Cathode active material and lithium secondary battery including same

By designing a positive electrode active material with a lithium ion diffusion path with an aspect ratio gradient, the problems of high energy density and life stability of the positive electrode material in lithium secondary batteries are solved, high energy density and stability are achieved, and battery expansion and cracks are reduced. Improves the life of lithium secondary batteries.

CN118943356APending Publication Date: 2024-11-12ECOPRO BM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410983612.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-08-19
Filing Date
2020-06-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The demand for cathode materials in lithium secondary batteries has challenges in high energy density and life stability in electric vehicle applications. Existing materials such as LiCoO2 are limited in cobalt resources, LiMnO2 is small in capacity and poor in high temperature characteristics, and LiNiO2 is difficult to synthesize. Cationic mixed discharge problem.

Method used

Using a positive electrode active material with a lithium ion diffusion path with an aspect ratio gradient, the specific structural design of primary and secondary particles can improve particle density and electrochemical characteristics, reduce strain caused by asymmetric volume expansion, and extend battery life.

Benefits of technology

It achieves high energy density and stability, reduces battery expansion and cracks, and improves the life and stability of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943356A_ABST
    Figure CN118943356A_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material and a lithium secondary battery comprising the same, the positive electrode active material comprising primary particles capable of occluding and releasing lithium; and secondary particles formed by aggregating the primary particles, the primary particles and the secondary particles satisfying formula 2: [formula 2] 1.35 < = X2 < = 1.95 (in formula 2, X2 is L2 / L3, and when the distance from the central part of the secondary particles to the surface part of the secondary particles is R, X2 is L2 / L3, and R is a distance from the central part of the secondary particles to the surface part of the secondary particles, X2 is L2 / L3, and R is a distance from the central part of the secondary particles to the surface part of the secondary particles. L2 represents the average aspect ratio of the primary particles present in a second region at a distance of 1 / 3R to 2 / 3R from the center of the secondary particles, and L3 represents the average aspect ratio of the primary particles present in a third region at a distance of 0 to 1 / 3R from the center of the secondary particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application with a filing date of June 29, 2020, application number 202010609508.7, and invention name “Positive electrode active material and lithium secondary battery comprising the same”. Technical Field

[0002] The present invention relates to a positive electrode active material and a lithium secondary battery using a positive electrode including the positive electrode active material, wherein primary particles contained in secondary particles have an aspect ratio gradient in which aspect ratios gradually increase from a central portion of the secondary particles toward a surface portion of the secondary particles. Background Art

[0003] Batteries store electricity using substances that can undergo electrochemical reactions at positive and negative electrodes. A representative example of such batteries is a lithium secondary battery that stores electrical energy by changes in chemical potential during the insertion / extraction of lithium ions at the positive and negative electrodes.

[0004] The lithium secondary battery is manufactured by using a material that can reversibly intercalate or deintercalate lithium ions as a positive electrode active material and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.

[0005] As a positive electrode active material of a lithium secondary battery, lithium composite oxides such as LiCoO 2 , LiMN 2 O 4 , LiNiO 2 , LiMnO 2 , etc. have been studied.

[0006] Among the above-mentioned positive electrode active materials, although LiCoO 2 having excellent life characteristics and charge and discharge efficiency is widely used, the above-mentioned material has limitations in price competitiveness due to the limited resources of cobalt used as a raw material and high price.

[0007] Although lithium manganese oxides such as LiMnO2 and LiMN2O4 have the advantages of good thermal stability and low price, they have problems such as small capacity and poor high temperature characteristics. In addition, although LiNiO2-based positive electrode active materials have battery characteristics of high discharge capacity, they are very difficult to synthesize due to the cation mixing problem between Li and transition metals, and there are great problems in rate characteristics.

[0008] In addition, according to the degree of the above-mentioned cation mixing, a large amount of Li by-products are generated, and since most of the Li by-products are composed of LiOH and Li2CO3 compounds, there are problems of gelation when manufacturing positive electrode slurry and gas generation during charge and discharge after manufacturing electrodes. Residual Li2CO3 increases the expansion of the battery, not only reducing the cycle, but also causing the battery to expand.

[0009] (Prior art literature)

[0010] (Patent Document)

[0011] (Patent Document 1) Korean Patent Publication No. 10-2015-0069334 Summary of the invention

[0012] Technical issues

[0013] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles plays a leading role in the market, and the demand for positive electrode materials used in lithium secondary batteries is also constantly changing.

[0014] For example, conventionally, lithium secondary batteries using LFP have been mainly used from the viewpoint of ensuring safety, but recently, the use of nickel-based lithium composite oxides having a larger energy capacity per unit weight than LFP has been expanding.

[0015] In light of these trends in cathode materials, an object of the present invention is to provide a cathode active material having high energy density and improved lifespan and stability.

[0016] In addition, another object of the present invention is to provide a positive electrode slurry composition comprising the positive electrode active material defined herein.

[0017] In addition, another object of the present invention is to provide a lithium secondary battery, wherein the lithium secondary battery comprises a positive electrode, and the positive electrode is formed by coating the positive electrode slurry composition defined herein on a current collector.

[0018] The purpose of the present invention is not limited to the purpose mentioned above (for example, electric vehicle use), and other purposes and advantages of the present invention not mentioned can be understood through the following description, and can be more clearly understood through the embodiments of the present invention. In addition, it can be easily understood that the purpose and advantages of the present invention can be achieved by the means and combinations thereof in the claims.

[0019] Solutions to the problem

[0020] According to one aspect of the present invention, there is provided a positive electrode active material, the positive electrode active material comprising primary particles capable of absorbing and releasing lithium; and secondary particles, the primary particles are agglomerated, the primary particles and the secondary particles satisfy the following formula 2,

[0021] [Formula 2]

[0022] 1.35≤X2≤1.95

[0023] In the above formula 2, X2 is L2 / L3, when the distance from the center of the secondary particle to the surface of the secondary particle is R,

[0024] The above-mentioned L2 represents the average aspect ratio of the above-mentioned primary particles existing in the second region with a distance of 1 / 3R to 2 / 3R from the center of the above-mentioned secondary particles, and L3 represents the average aspect ratio of the above-mentioned primary particles existing in the third region with a distance of 0 to 1 / 3R from the center of the above-mentioned secondary particles.

[0025] In one embodiment, the primary particles and the secondary particles may satisfy the following formula 1:

[0026] [Formula 1]

[0027] 1.15≤X1≤1.75

[0028] In Formula 1, X1 is L1 / L2, and L1 represents the average aspect ratio of the primary particles present in the first region at a distance of 2 / 3R to R from the center of the secondary particles.

[0029] In one embodiment, the primary particles and the secondary particles may satisfy the following formula 3:

[0030] [Formula 3]

[0031] X1 / X2≥0.70.

[0032] In one embodiment, the L1 may be greater than or equal to 2.13 and less than or equal to 3.94.

[0033] In one embodiment, the primary particles and the secondary particles may satisfy the following formula 4:

[0034] [Formula 4]

[0035] X3≥1.70

[0036] In the above formula 4, X3 is L1 / L3, and L1 represents the average aspect ratio of the primary particles present in the first region at a distance of 2 / 3R to R from the center of the secondary particles.

[0037] In one embodiment, the X3 may be greater than or equal to 1.76 and less than or equal to 3.23.

[0038] In one embodiment, the above L3 may be greater than 1.09.

[0039] In one embodiment, the primary particle may have an aspect ratio that continuously increases from a center portion of the secondary particle toward a surface portion of the secondary particle.

[0040] In one embodiment, the primary particle may be in a rod shape radiating from a center portion of the secondary particle toward a surface portion of the secondary particle, and a long axis direction of the primary particle may be directional toward the center portion of the secondary particle.

[0041] In one embodiment, the angle formed by the lithium ion diffusion path in the primary particle and the long axis direction of the primary particle may be ±40°.

[0042] In one embodiment, the lithium ion diffusion path may be formed to have an angle within ±40° with respect to a direction connecting a central portion of the secondary particle to a surface portion of the secondary particle.

[0043] In one embodiment, the primary particle may be represented by the following chemical formula 1:

[0044] [Chemical formula 1]

[0045] Li w Ni 1-(x+y+z) Co x M1 y M2 z O2

[0046] Among them, M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, B, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0.01≤x≤0.50, 0.01≤y≤0.20, 0.001≤z≤0.20.

[0047] In one embodiment, the positive electrode active material may include a coating, the coating covers at least a portion of a region selected from the interface between the primary particles and the surface of the secondary particles, and the coating includes at least one oxide represented by the following chemical formula 2:

[0048] [Chemical formula 2]

[0049] Li a M3b O c

[0050] Among them, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, and 0≤a≤10, 0≤b≤8, 2≤c≤13.

[0051] According to still another aspect of the present invention, there is provided a lithium secondary battery, wherein a positive electrode including the positive electrode active material described above is used.

[0052] According to one aspect of the present invention, there is provided a positive electrode active material, the positive electrode active material comprising: primary particles capable of absorbing and releasing lithium; and secondary particles formed by agglomeration of the primary particles.

[0053] The primary particles included in the secondary particles have an aspect ratio gradient in which the aspect ratio gradually increases from the center of the secondary particles toward the surface of the secondary particles.

[0054] At this time, the primary particles and the secondary particles contained in the positive electrode active material can increase the particle density in the positive electrode active material by at least satisfying the following formula 1. Thus, the electrochemical characteristics of the positive electrode active material can be improved.

[0055] [Formula 1]

[0056] X1≥1.15(X1=L1 / L2)

[0057] (Wherein, when the distance from the center of the secondary particle to the surface of the secondary particle is R, the L1 represents the average aspect ratio of the primary particles in the first region where the distance from the center of the secondary particle is 2 / 3R to R, and the L2 represents the average aspect ratio of the primary particles in the second region where the distance from the center of the secondary particle is 1 / 3R to 2 / 3R)

[0058] Furthermore, the primary particles and the secondary particles contained in the positive electrode active material can further increase the particle density in the positive electrode active material by at least satisfying the following formula 2. In addition, when the lithium secondary battery prepared using the positive electrode active material is charged / discharged, the partial strain caused by asymmetric volume expansion can be effectively reduced.

[0059] [Formula 2]

[0060] X2≥1.35(X2=L2 / L3)

[0061] (wherein L3 represents the average aspect ratio of the primary particles present in the third region having a distance of 0 to 1 / 3R from the center of the secondary particles)

[0062] Furthermore, the primary particles in the secondary particles are in the shape of rods radiating from the center portion of the secondary particles toward the surface portion of the secondary particles, and the primary particles have an aspect ratio gradient increasing from the center portion of the secondary particles toward the surface portion of the secondary particles, so that the rod shape of the primary particles can develop toward the surface portion of the secondary particles.

[0063] The primary particles are in the shape of rods with different lengths of the long axis (a-axis) and the short axis (c-axis), and a lithium ion diffusion path exists in a direction parallel to the long axis (a-axis) of the primary particles, thereby further improving the electrochemical properties of the positive electrode active material.

[0064] Furthermore, according to another aspect of the present invention, a positive electrode slurry composition is provided, wherein the positive electrode slurry composition comprises a positive electrode active material as defined herein, a conductive material and a binder.

[0065] In addition, according to another aspect of the present invention, a lithium secondary battery is provided. The lithium secondary battery includes a positive electrode, and the positive electrode is formed by coating the positive electrode slurry composition as defined herein on a current collector.

[0066] Effects of the Invention

[0067] The positive electrode active material according to various embodiments of the present invention includes: primary particles capable of occluding and releasing lithium; and secondary particles formed by agglomeration of the primary particles, wherein the primary particles contained in the secondary particles present an aspect ratio gradient in which the aspect ratio gradually increases from the central portion of the secondary particles toward the surface portion of the secondary particles, thereby increasing the density of the primary particles in the secondary particles. As a result, a high energy density of the positive electrode active material can be expected.

[0068] Furthermore, the aspect ratio gradient presented by the primary particles contained in the secondary particles has a directionality that increases within a specific range, and in particular, when the lithium secondary battery is charged / discharged, the partial strain caused by the asymmetric volume expansion of the positive electrode active material can be effectively reduced. By reducing the strain as above, the generation of cracks after the life of the positive electrode active material can be reduced. Therefore, the life and stability of the lithium secondary battery can be improved.

[0069] Specific matters for implementing the invention will be described below, and specific effects of the present invention and the above-mentioned effects will be described. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 The diagram shows the direction of the major axis (a-axis) of the primary particles contained in a partial region of the positive electrode active material (secondary particles) of one embodiment of the present invention and the lithium ion diffusion path formed in the primary particles.

[0071] Figure 2 and Figure 3 The figure shows the aspect ratio gradient of the primary particles contained in the positive electrode active material (secondary particles) and the lithium ion diffusion path according to one embodiment of the present invention.

[0072] Figures 4 to 9 1 and 2 are cross-sectional SEM images of the positive electrode active materials according to Examples 1 to 6 of the present invention.

[0073] Fig.10 and Fig.11 The cross-sectional SEM images of the positive electrode active materials according to Comparative Example 1 and Comparative Example 2, respectively.

[0074] Fig.12 The cross-sectional SEM photos of the positive electrode active material before (a) and after (b) the life of the positive electrode active material according to Example 1 of the present invention are as follows: Fig.13 These are cross-sectional SEM photographs of the positive electrode active material according to Comparative Example 1 before (a) and after (b) the lifespan. DETAILED DESCRIPTION

[0075] In order to easily understand the present invention, specific terms are appropriately defined in this application. Unless otherwise defined herein, the scientific terms and technical terms used in the present invention have the meanings commonly understood by those skilled in the art to which the present invention belongs. In addition, unless the context requires otherwise, the terms in the singular form shall include the plural form and the terms in the plural form shall include the singular form.

[0076] Hereinafter, the cathode active material according to the present invention and a lithium secondary battery using a cathode including the cathode active material will be described in further detail.

[0077] Positive electrode active material

[0078] According to one aspect of the present invention, there is provided a positive electrode active material, the positive electrode active material comprising: primary particles capable of absorbing and releasing lithium; and secondary particles formed by agglomeration of the primary particles.

[0079] The primary particle refers to a crystal grain or crystallite, and the secondary particle refers to an aggregate formed by agglomeration of a plurality of primary particles. There may be gaps and / or grain boundaries between the primary particles constituting the secondary particle.

[0080] In addition, the shape of the primary particle is not particularly limited, but preferably, it can have a rod shape relative to a spherical shape in a region adjacent to the central portion of the secondary particle. On the other hand, the primary particle has an aspect ratio gradient that increases from the central portion of the secondary particle toward the surface portion of the secondary particle, so that the rod shape can be developed toward the surface portion of the secondary particle.

[0081] Here, the average major axis length of the primary particles is in the range of 0.01 μm to 5 μm, preferably in the range of 0.01 μm to 2 μm, so that the optimal density of the positive electrode prepared using the positive electrode active material of various embodiments of the present invention can be achieved. In addition, the average particle size of the secondary particles may vary depending on the number of agglomerated primary particles, but may be in the range of 0.1 μm to 25 μm.

[0082] In one embodiment, the primary particles included in the secondary particles have an aspect ratio gradient in which the aspect ratio gradually increases from a center portion of the secondary particles toward a surface portion of the secondary particles.

[0083] As used herein, the term "aspect ratio" refers to the ratio (Length / Width ratio) of the major axis (Length; a-axis) to the minor axis (Width; c-axis) of the primary particle. When the major axis represents the direction of the relatively long region of the primary particle, the minor axis represents the length of the relatively short region of the primary particle. In this case, the minor axis may be a direction perpendicular to the major axis.

[0084] Thus, the primary particles can be in the shape of rods having different lengths of the major axis (a-axis) and the minor axis (c-axis).

[0085] Hereinafter, for convenience, the major axis is defined as an a-axis, and the minor axis is defined as a c-axis.

[0086] In one embodiment, a lithium ion diffusion path may exist in the primary particle, and the lithium ion diffusion path may exist in a direction parallel to the a-axis direction of the primary particle.

[0087] In the case of the existing positive electrode active material (secondary particle), since the a-axis of the primary particle forming the positive electrode active material (secondary particle) is randomly oriented, the lithium ion diffusion path existing along the a-axis direction of the primary particle must also exist randomly. Therefore, it is difficult to effectively form a lithium ion diffusion path in the direction from the center of the secondary particle toward the surface of the secondary particle.

[0088] In addition, in the case of existing positive electrode active materials, there is no aspect ratio gradient that gradually increases from the center of the above-mentioned secondary particles toward the surface of the above-mentioned secondary particles. Therefore, the density of the above-mentioned primary particles in the above-mentioned secondary particles must be relatively low. During charging / discharging, due to the random volume expansion of the above-mentioned primary particles, cracks are likely to occur in the above-mentioned positive electrode active material.

[0089] On the other hand, according to one embodiment of the present invention, the primary particle has an aspect ratio gradient that increases from the center of the secondary particle toward the surface of the secondary particle, and at this time, the aspect ratio gradient is characterized by satisfying the following specific numerical range. In addition, the primary particle having the aspect ratio gradient pattern exists radially from the center of the secondary particle, so that during charging / discharging, the strain caused by the volume expansion of the primary particle can be effectively reduced. Therefore, the life and stability of the lithium secondary battery using the positive electrode active material can be improved.

[0090] In addition, in the case of forming the primary particles of the positive electrode active material (secondary particles) of one embodiment of the present invention, the a-axis direction is oriented in a manner toward the center of the secondary particles. In addition, the primary particles have a rod shape radiating from the center of the secondary particles toward the surface of the secondary particles. By the agglomerated shape as described above, a lithium ion diffusion path can be formed in the direction from the center of the secondary particles toward the surface of the secondary particles. The energy density can be increased by increasing the density of the primary particles agglomerated in the secondary particles.

[0091] Figure 1 The diagram shows the direction of the major axis (a-axis) of the primary particles contained in a partial region of the positive electrode active material (secondary particles) of one embodiment of the present invention and the lithium ion diffusion path formed in the primary particles. Figure 2 and Figure 3 The figure shows the aspect ratio gradient of the primary particles contained in the positive electrode active material (secondary particles) and the lithium ion diffusion path according to one embodiment of the present invention.

[0092] Reference Figures 1 to 3The lithium ion diffusion path existing in the above-mentioned primary particle, which presents an aspect ratio gradient increasing from the central portion of the above-mentioned secondary particle toward the surface portion of the above-mentioned secondary particle, can exist in a direction parallel to the a-axis direction of the above-mentioned primary particle.

[0093] At this time, the existence of the above-mentioned lithium ion diffusion path in a direction parallel to the a-axis direction of the above-mentioned primary particle should be understood as not only including the situation where the above-mentioned lithium ion diffusion path exists in a direction exactly consistent with the a-axis direction of the above-mentioned primary particle, but also including the situation where the angle formed by the above-mentioned lithium ion diffusion path and the a-axis direction of the above-mentioned primary particle is within ±40°, preferably within ±30°.

[0094] That is to say, the lithium ion diffusion path may exist in a manner forming an angle within ±40° relative to the a-axis direction of the primary particle. At this time, the angle formed by the lithium ion diffusion path relative to the direction connecting the surface of the secondary particle from the center of the secondary particle may also be within ±40°.

[0095] In the above embodiment, the primary particle may have an aspect ratio gradient that continuously increases from the center portion of the secondary particle toward the surface portion of the secondary particle, but the present invention is not limited thereto.

[0096] That is, the aspect ratio of the primary particle increases from the center of the secondary particle toward the surface of the secondary particle, and at the same time, the aspect ratio gradient of the primary particle can increase continuously or discontinuously according to the way the gradient is defined. In this case, the primary particle and the secondary particle preferably have an aspect ratio gradient satisfying the following formulas 1 to 4.

[0097] At this time, the primary particles and the secondary particles contained in the positive electrode active material can increase the particle density in the positive electrode active material by at least satisfying the following formula 1. Thus, the electrochemical characteristics of the positive electrode active material can be improved.

[0098] [Formula 1]

[0099] X1≥1.15(X1=L1 / L2)

[0100] (in,

[0101] When the distance from the center of the secondary particle to the surface of the secondary particle is R,

[0102] L1 represents the average aspect ratio of the primary particles present in the first region ranging from 2 / 3R to R from the center of the secondary particles.

[0103] The above L2 represents the average aspect ratio of the above primary particles present in the second region having a distance of 1 / 3R to 2 / 3R from the center of the above secondary particles)

[0104] When X1 in Formula 1 is less than 1.15, as the density of the primary particles present in the first region decreases, the surface area of ​​the secondary particles may increase. When the surface area of ​​the secondary particles increases, the possibility of side reactions with the electrolyte in the lithium secondary battery increases, and thus the life and / or stability of the lithium secondary battery may decrease.

[0105] On the other hand, when X1 in Formula 1 is greater than 1.75, as the difference in aspect ratio of the primary particles existing in the first region and the second region becomes relatively large, asymmetric volume expansion may occur during charge / discharge.

[0106] In addition, the primary particles and the secondary particles contained in the positive electrode active material can further increase the particle density in the positive electrode active material by at least satisfying the following formula 2. In addition, when the lithium secondary battery prepared using the positive electrode active material is charged / discharged, the partial strain caused by asymmetric volume expansion can be effectively reduced.

[0107] [Formula 2]

[0108] X2≥1.35(X2=L2 / L3)

[0109] (in,

[0110] L3 represents the average aspect ratio of the primary particles present in the third region having a distance of 0 to 1 / 3R from the center of the secondary particles.

[0111] When X2 in the above formula 1 is less than 1.35, it is difficult for the above-mentioned primary particles present in the above-mentioned second region surrounding the above-mentioned third region to have sufficient radial orientation relative to the above-mentioned third region, and it may be difficult to fully increase the density of the above-mentioned primary particles in the above-mentioned second region located between the above-mentioned first region and the above-mentioned third region.

[0112] On the other hand, when X1 in the above formula 1 is greater than 1.95, the difference in aspect ratio of the above-mentioned primary particles existing in the above-mentioned second region and the above-mentioned third region becomes relatively large, and the difference in aspect ratio of the above-mentioned primary particles existing in the above-mentioned first region and the above-mentioned second region becomes relatively small, and as a result, the difference in aspect ratio of the above-mentioned primary particles existing in the central portion of the above-mentioned secondary particles and the surface portion of the above-mentioned secondary particles becomes too large, and thus the possibility of rupture due to volume expansion of the above-mentioned primary particles during charging / discharging may increase.

[0113] In addition, the primary particles and the secondary particles contained in the positive electrode active material may satisfy the following formula 3 representing the ratio of the result values ​​of the formula 1 and the formula 2. Thus, the primary particles may present an aspect ratio gradient that gradually increases from the center of the secondary particles toward the surface of the secondary particles, and may be in a rod shape that gradually develops from the center of the secondary particles toward the surface of the secondary particles.

[0114] [Formula 3]

[0115] X2 / X1≥0.70

[0116] In addition, preferably, the primary particles and the secondary particles contained in the positive electrode active material at least satisfy the following formula 4. The following formula 4 is the minimum size of the aspect ratio gradient of the primary particles present in the secondary particles, and by making the primary particles and the secondary particles satisfy the following formula 4, a high energy density in the positive electrode active material can be expected.

[0117] [Formula 4]

[0118] X3≥1.70(X3=L1 / L3)

[0119] The primary particles satisfying the above Formulas 1 to 4 may be defined as a lithium composite oxide represented by the following Chemical Formula 1.

[0120] [Chemical formula 1]

[0121] Li w Ni 1-(x+y+z) Co x M1 y M2 z O2

[0122] (Wherein, M1 is at least one selected from Mn and Al,

[0123] M2 is at least one selected from the group consisting of Mn, B, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu,

[0124] M1 and M2 are different elements.

[0125] 0.5≤w≤1.5,0.01≤x≤0.50,0.01≤y≤0.20,0.001≤z≤0.20)

[0126] In addition, M2 present on the surface of the secondary particle may represent a concentration gradient that decreases toward the center of the secondary particle. In other words, the concentration gradient direction of M2 may be from the surface of the secondary particle toward the center of the secondary particle.

[0127] Furthermore, in another embodiment, the positive electrode active material may include a coating layer covering at least a portion of the surface of the primary particles (eg, the interface between the primary particles) and / or the secondary particles formed by agglomeration of the primary particles.

[0128] For example, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle. In particular, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle.

[0129] Thus, the coating layer may exist as a layer that continuously or discontinuously coats the surface of the primary particles and / or the secondary particles formed by agglomerating the primary particles. When the coating layer exists discontinuously, it may exist in the form of islands.

[0130] The presence of the coating as above can help improve the physical and electrochemical characteristics of the positive electrode active material.

[0131] Furthermore, the coating layer may exist in the form of a solid solution without forming a boundary with the primary particles and / or the secondary particles formed by agglomerating the primary particles.

[0132] The coating layer may include at least one oxide represented by the following Chemical Formula 2. That is, the coating layer may be defined as a region where the oxide represented by the following Chemical Formula 2 exists.

[0133] [Chemical formula 2]

[0134] Li a M3 b O c

[0135] (in,

[0136] M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd,

[0137] and 0≤a≤10, 0≤b≤8, 2≤c≤13)

[0138] Also, the coating layer may have a form in which different types of oxides exist simultaneously in one layer or may have a form in which different types of oxides represented by the above Chemical Formula 2 exist in different layers, respectively.

[0139] The oxide represented by the above Chemical Formula 2 may be physically and / or chemically bonded to the primary particles represented by the above Chemical Formula 1. Also, the oxide may exist in a state of forming a solid solution with the primary particles represented by the above Chemical Formula 1.

[0140] The positive electrode active material according to the present embodiment includes a coating, and the coating covers at least a portion of the surface of the primary particles (e.g., the interface between the primary particles) and / or the secondary particles formed by the agglomeration of the primary particles, thereby improving the structural stability. Moreover, when the positive electrode active material is used in a lithium secondary battery, the high temperature storage stability and life characteristics of the positive electrode active material can be improved. Moreover, the oxide reduces the residual lithium in the positive electrode active material and serves as a path for the movement of lithium ions, thereby affecting the efficiency characteristics of the lithium secondary battery.

[0141] Furthermore, depending on circumstances, the oxide may exist not only at the interface between the primary particles and at least a portion of the surface of the secondary particles, but also in internal voids formed in the secondary particles.

[0142] The oxide is an oxide obtained by combining lithium and an element represented by A or an oxide of A. Examples of the oxide are Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a B b O c , Li a Co b O c , Li a Al b O c 、Co b O c 、Al b O c , W b O c 、Zr b O c 、Tib O c or B b O c However, the above examples are only described for ease of understanding, and the oxides defined in this article are not limited to the above examples.

[0143] In another embodiment, the oxide may be an oxide formed by compounding lithium and at least two elements represented by A or further includes an oxide formed by compounding lithium and at least two elements represented by A. Examples of the oxide formed by compounding lithium and at least two elements represented by A may be Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c Li a (W / Ti / B) b O c Etc., but the present invention is not limited thereto.

[0144] The oxide may have a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle. Thus, the concentration of the oxide may decrease from the outermost surface of the secondary particle toward the center of the secondary particle.

[0145] As described above, the oxide has a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle, thereby effectively reducing the residual lithium present on the surface of the positive electrode active material to prevent side reactions caused by unreacted residual lithium. In addition, the oxide can also prevent the crystallinity of the inner surface area of ​​the positive electrode active material from decreasing. In addition, the oxide can prevent the overall structure of the positive electrode active material from collapsing during the electrochemical reaction.

[0146] In addition, the coating layer may include a first oxide layer and a second oxide layer, wherein the first oxide layer includes at least one oxide represented by the chemical formula 2, and the second oxide layer includes at least one oxide represented by the chemical formula 2 but includes an oxide different from the oxide included in the first oxide layer.

[0147] For example, the first oxide layer may exist in a manner that covers at least a portion of the exposed surface of the primary particle present at the outermost periphery of the secondary particle, and the second oxide layer may exist in a manner that covers the exposed surface of the primary particle not covered by the first oxide layer and at least a portion of the surface of the first oxide layer.

[0148] Lithium secondary battery

[0149] According to another aspect of the present invention, a positive electrode including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector may be provided. The positive electrode active material layer may include a positive electrode active material according to various embodiments of the present invention. Therefore, the positive electrode active material is the same as the positive electrode active material described above, so a detailed description will be omitted for convenience, and only the remaining composition will be specifically described below.

[0150] The positive electrode collector is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and examples thereof may include: stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode collector may generally have a thickness of 3 μm to 500 μm, or the adhesion of the positive electrode active material may be increased by forming micro-concave and convex on the surface of the collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0151] The positive electrode active material layer can be prepared by coating a positive electrode slurry composition on the positive electrode current collector. The positive electrode slurry composition includes the positive electrode active material, a conductive material, and a selective binder as required.

[0152] The content of the positive electrode active material may be 80 to 99 wt %, more specifically 85 to 98.5 wt %, relative to the total weight of the positive electrode active material layer. When the content of the positive electrode active material is within the above range, excellent capacity characteristics may be achieved, but the present invention is not necessarily limited thereto.

[0153] The above-mentioned conductive material is used to provide conductivity to the electrode, and can be used without limitation, as long as it has electronic conductivity and does not cause chemical changes in the assembled battery. Specific examples thereof may include: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc., and these substances can be used as a single one or as a mixture of two or more. The content of the above-mentioned conductive material can be 0.1 wt% to 15 wt% relative to the total weight of the positive electrode active material layer.

[0154] The above-mentioned binder serves to adhere the positive electrode active material particles to each other and improve the adhesion of the positive electrode active material and the collector. Specific examples thereof may include: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile (polyacrylonitrile), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, etc., and these substances can be used as a single or as a mixture of two or more. Relative to the total weight of the positive electrode active material layer, the content of the above-mentioned binder can be 0.1% by weight to 15% by weight.

[0155] In addition to using the above-mentioned positive electrode active material, the above-mentioned positive electrode can be prepared using a common positive electrode preparation method. Specifically, the above-mentioned positive electrode can be prepared by coating a positive electrode slurry composition prepared by dissolving or dispersing the above-mentioned positive electrode active material and a selective binder and a conductive material in a solvent onto a positive electrode collector, and then drying and rolling the obtained product.

[0156] The above-mentioned solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and these substances may be used alone as a substance, or as a mixture of two or more. Considering the coating thickness and preparation yield of the slurry, as long as the above-mentioned solvent can dissolve or disperse the above-mentioned positive electrode active material, conductive material and binder and has a viscosity sufficient to obtain excellent thickness uniformity when it is used to prepare the positive electrode coating thereafter, the amount of the solvent used is sufficient.

[0157] Furthermore, in another embodiment, the positive electrode may be prepared by casting the positive electrode slurry composition on a separate support, and then laminating a film obtained by peeling off the support on a positive electrode collector.

[0158] In addition, according to another aspect of the present invention, an electrochemical device including the positive electrode may be provided. The electrochemical device may be specifically a battery, a capacitor, etc., and more specifically, may be a lithium secondary battery.

[0159] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, and a separator and an electrolyte between the positive electrode and the negative electrode. Since the positive electrode is the same as the positive electrode described above, a detailed description will be omitted for convenience, and only the remaining components will be described in detail below.

[0160] The lithium secondary battery may further include a battery container for accommodating an electrode assembly including the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0161] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0162] The above-mentioned negative electrode collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and examples thereof may include: copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel, aluminum-cadmium alloy, etc., whose surface is treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode collector may generally have a thickness of 3 μm to 500 μm, or may increase the adhesion of the negative electrode active material by forming tiny concave-convex shapes on the surface of the collector, as with the positive electrode collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0163] The negative electrode active material layer can be prepared by coating a negative electrode slurry composition on the negative electrode current collector. The negative electrode slurry composition includes the negative electrode active material, a conductive material, and a selective binder as required.

[0164] The above-mentioned negative electrode active material can use a compound that can reversibly intercalate and deintercalate lithium. Specific examples thereof may include: carbon materials such as artificial graphite, natural graphite, graphitized carbon fiber and amorphous carbon; metal compounds that can be alloyed with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy or Al alloy; metal oxides that can be doped and dedoped with lithium such as SiO β(0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite comprising a metal compound and a carbon material such as a Si-C composite or a Sn-C composite, and any one of these substances or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, the carbon material can use both low-crystalline carbon and high-crystalline carbon. Low-crystalline carbon generally includes soft carbon and hard carbon, and high-crystalline carbon generally includes: amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, and high-temperature sintered carbon such as floating graphite (Kish graphite), pyrolytic carbon (pyrolytic carbon), mesophase pitch carbon fiber (mesophase pitch based carbon fiber), mesophase carbon microbeads (meso-carbon microbeads), mesophase pitch (Mesophase pitches) and petroleum or coal tar pitch derived coke (petroleum or coal tar pitch derived cokes).

[0165] The negative electrode active material may be included in an amount of 80 to 99 wt % based on the total weight of the negative electrode active material layer.

[0166] The binder is a component that helps to bind the conductive material, the active material and the current collector, and its content is generally 0.1 to 10% by weight based on the total weight of the negative electrode active material layer. Examples of the binder may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber and various copolymers thereof.

[0167] The above conductive material is a component for further improving the conductivity of the negative electrode active material, and the content of the conductive material can be 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. The above conductive material is not subject to any restrictions as long as it has conductivity and does not cause chemical changes in the battery, and conductive materials such as graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black can be used; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbons, aluminum or nickel powders; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.

[0168] In one embodiment, the negative electrode active material layer can be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing the negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition for forming a negative electrode on a separate carrier, and then laminating a film obtained by peeling off the carrier on the negative electrode collector.

[0169] Furthermore, in another embodiment, the negative electrode active material layer may be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing the negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition on a separate carrier and then laminating the film obtained by peeling off the carrier on the negative electrode collector.

[0170] On the other hand, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode, and provides a migration channel for lithium ions, and there is no particular limitation, as long as it is generally used as a separator in a lithium secondary battery. In particular, a separator with low resistance to electrolyte ion migration and excellent ability to contain electrolyte liquid moisture is preferred. Specifically, it is possible to use: a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure of more than two layers thereof. In addition, commonly used porous non-woven fabrics such as non-woven fabrics made of high melting point glass fibers or polyethylene terephthalate fibers can be used. In addition, in order to ensure heat resistance and mechanical strength, a coated separator comprising a ceramic component or a polymer material can also be used, and can be selectively used in a single-layer or multilayer structure.

[0171] In addition, the electrolyte used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc. that can be used in the preparation of lithium secondary batteries, but the present invention is not limited thereto.

[0172] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0173] The above-mentioned organic solvent can be used without particular limitation as long as it can function as a medium through which ions participating in the electrochemical reaction of the battery can migrate. Specific examples of the above-mentioned organic solvents may include: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene or fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methylethyl carbonate (MEC), ethylmethyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents such as ethanol or isopropanol; nitrile solvents such as R-CN (R is C2~C 20 Straight chain, branched or cyclic hydrocarbon group, and may contain double bond aromatic ring or ether bond); amide such as dimethylformamide; dioxolane such as 1,3-dioxolane; sulfolane, etc. Among them, carbonate solvents are preferred, and a mixture of cyclic carbonates (such as ethylene carbonate, propylene carbonate, etc.) with high ion conductivity and high dielectric constant that can enhance the charging and discharging performance of the battery and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, mixing cyclic carbonates and chain carbonates in a volume ratio of about 1:1 to 1:9 can produce excellent electrolyte performance.

[0174] The above-mentioned lithium salt can be used without particular limitation, as long as it is a compound capable of providing lithium ions in a lithium secondary battery. Specific examples of the above-mentioned lithium salts may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The lithium salt can be advantageously used in a concentration range of 0.1M to 2.0M. When the lithium salt concentration is included in the above range, the electrolyte has appropriate conductivity and viscosity, thereby being able to exhibit excellent electrolyte performance, and lithium ions can be effectively migrated.

[0175] In the above electrolyte, in order to increase the battery life property, inhibit the decline of battery capacity, improve the battery discharge capacity, etc., in addition to the above electrolyte forming components, one or more additives may be further included, including, for example: halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride. Wherein, relative to the total weight of the electrolyte, the content of the above additives can be 0.1% by weight to 5% by weight.

[0176] The lithium secondary battery containing the positive electrode active material according to the present invention as described above stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore used in the following fields: the field of portable devices such as mobile phones, laptop computers and digital cameras; and the field of electric vehicles such as hybrid electric vehicles (HEV) and the like.

[0177] The shape of the lithium secondary battery according to the present invention is not particularly limited, but may have a cylindrical, angular, pouch or coin shape using a can. And, preferably, the lithium secondary battery can be used as a battery cell for a power source of a small device, and can also be used as a unit battery of a medium and large battery module including a plurality of battery cells.

[0178] According to another aspect of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit battery and / or a battery pack including the same may be provided.

[0179] The battery module or the battery pack may be used in a power tool; an electric vehicle including an electric vehicle (EV), a hybrid vehicle (HEV) and a plug-in hybrid electric vehicle (PHEV); or a power source for one or more medium and large devices in a system for storing electricity.

[0180] Hereinafter, the present invention will be described in more detail with reference to Examples. However, it should be understood that these Examples are for illustrative purposes only and should not be construed as limiting the scope of the present invention.

[0181] Experimental example 1.

[0182] (1) Preparation of positive electrode active materials

[0183] Example 1

[0184] Spherical Ni was synthesized by co-precipitation method. 0.92 Co 0.08 (OH)2 hydroxide precursor. In a 90L reactor, a 1.5M metal aqueous solution is continuously added to the reactor at a rate of 3.0kg / hr and a 30 wt% ammonia solution is continuously added to the reactor at a rate of 0.2kg / hr for 20 to 40 hours. The above-mentioned metal aqueous solution is prepared by mixing NiSO4·7H2O and CoSO4·7H2O in a molar ratio of 92:8. In addition, in order to maintain the pH in the reactor at 11.5, a 20 wt% sodium hydroxide aqueous solution is supplied at a rate of 2kg / hr. At this time, the reactor temperature is maintained at 60°C, and N2 as an inert gas is added to the reactor to prevent the prepared precursor from being oxidized. After the synthesis stirring is completed, a filter press (F / P) equipment is used for washing and dehydration to obtain Ni 0.92 Co 0.08 (OH)2 hydroxide precursor.

[0185] The hydroxide precursor was mixed with LiOH as a raw material containing Li and Al2O3 as a raw material containing Al using a mixer, and the temperature was raised by 1°C per minute while maintaining an O2 atmosphere in a calcining furnace, maintained at 350°C for 4 hours, and the temperature was raised by 2°C per minute, maintained at a heat treatment temperature of 650°C for 10 hours, and then naturally cooled. It can be confirmed that the positive electrode active material prepared in Example 1 has Li 1.010 Ni 0.907 Co 0.079 Al 0.014The cross-sectional SEM image of the above positive electrode active material is shown in Figure 4 middle.

[0186] Example 2

[0187] The positive electrode active material obtained in Example 1 was mixed with the W-containing raw material (WO3) using a mixer, and then the temperature was raised by 2°C per minute while maintaining an O2 atmosphere in the same calcining furnace, and the heat treatment temperature was maintained at 600°C for 5 hours, and then naturally cooled. Then, the heat treatment and cooling were further performed once under the same conditions as above. It can be confirmed that the positive electrode active material prepared in Example 2 has Li 1.010 Ni 0.903 Co 0.078 Al 0.014 W 0.005 The cross-sectional SEM image of the above positive electrode active material is shown in Figure 5 middle.

[0188] Example 3

[0189] In addition to mixing a cobalt raw material (Co(OH)2) instead of a W-containing raw material (WO3), the positive electrode active material obtained in Example 3 has Li 1.010 Ni 0.903 Co 0.083 Al 0.014 The positive electrode active material was prepared in the same manner as in Example 2 except for the composition formula of O2. The cross-sectional SEM image of the positive electrode active material is shown in Figure 6 middle.

[0190] Example 4

[0191] In addition to mixing the cerium raw material (CeO2) instead of the W-containing raw material (WO3), the positive electrode active material obtained in Example 4 has Li 1.010 Ni 0.903 Co 0.078 Al 0.014 Ce 0.005 The positive electrode active material was prepared in the same manner as in Example 2 except for the composition formula of O2. The cross-sectional SEM image of the positive electrode active material is shown in Figure 7 middle.

[0192] Example 5

[0193] In addition to mixing the niobium raw material (Nb2O5) instead of the W-containing raw material (WO3), the positive electrode active material obtained in Example 5 has Li 1.010 Ni 0.903 Co 0.078 Al0.014 Nb 0.005 The positive electrode active material was prepared in the same manner as in Example 2 except for the composition formula of O2. The cross-sectional SEM image of the positive electrode active material is shown in Figure 8 middle.

[0194] Example 6

[0195] In addition to mixing the boron raw material (H3BO3) instead of the W-containing raw material (WO3), the positive electrode active material obtained in Example 6 has Li 1.010 Ni 0.903 Co 0.078 Al 0.014 B 0.005 The positive electrode active material was prepared in the same manner as in Example 2 except for the composition formula of O2. The cross-sectional SEM image of the positive electrode active material is shown in Fig. 9 middle.

[0196] Comparative Example 1

[0197] The positive electrode active material was prepared in the same manner as in Example 1 except that the metal aqueous solution was fed into the reactor at a rate of 6.0 kg / hr, the 30 wt% ammonia solution was fed at a rate of 0.4 kg / hr, and the 20% sodium hydroxide aqueous solution was fed at a rate of 4 kg / hr for 10 to 20 hours. The cross-sectional SEM image of the positive electrode active material is shown in FIG. Fig.10 middle.

[0198] Comparative Example 2

[0199] The positive electrode active material obtained in Comparative Example 1 was mixed with the W-containing raw material (WO3) using a mixer, and then maintained in the same calcining furnace with an O2 atmosphere and the temperature increased by 2°C per minute, maintained at a heat treatment temperature of 600°C for 5 hours, and then naturally cooled. Subsequently, heat treatment and cooling were further performed once under the same conditions as above. It can be confirmed that the positive electrode active material prepared in Comparative Example 2 has Li 1.010 Ni 0.903 Co 0.078 Al 0.014 W 0.005 The cross-sectional SEM image of the above positive electrode active material is shown in Fig.11 middle.

[0200] (2) SEM analysis of positive electrode active materials

[0201] The positive electrode active materials (secondary particles) of the examples and comparative examples were cross-sectioned using a cross-section polisher (accelerating voltage of 5.0 kV, grinding for 4 hours), and then FIB-SEM (Ga ion mode, accelerating voltage of 30.0 kV, probe current of 0.3 to 0.5 nA) images were obtained. The aspect ratios of the primary particles confirmed from the cross-section SEM images were measured and are shown in Tables 1 and Figures 5 to 11 middle.

[0202] Table 1

[0203] Classification <![CDATA[L1]]> <![CDATA[L2]]> <![CDATA[L3]]> <![CDATA[X1]]> <![CDATA[X2]]> <![CDATA[X3]]> <![CDATA[X2 / X1]]> Example 1 2.62 2.03 1.25 1.29 1.62 2.10 0.79 Example 2 2.66 2.08 1.38 1.28 1.51 1.93 0.85 Example 3 2.71 2.04 1.35 1.33 1.51 2.01 0.88 Example 4 2.72 2.05 1.16 1.33 1.77 2.34 0.75 Example 5 2.42 2.07 1.29 1.17 1.60 1.88 0.73 Example 6 2.62 1.89 1.21 1.39 1.56 2.17 0.89 Comparative Example 1 1.68 1.6 1.33 1.05 1.20 1.26 0.87 Comparative Example 2 1.65 1.78 1.23 0.93 1.45 1.34 0.64

[0204] The average aspect ratio L1 shown in Table 1 above is the average value of the aspect ratios measured by 35 to 50 primary particles in the first region at a distance of 2 / 3R to R from the center of the secondary particle, the average aspect ratio L2 is the average value of the aspect ratios measured by 20 to 30 primary particles in the second region at a distance of 1 / 3R to 2 / 3R from the center of the secondary particle, and the average aspect ratio L3 is the average value of the aspect ratios measured by 9 to 15 primary particles in the third region at a distance of 0 to 1 / 3R from the center of the secondary particle. In addition, X1 is L1 / L2, X2 is L2 / L3, and X3 is L1 / L3.

[0205] (3) Density determination of positive electrode active materials

[0206] When a positive electrode for a lithium secondary battery is prepared using a positive electrode active material, a slurry containing the positive electrode active material is coated on a positive electrode collector, and then a drying and rolling (pressing) process is performed. At this time, when rolling is performed under high pressure, the particles of the positive electrode active material coated on the positive electrode collector collapse, so that the performance of the positive electrode active material may be deteriorated.

[0207] In this experimental example, in order to confirm the strength change of the positive electrode active material according to the composition of the aggregates of multiple secondary particles contained in the positive electrode active material, the positive electrode active materials prepared according to the embodiment and the comparative example were prepared respectively, and then the change rates of d(10), d(50) and d(90) of the particle size distribution before pressing, after pressing at 2.5 tons, after pressing at 4.5 tons and after pressing at 6 tons were measured.

[0208] The measurement results of the change rates of d(10), d(50) and d(90) of the particle size distribution after pressing according to the various pressure conditions are shown in Tables 2 to 4 below.

[0209] Table 2

[0210]

[0211] Table 3

[0212]

[0213] Table 4

[0214]

[0215] Referring to Tables 2 to 4 above, the change rates of d(10), d(50) and d(90) of the particle size distribution before / after pressing of the secondary particles included in the positive electrode active material prepared according to Example 2 are smaller than those of the positive electrode active material prepared according to Comparative Example 1.

[0216] Experimental example 2.

[0217] (1) Preparation of lithium secondary batteries

[0218] The positive electrode slurry was prepared by dispersing 94 wt % of each positive electrode active material prepared according to the examples and comparative examples, 3 wt % of carbon black and 3 wt % of PVDF binder in 30 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was coated on an aluminum (Al) film as a positive electrode collector having a thickness of 15 μm, dried and roll pressed to prepare a positive electrode. The loading level of the positive electrode was 10 mg / cm 2 , the electrode density is 3.2g / cm 3 .

[0219] Metallic lithium was used as a counter electrode of the positive electrode, and an electrolyte was prepared by adding 1.15 M LiPF6 to a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 2:4:4.

[0220] A lithium secondary battery (button battery) was prepared by interposing a separator made of a porous polyethylene (PE) film between the positive electrode and the negative electrode to form a battery assembly, and injecting the above electrolyte.

[0221] (2) Evaluation of capacity characteristics of lithium secondary batteries

[0222] The lithium secondary battery prepared by the method described above was subjected to a charge and discharge experiment using an electrochemical analyzer (Toyo, Toscat-3100) at 25°C, a voltage range of 3.0V to 4.25V, and a discharge rate of 0.5C to 4.0C to measure the initial charge capacity, initial discharge capacity, initial reversible efficiency, and rate characteristics. The measured battery capacity and charge / discharge efficiency are shown in Table 5 below.

[0223] Table 5

[0224] Classification Charging capacity (mAh / g) Discharge capacity (mAh / g) Charge and discharge efficiency (%) 4.0C / 0.2C rate characteristics (%) Example 1 233.6 212.9 91.2 76.6 Example 2 231.9 211.5 91.2 79.2 Example 3 231.4 209.2 90.4 78.9 Example 4 232.4 209.6 90.2 78.6 Example 5 232.0 207.9 89.6 78.7 Example 6 232.6 208.9 89.8 79.0 Comparative Example 1 233.8 211.4 90.4 72.0 Comparative Example 2 233.4 212.4 91.0 73.2

[0225] Referring to the results in Table 5 above, the initial capacity and charge and discharge efficiency of the lithium secondary battery including the positive electrode using the positive electrode active material according to the embodiment and the comparative example are similar, but in the case of the lithium secondary battery including the positive electrode using the positive electrode active material according to the embodiment, compared with the comparative example, the high rate characteristics can be confirmed from the results of the charge and discharge experiment with a discharge rate of 0.5C to 4.0C.

[0226] (3) Evaluation of lithium secondary battery stability

[0227] The lithium secondary battery (button cell) prepared above was charged and discharged 100 times at a constant current (CC) of 1 C at a temperature of 25° C. within a driving voltage range of 3.0 to 4.25. Thus, after charging and discharging 100 times at normal temperature, the cycle capacity retention, which is the ratio of the discharge capacity at the 100th cycle to the initial capacity, was measured.

[0228] Furthermore, the resistance variation range of the lithium secondary battery was confirmed by measuring the resistance before and after the life of the battery.

[0229] The above measurement results are shown in Table 6 below.

[0230] Table 6

[0231] Classification Capacity retention rate (%) Resistance before life (Ω) Resistance after life (Ω) Example 1 85.1 4.2 35.6 Example 2 88.9 4.0 19.9 Example 3 90.1 4.7 29.6 Example 4 90.2 6.0 24.2 Example 5 90.1 5.1 20.7 Example 6 88.8 4.2 18.4 Comparative Example 1 75.8 4.1 44.0 Comparative Example 2 77.3 3.9 40.9

[0232] Referring to the results in Table 6 above, it can be confirmed that the capacity retention rate of the lithium secondary battery using the positive electrode active material according to the embodiment of the present invention is better than that of the lithium secondary battery using the positive electrode active material according to the comparative example, and the resistance change range before and after high temperature storage is also smaller.

[0233] In addition, referring to the before (a) / after (b) cross-sectional SEM photographs of the life of the positive electrode active material according to Example 1 Fig.12 and cross-sectional SEM images of the positive electrode active material before (a) and after (b) the life of the positive electrode active material according to Comparative Example 1 Fig.13It can be confirmed that the positive electrode active material according to Example 1 has fewer cracks after life than the positive electrode active material according to Comparative Example 1. This result is because the aspect ratio gradient presented by the primary particles contained in the positive electrode active material according to Example 1 has a directionality that increases within a specific range, thereby effectively reducing the partial strain caused by the asymmetric volume expansion of the above-mentioned positive electrode active material during the charge and discharge of the lithium secondary battery. Through this strain reduction, the generation of cracks after the life of the above-mentioned positive electrode active material may be reduced, which can help to improve the life and stability of the lithium secondary battery.

[0234] Although the embodiments of the present invention are described above, those skilled in the art will understand that various modifications and changes can be made to the present invention by adding, modifying, deleting, increasing, etc., without departing from the scope of the idea of ​​the present invention as described in the claims, and these also fall within the scope of the rights of the present invention.

Claims

1. A positive electrode active material, wherein include: Primary particles capable of occluding and releasing lithium; and Secondary particles, formed by the aggregation of the above primary particles, The primary particles and the secondary particles satisfy the following formula 2: [Formula 2] 1.35≤X2≤1.95 In the above formula 2, X2 is L2 / L3, When the distance from the center of the secondary particle to the surface of the secondary particle is R, The above L2 represents the average aspect ratio of the above primary particles present in the second region having a distance of 1 / 3R to 2 / 3R from the center of the above secondary particles, L3 represents an average aspect ratio of the primary particles present in a third region having a distance from 0 to 1 / 3R from the center of the secondary particles.

2. The positive electrode active material according to claim 1, wherein The primary particles and the secondary particles satisfy the following formula 1: [Formula 1] 1.15≤X1≤1.75 In the above formula 1, X1 is L1 / L2, The L1 represents an average aspect ratio of the primary particles present in a first region ranging from 2 / 3R to R from the center of the secondary particles.

3. The positive electrode active material according to claim 2, wherein The primary particles and the secondary particles satisfy the following formula 3: [Formula 3] X1 / X2≥0.

70.

4. The positive electrode active material according to claim 2, wherein The above-mentioned L1 is 2.13 or more and 3.94 or less.

5. The positive electrode active material according to claim 1, wherein The primary particles and the secondary particles satisfy the following formula 4: [Formula 4] X3≥1.70 In the above formula 4, X3 is L1 / L3, The L1 represents an average aspect ratio of the primary particles present in a first region ranging from 2 / 3R to R from the center of the secondary particles.

6. The positive electrode active material according to claim 5, wherein The above X3 is greater than or equal to 1.76 and less than or equal to 3.

23.

7. The positive electrode active material according to claim 1, wherein The above L3 is 1.09 or more.

8. The positive electrode active material according to claim 1, wherein The primary particle has an aspect ratio that continuously increases from a center portion of the secondary particle toward a surface portion of the secondary particle.

9. The positive electrode active material according to claim 1, wherein The primary particle has a rod shape radiating from a center portion of the secondary particle toward a surface portion of the secondary particle, and a major axis direction of the primary particle has a directivity toward a center portion of the secondary particle.

10. The positive electrode active material according to claim 1, wherein The angle formed by the lithium ion diffusion path in the primary particle and the long axis direction of the primary particle is ±40°.

11. The positive electrode active material according to claim 10, wherein The lithium ion diffusion path is formed to have an angle within ±40° with respect to a direction extending from a center portion of the secondary particle to a surface portion of the secondary particle.

12. The positive electrode active material according to claim 1, wherein The primary particle is represented by the following chemical formula 1: [Chemical formula 1] The w Nor 1-(x+y+z) Co x M1 y M2 z O2 in, M1 is at least one selected from Mn and Al, M2 is at least one selected from the group consisting of Mn, B, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements. 0.5≤w≤1.5, 0.01≤x≤0.50, 0.01≤y≤0.20, 0.001≤z≤0.

20.

13. The positive electrode active material according to claim 1, wherein The positive electrode active material includes a coating layer, the coating layer covers at least a portion of a region selected from the interface between the primary particles and the surface of the secondary particles, The coating layer includes at least one oxide represented by the following chemical formula 2: [Chemical formula 2] Read a M3 b Oh c Among them, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, and 0≤a≤10, 0≤b≤8, 2≤c≤13.

14. A lithium secondary battery, wherein: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 13 is used.

Citation Information

Patent Citations

  • Cathode active material, method for preparing the same, and lithium secondary batteries comprising the same

    KR1020150069334A