A can synergistically further enhance the fast charging and high temperature stability of the material.

[0022] In the present invention, the polyetheramine can be a conventional polyetheramine in the industry. For example, it can be a conventional polyether polymer with -NH2 at the end. There is no special requirement for the molecular weight of the polyetheramine, for example, it can be 200 to 2500, more preferably 350 to 450, and specifically can be P108071 polyetheramine D-230, P108072 polyetheramine D-400, P108073 polyetheramine D-2000 provided by Aladdin Reagent.

[0023] In the present invention, the molar ratio of -NCO in monomer A to -NH2 in monomer B is 0.9 to 1.1:1.

[0024] In the present invention, the additive C comprises at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, and lithium difluorobis(oxalatoborate).

[0025] Preferably, the additive C is a composite of lithium difluorophosphate and lithium difluorooxalate borate; further, the weight ratio of lithium difluorophosphate to lithium difluorooxalate borate is 0.5 to 2: 1. The present invention shows that the preferred additive C can synergistically further enhance the fast charging and high temperature stability of the material.

[0026] Preferably, the weight ratio of additive C to total monomers is 0.005-0.01:1.

[0027] Preferably, the coating liquid is 1-10% by weight of the ultra-high nickel ternary material.

[0028] A dispersant is also added to the mixed system of the ultra-high nickel ternary material and the coating liquid, wherein the dispersant includes at least one of acetone and ethanol;

[0029] Preferably, the dispersant has a volume-to-weight ratio of 10 to 30 ml / g for the ultra-high nickel ternary material.

[0030] In the present invention, the high-nickel ternary material is an ultra-high nickel ternary material in which the nickel content accounts for more than 70 mol% of the total transition metals; preferably, it is at least one of the 8-series ultra-high nickel materials and the 9-series ultra-high nickel materials; further, it can be at least one of NCM811 and NCM90.

[0031] In the present invention, the ultra-high nickel ternary material is placed in a coating liquid for encapsulation treatment, and then the two-stage in-situ polymerization is carried out. This can achieve synergy, optimize the structure of the in-situ polymerization, improve its interface and mechanical properties, and further improve its active ion transmission ability, thereby synergistically improving its fast charging and long cycle stability.

[0032] In the present invention, the temperature T1 is 60-80°C;

[0033] Preferably, the holding time t1 at temperature T1 is 0.5 to 1.5 hours;

[0034] Preferably, the temperature T2 is 70-90°C;

[0035] Preferably, the holding time t2 at temperature T2 is 6 to 12 hours;

[0036] In the present invention, the preparation of the coating liquid and the first stage polymerization and the second stage polymerization can be carried out under an inert atmosphere; the inert atmosphere is, for example, at least one of nitrogen and argon.

[0037] The present invention also provides an in-situ polymerization-coated modified ultra-high nickel ternary material obtained by the preparation method.

[0038] The preparation method described in the present invention can give the prepared material special physical and chemical characteristics, and the material prepared by the preparation method has both excellent fast charging and long-range cycle performance.

[0039] The present invention also provides an application of the in-situ polymerization-coated modified ultra-high nickel ternary material, which is combined with a negative electrode, a separator and an electrolyte to assemble a lithium-ion battery.

[0040] The application described in the present invention can use the in-situ polymerization-coated modified ultra-high nickel ternary material described in the present invention as a positive electrode active material, and based on existing conventional principles and methods, produce the required lithium-ion battery.

[0041] The present invention also provides a composite positive electrode material, which includes a positive electrode active material, a conductive agent and a binder. The positive electrode active material contains the in-situ polymerization-coated modified ultra-high nickel ternary material described in the present invention as a positive electrode active material.

[0042] In the positive electrode active material of the present invention, the content of the in-situ polymerization-coated modified ultra-high nickel ternary material used as the positive electrode active material is above 50wt.%, and further above 80wt.%.

[0043] In the present invention, the conductive agent and the binder can be conventional components in the industry.

[0044] In the present invention, in the composite positive electrode material, the weight ratio of the positive electrode active material, the conductive agent and the binder can be 7-9.5:0.1-1.5:0.1-1.5.

[0045] The present invention also provides a positive electrode of a lithium ion battery, which comprises a current collector and a positive electrode material composited on the surface of the current collector, wherein the positive electrode material is the positive electrode active material described in the present invention.

[0046] The present invention also provides a lithium-ion battery, comprising a battery core and an electrolyte soaking the battery core, wherein the battery core comprises a positive electrode, a separator and a negative electrode compounded in sequence, and the positive electrode is compounded with the in-situ polymerized coated modified ultra-high nickel ternary material obtained by the preparation method.

[0047] Beneficial Effects

[0048] The present invention performs two-stage in-situ polymerization on the ultra-high nickel ternary material through the monomer A, monomer B and additive C of the structure, which can optimize the in-situ polymerization network structure, improve the interface structure, mechanical properties and ion conductivity, and improve its tolerance in the electrolyte, thereby synergistically improving its fast charging and high-temperature cycle stability.

[0049] The research of the present invention also shows that optimizing and controlling the composition of monomer A, monomer B and additive C and the in-situ polymerization process can further optimize the polymerization network and interface structure, and can further improve its fast charging and high-temperature cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 XRD patterns of samples prepared in Example 1, Example 2 Group A, Example 3 Group A and Example 4 Group A.

[0051] Figure 2 These are SEM images of samples prepared in Example 1, Example 2 Group A, Example 3 Group A, and Example 4 Group A.

[0052] Figure 3 This is the TEM image of Example 1.

[0053] Figure 4 4C / 100 cycle diagram of Example 1;

[0054] Figure 5 This is the 50°C / 100 cycle diagram of Example 1. DETAILED DESCRIPTION

[0055] The following examples are intended to further illustrate the present invention, but are not intended to limit the scope of protection of the present invention. The materials involved in the following examples can all be obtained from commercial channels.

[0056] The structure of the polyetheramine may be, for example, a component of the structure of Formula 3 It can be obtained based on conventional means. In the present invention, the polyetheramine can be purchased from Aladdin Company.

[0057] In the present invention, the monomer B can be obtained by a conventional Michael addition reaction between polyetheramine and Formula 2. For example, optionally, the polyetheramine is placed in a nitrogen atmosphere and stirred, and then Formula 2 is slowly added to the polyetheramine at 20 to 50° C., and after the dropwise addition is completed, the temperature is raised to 90 to 100° C. for Michael addition reaction (reaction time is, for example, 12 to 20 hours), and monomer B can be obtained, wherein the molar ratio of the input amount of polyetheramine (in terms of -NH2) and Formula 2 is 1:1 to 3.

[0058] As an optional scheme, the monomer B1 described in the following case is obtained by Michael addition reaction of formula 3A (polyetheramine D-230 with brand name P108071 and molecular weight of 230) and formula 2-A (compound of formula 2 wherein R2 is ethyl).

[0059] As an optional scheme, the monomer B2 described in the following case is obtained by Michael addition reaction of formula 3B (polyetheramine D-400 with brand name P108072 and molecular weight of 400) and formula 2-A (compound of formula 2 wherein R2 is ethyl).

[0060] As an optional scheme, the monomer B3 described in the following case is obtained by Michael addition reaction of formula 3C (a polyetheramine with the brand name P108073 polyetheramine D-2000 and a molecular weight of 2000) and formula 2-A (a compound of formula 2 in which R2 is ethyl).

[0061] Example 1

[0062] (1) 2 g of monomer A (Formula 1-a) and monomer B (monomer B1 in this case) were mixed in a molar ratio of -NCO and -NH2 of 1:1, and 0.01 g of additive C (lithium difluorophosphate) was added. The mixture was stirred in a magnetic stirrer at 30° C. and 100 rpm for 1 h to obtain a mixture, and the stirring was carried out under an argon atmosphere.

[0063] (2) 2 g of 9-series ultra-high nickel material NCM90 was dispersed in 25 ml of acetone, and then 0.02 g of the mixture of step (1) was added. After mixing, the mixture was pre-heated at temperature T1 (60°C) for t1 (0.5 h), and then heat-treated at temperature T2 (80°C) for t2 (6 h) to obtain an in-situ coated positive electrode material.

[0064] The positive electrode material obtained in Example 1 was configured into a positive electrode sheet according to the ratio of positive electrode active material: PVDF:super P of 8:1:1, and assembled into a 2016 type button lithium ion battery (the diaphragm was a PP diaphragm, and the electrolyte was a 1M concentration of LiTFSI lithium salt + (DOL:DME=1:1 volume ratio of solvent)). The charge and discharge test was carried out in the voltage range of 3.0-4.3V, and a metal lithium sheet was used as the battery negative electrode.

[0065] High rate test: The test was conducted at a high rate of 4C, the test temperature was 30°C, the battery was cycled at 4.0C, and 1C was 200mA / g. The test conditions were: the battery was first activated at 0.1C for 5 cycles, then activated at 0.5C for 2 cycles, and then cycled at 4.0C, 30°C, for 100 cycles. The test results are shown in Table 1.

[0066] High temperature test: The test was conducted at high temperature, the test temperature was 50°C, and the battery was cycled at 1.0C, 1C was 200mA / g. The test conditions were: the battery was first activated at 0.1C for 5 cycles, then activated at 0.5C for 2 cycles, and then cycled at 1.0C, 50°C for 100 cycles. The test results are shown in Table 2.

[0067] Example 2

[0068] Compared with Example 1, the only difference is that monomer A is changed. The experimental groups are:

[0069] Group A: Monomer A is of formula 1-b;

[0070] Group B: Monomer A is of formula 1-c;

[0071] Group C: Monomer A is a combination of formula 1-a and 1-c in equal weight proportions;

[0072] Comparative group A: Monomer A was replaced by

[0073] Other operations and parameters are the same as in Example 1.

[0074] Example 3

[0075] Compared with Example 1, the only difference is that monomer B is changed. The experimental groups are:

[0076] Group A: Monomer B is replaced by monomer B2;

[0077] Group B: monomer B is replaced by monomer B3;

[0078] Comparative group A: monomer B is pentamethylenediamine;

[0079] Other operations and parameters are the same as in Example 1.

[0080] Example 4

[0081] Compared with Example 1, the only difference is that the additive C is changed, and the other operations and parameters are the same as Example 1. The experimental groups are:

[0082] Group A: Additive C is lithium difluorobisoxalate borate;

[0083] Group B: Additive C is lithium difluorooxalate borate.

[0084] Group C: Additive C is a weight combination of lithium difluorophosphate, lithium difluorooxalatoborate, and the like.

[0085] Comparative group A: Additive C was replaced with an equal amount of lithium hexafluorophosphate;

[0086] Comparative group B: Additive C was replaced with an equal amount of lithium bis(trifluoromethanesulfonyl)imide.

[0087] Other operations and parameters are the same as in Example 1.

[0088] Example 5

[0089] Compared with Example 1, the only difference is that the weight ratio of additive C to total monomers is changed. The experimental groups are:

[0090] Group A: The weight ratio of additive C to total monomer is 0.01:1;

[0091] Group B: The weight ratio of additive C to total monomer is 0.015:1;

[0092] Comparative group A: the amount of additive C added was 0;

[0093] Other operations and parameters are the same as in Example 1.

[0094] Example 6

[0095] Compared with Example 1, the only difference is that the polymerization conditions are changed, that is, T1 is 70°C, t1 is 1.0H, T2 is 85°C, t2 is 8H. Other operations and parameters are the same as in Example 1.

[0096] Example 7

[0097] Compared with Example 1, the only difference is that the positive electrode active material is changed to NCM811, and the other operations and parameters are the same as Example 1.

[0098] Comparative Example 1

[0099] Compared with Example 1, the only difference is that no in-situ coating modification treatment is performed, that is, the mixture of step 1 is directly kept warm at temperature T1 (60°C) for t1 (0.5h) in advance, and then kept warm at temperature T2 (80°C) for t2 (6h) to react to obtain product a, and then 0.02g of product a is mixed with 25ml acetone solution containing 2g of 9-series ultra-high nickel material NCM90, and after mixing evenly, the acetone is evaporated to obtain the active material.

[0100] Other operations and parameters are the same as in Example 1. The results are shown in Table 1.

[0101] Comparative Example 2

[0102] Compared with Example 1, the only difference is that in step 1, the coating solution lacks additive C, and the solution containing monomer A and monomer B is pre-heated at temperature T1 (60° C.) for t1 (0.5 h), and then heated at temperature T2 (80° C.) for t2 (6 h) to react to obtain product b;

[0103] In step 2, 2 g of NCM90, 0.02 g of product b and 0.01 g of additive C are mixed and slurried with 25 mL of acetone, and then the acetone is removed to obtain the active material.

[0104] Other operations and parameters are the same as in Example 1. The results are shown in Table 1.

[0105] Comparative Example 3

[0106] Compared with Example 1, the only difference is that polymerization is carried out at a single temperature T1, that is, the temperature T2 is set to be the same as the temperature T1, and other operations and parameters are the same as in Example 1.

[0107] Comparative Example 4

[0108] Compared with Example 1, the only difference is that polymerization is carried out at a single temperature T2, that is, the temperature T1 is set to be the same as the temperature T2, and other operations and parameters are the same as in Example 1.

[0109] The positive electrode active materials obtained in Example 1, Example 2-A, Example 3-A and Example 4-A were tested and analyzed by X-ray diffraction (XRD) to obtain their XRD patterns, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the coated material obtained by the coating modification strategy adopted in the present invention still has the characteristic peaks of the standard NCM90 material, which shows that this modification strategy does not damage the ultra-high nickel positive electrode structure with poor stability due to high nickel content. The coating material and coating method are gentle and effective.

[0110] The positive electrode materials obtained in Example 1, Example 2-A, Example 3-A and Example 4-A were tested and analyzed using a scanning electron microscope (SEM) to obtain their SEM images. Figure 2 As shown in the figure, it can be seen that all samples have a complete spherical shape.

[0111] Combination Figure 3 , an amorphous layer can be observed on the surface of Example 1, which is attributed to the polymer coating layer.

[0112] Table 1 Comparison of electrochemical properties of the positive electrode materials prepared in the examples and comparative examples (tested at 30°C, first charge and discharge at 0.1C, followed by 4.0C cycles)

[0113]

[0114]

[0115] Table 2 Comparison of electrochemical properties of the positive electrode materials prepared in the examples and comparative examples (tested at 50°C, first charge and discharge at 0.1C, followed by 1.0C cycles)

[0116]

[0117]

[0118] It can be seen from the present invention that by adopting the method described in the present invention, excellent performance can be obtained, and under optimal conditions, better performance can be obtained.

Claims

1. A method for preparing an in-situ polymerization-coating modified ultra-high nickel ternary material, characterized in that: Obtaining a coating solution containing monomer A, monomer B and additive C; placing an ultra-high nickel ternary material in the coating solution, then pre-polymerizing at a temperature T1 for the first stage, and then polymerizing at a temperature T2 for the second stage, to obtain the in-situ polymerization-coated modified ultra-high nickel ternary material; The monomer A is a monomer having a structure of formula 1; The R1 is a saturated carbon chain, a saturated carbon ring, an unsaturated carbon ring, a carbon chain with a carbon ring, or a carbon chain with an unsaturated carbon ring; The monomer B is obtained by Michael addition reaction of polyetheramine and compound of formula 2; The R2 is a C1-C6 alkyl group; The additive C is a lithium-containing compound that is difficult to dissolve in the electrolyte; wherein the weight ratio of the additive C to the total monomer is 0.003 to 0.02:1; 40℃≤T1<T2≤100℃.

2. The method for preparing the in-situ polymerization-coating-modified ultra-high nickel ternary material according to claim 1, characterized in that: In the formula 1, R1 is a C1-C10 saturated carbon chain, a cyclohexyl ring, a cyclohexyl ring with a carbon chain, or a benzene ring; Preferably, the monomer A is at least one of formula 1-a, formula 1-b, and formula 1-c; Preferably, monomer A is a composite monomer of formula 1-a and formula 1-c.

3. The method for preparing the in-situ polymerization-coating-modified ultra-high nickel ternary material according to claim 1, characterized in that: The molar ratio of -NCO in monomer A to -NH2 in monomer B is 0.9 to 1.1:

1.

4. The method for preparing the in-situ polymerization-coating modified ultra-high nickel ternary material according to claim 1, characterized in that: The additive C comprises at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, and lithium difluorobis(oxalatoborate); Preferably, the additive C is a composite additive of lithium difluorophosphate and lithium difluorooxalate borate; Preferably, the weight ratio of additive C to total monomers is 0.005 to 0.01:

1.

5. The method for preparing the in-situ polymerization-coating-modified ultra-high nickel ternary material according to claim 1, characterized in that: The coating liquid is 1 to 10% of the weight of the ultra-high nickel ternary material; Preferably, a dispersant is further added to the mixed system of the ultra-high nickel ternary material and the coating liquid, and the dispersant includes at least one of acetone and ethanol; Preferably, the dispersant has a volume-to-weight ratio of 10 to 30 ml / g for the ultra-high nickel ternary material.

6. The method for preparing the in-situ polymerization-coating modified ultra-high nickel ternary material according to claim 1, characterized in that: The high nickel ternary material is an ultra-high nickel ternary material in which the nickel content accounts for more than 70 mol% of the total transition metals; preferably, at least one of the 8 series ultra-high nickel materials and the 9 series ultra-high nickel materials.

7. The method for preparing the in-situ polymerization-coating modified ultra-high nickel ternary material according to claim 1, characterized in that: The temperature T1 is 60-80°C; Preferably, the holding time t1 at temperature T1 is 0.5 to 1.5 hours; Preferably, the temperature T2 is 70-90°C; Preferably, the holding time t2 at temperature T2 is 6 to 12 hours.

8. An in-situ polymerization-coated modified ultra-high nickel ternary material obtained by the preparation method according to any one of claims 1 to 7.

9. An application of the in-situ polymerization-coating modified ultra-high nickel ternary material according to any one of claim 8, characterized in that: Combine it with the negative electrode, separator and electrolyte to assemble a lithium-ion battery.

10. A lithium ion battery, comprising a battery cell and an electrolyte for soaking the battery cell, wherein: The battery cell comprises a positive electrode, a separator and a negative electrode which are compounded in sequence, and is characterized in that the positive electrode is compounded with an in-situ polymerized, coated and modified ultra-high nickel ternary material obtained by the preparation method described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Coating method for improving ionic conductivity of positive electrode material of lithium ion battery and coated and modified positive electrode material

    CN111342050A

  • In-situ oxidative polymerization coated lithium ion ternary cathode material and preparation method thereof

    CN112164775A

  • Modified high-nickel ternary positive electrode material and preparation method thereof

    CN112864369A

  • Polymer coated high-nickel ternary positive electrode material as well as preparation method and application thereof

    CN114188515A

  • Method for preparing coating-modified high-nickel ternary cathode material, and prepared material

    US20240072245A1