Conductive agent, slurry for forming electrode including the conductive agent, electrode, and lithium secondary battery manufacturing using the electrode

By optimizing the preparation of graphene sheets, ensuring its high dispersion and conductivity in the electrodes of lithium secondary battery, the problems of deformation of electrode active materials and poor dispersion of conductive agents are solved, and the high efficiency and long life of the battery are achieved.

CN118943370APending Publication Date: 2024-11-12LG ENERGY SOLUTION LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062602.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-01-26
Filing Date
2019-01-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing lithium secondary battery electrode active materials are prone to deform during rolling, resulting in a decrease in electrolyte permeability. Traditional conductive agents such as carbon nanotubes are difficult to commercially apply, due to strong aggregation and poor dispersion.

Method used

Using graphene sheets determined by X-ray diffraction analysis as conductive agent to ensure their maximum peak value in the range of 2θ of 24.5° to 26° and optimized aspect ratio, combined with Raman spectroscopy analysis to ensure high crystallinity and dispersion, prepare A slurry with high dispersion and high conductivity is produced for the production of electrodes.

Benefits of technology

The conductivity of the battery and the adhesion of the electrodes are significantly improved, the cycle life of the battery is extended, and the capacity retention rate is maintained, while reducing the resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943370A_ABST
    Figure CN118943370A_ABST
Patent Text Reader

Abstract

The present invention provides a conductive agent, a slurry for forming an electrode, a slurry including the conductive agent, an electrode manufactured using the conductive agent, and a lithium secondary battery, in which the conductive agent includes graphene flakes, the maximum peak value of the graphene flakes is observed in the range of 2theta being 24.5-26 degrees in a data map obtained by X-ray diffraction (XRD) analysis, and the maximum peak value of the graphene flakes is observed in the range of 2theta being 24.5-26 degrees in the data map obtained by X-ray diffraction (XRD) analysis. Wherein an aspect ratio of an average lateral dimension of a surface of the graphene flakes to an average thickness of the graphene flakes in a direction perpendicular to the surface of the graphene flakes is 500 to 50,000.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a Chinese patent application filed on January 28, 2019, with application number "201980006894.6" and invention name "Conductive agent, slurry for forming an electrode including the conductive agent, electrode, and lithium secondary battery manufactured using the electrode".

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of Korean Patent Application No. 2018-0009777 filed in the Korean Intellectual Property Office on January 26, 2018, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0004] The present invention relates to a conductive agent and a lithium secondary battery manufactured using the conductive agent, and more specifically, to a conductive agent including graphene flakes with excellent conductivity, a slurry for forming an electrode, a slurry including the conductive agent, an electrode, and a lithium secondary battery manufactured using the electrode. Background Art

[0005] With the increase of technology development and demand for mobile devices, the demand for secondary batteries as energy sources has increased rapidly. Among these secondary batteries, lithium secondary batteries with high energy density and voltage, long cycle life and low self-discharge rate have been commercialized and widely used. In addition, as the electrode of this high-capacity lithium secondary battery, the method of manufacturing a high-density electrode with higher energy density per unit volume has been actively studied.

[0006] Generally, high-density electrodes are prepared by applying a slurry including electrode active material particles with a size of several μm to several tens of μm on a substrate, followed by drying and rolling to form a mixture layer. However, the electrode active material particles may be deformed by the high pressure pressing applied in the rolling step, and the space between the particles may also be reduced, and therefore, the permeability of the electrolyte into the mixture layer may be deteriorated.

[0007] In order to solve these problems, in the process of forming the mixture layer of the electrode, in addition to the electrode active material particles, a conductive agent with excellent strength and conductivity is used. When the conductive agent is used to make the electrode, the conductive agent is dispersed in the compressed electrode active material, and the pores between the active material particles are maintained, thereby improving the permeability of the electrolyte. In addition, the conductive agent has high conductivity, so the resistance of the battery can be reduced. In recent years, research using carbon nanotubes (CNT), graphene, carbon black and the like as conductive agents is underway.

[0008] Carbon nanotubes, as a type of fine carbon fiber, are tubular carbon with a diameter of less than 1 μm. Carbon nanotubes have high electrical conductivity, tensile strength, and heat resistance due to their specific structure, so their uses are increasing. However, carbon nanotubes easily aggregate due to the strong van der Waals attraction acting between them, and thus have low solubility and dispersibility. In order to overcome this limitation, methods such as introducing functional groups into the surface of carbon nanotubes have been designed. However, it is still difficult to commercialize carbon nanotubes as conductive agents due to the possibility of side reactions.

[0009] Graphene is a semi-metallic material with a layered structure, which is formed in which carbon atoms are connected into a hexagonal arrangement through two-dimensional sp2 bonds. Graphene not only has excellent electrical conductivity, but also has structural and chemical stability and excellent thermal conductivity. In addition, graphene is composed of carbon, which is a relatively light element, so it is easy to process one-dimensional or two-dimensional nano patterns. Most importantly, graphene sheets are cheap, so they have excellent price competitiveness compared to traditional nanomaterials.

[0010] Due to such excellent characteristics of graphene, various methods for more efficiently mass-producing graphene from carbon-based materials such as graphite have been proposed or studied.

[0011] For example, a method for preparing graphene by pulverizing graphite together with a dispersant has been proposed, but graphite is excessively pulverized, so it is difficult to obtain graphene having a desired size and shape, and the types of dispersants that can be used are limited.

[0012] Therefore, there is a need to develop graphene having electrical conductivity higher than a predetermined level while having high dispersibility and a conductive material using the graphene.

[0013] (Patent Document 1) Korean Patent Unexamined Publication No. 10-2011-0077606 Summary of the invention

[0014] Technical issues

[0015] One aspect of the present invention provides a conductive agent including graphene flakes having excellent conductivity and significantly improved dispersibility, a slurry for forming an electrode, a slurry including the conductive agent, an electrode, and a lithium secondary battery manufactured using the electrode.

[0016] Technical Solution

[0017] According to one aspect of the present invention, there is provided a conductive agent comprising graphene flakes, wherein in a data graph obtained by X-ray diffraction (XRD) analysis, a maximum peak of the graphene flakes is observed in the range of 2θ of 24.5° to 26°, wherein an aspect ratio of an average lateral dimension of a surface of the graphene flakes to an average thickness of the graphene flakes in a direction perpendicular to the surface of the graphene flakes is 500 to 50,000.

[0018] At this time, the average thickness of the graphene sheet may be 1 nm to 10 nm.

[0019] At the same time, the graphene flakes are at 1360±50cm -1 The maximum peak intensity of the D band at 1580±50cm -1 An average ratio of the maximum peak intensities of the G band at , which is obtained by Raman spectroscopy using a laser having a wavelength of 532 nm, may be 0.06 to 0.5.

[0020] According to another aspect of the present invention, a slurry for forming an electrode, an electrode manufactured using the slurry, and a lithium secondary battery are provided, wherein the slurry includes an electrode active material, a binder, a dispersion medium, and the conductive agent.

[0021] Beneficial Effects

[0022] The conductive agent according to the present invention includes graphene flakes, and in the data graph obtained by X-ray diffraction (XRD) analysis, the maximum peak of the graphene flakes is observed in the range of 2θ of 24.5° to 26°, so the exfoliation and crystallinity are excellent. In addition, the conductive agent includes graphene flakes that meet an appropriate level of aspect ratio (Aspect ratio), which is the ratio of the lateral dimension of the surface of the graphene flakes to the thickness of the graphene flakes in the direction perpendicular to the surface of the graphene flakes, so the conductive agent has high dispersibility to be uniformly placed in the electrode. As a result, the conductivity in the battery can be improved.

[0023] Furthermore, even when a small amount of a slurry for forming an electrode including the conductive agent is used, dispersibility and viscosity are high while conductivity is maintained above a predetermined level, so that electrode adhesion can also be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a data diagram obtained by X-ray diffraction (XRD) of the graphene sheets produced in Example 1 and Comparative Examples 1 and 2 of the present invention.

[0025] Figure 2 It is a data graph obtained by XPS analysis of the graphene flakes in Example 1 and Comparative Examples 1 and 2 of the present invention.

[0026] Figure 3 : is a graph showing changes in powder resistance according to compaction density of slurries for forming electrodes of Examples 2-4 and Comparative Examples 3-6.

[0027] Figure 4 is a graph showing the results of measuring adhesion when the slurries for forming an electrode according to Examples 2-4 and Comparative Examples 3-6 were peeled at 90°.

[0028] Figure 5 : is a graph showing the capacity retention rate (capacity retention %) of the secondary battery manufactured according to the manufacturing example of the present invention, the capacity retention rate being measured according to the cycle at 45° C.

[0029] Figure 6 is a graph showing the capacity retention % and resistance increase (%) of the secondary battery manufactured according to the manufacturing example of the present invention, the capacity retention % and the resistance increase (%) being measured at 60° C. on a weekly basis. DETAILED DESCRIPTION

[0030] Hereinafter, the present invention will be described in more detail to facilitate understanding of the present invention.

[0031] It will be understood that the words or terms used in this application should not be interpreted as the meanings defined in commonly used dictionaries. It will be further understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best explain the present invention, these words or terms should be interpreted as having a meaning consistent with the meanings in the context of the technical concept of the present invention and the related technology.

[0032] The terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting of the present invention. Terms in the singular may include plural forms unless the context clearly indicates otherwise.

[0033] It will be further understood that when the terms "include", "comprises" or "has" are used in this specification, they specifically specify the existence of the features, numbers, steps, elements or combinations thereof, but do not exclude the existence or addition of one or more other features, numbers, steps, elements or combinations thereof.

[0034] Conductive agent

[0035] The conductive agent according to the present invention includes graphene flakes, and in a data graph obtained by X-ray diffraction (XRD) analysis, a maximum peak of the graphene flakes is observed in the range of 2θ of 24.5° to 26°, wherein the aspect ratio of the average lateral dimension of the surface of the graphene flakes to the average thickness of the graphene flakes in a direction perpendicular to the surface of the graphene flakes is 500 to 50,000.

[0036] Generally, an electrode for a secondary battery including a conductive agent is prepared by preparing a slurry for forming an electrode including the conductive agent, applying the slurry for forming an electrode on a substrate, and then drying and rolling. Therefore, only when the conductive agent is uniformly dispersed in the slurry for forming an electrode and the slurry maintains a predetermined viscosity level, the conductive agent can be uniformly dispersed on the surface of the substrate to improve conductivity.

[0037] However, in the case of graphene generally used as a conductive agent, exfoliation into a single layer cannot be properly achieved, so that the dispersibility and viscosity of a slurry for forming an electrode including the conductive agent are reduced.

[0038] Therefore, in the present invention, a graphene sheet in which a maximum peak is observed in a range of 2θ of 24.5° to 26° in a data graph obtained by X-ray diffraction (XRD) analysis is used as the conductive agent of the present invention (see Figure 1 ).

[0039] X-ray diffraction (XRD) analysis can be derived from the results measured by using a thin film X-ray diffraction analyzer (Rigaku Ultima IV). It can be measured by scanning at intervals of 0.2° with an applied voltage of 40 kV, an applied current of 40 mA, and a 2θ measurement range of 24° to 28°. At this time, a 2 mm variable divergence slit can be used as a slit.

[0040] Reference Figure 1 When 2θ is in the range of 24.5° to 28°, more preferably in the range of 25° to 26°, the graphene flakes according to the present invention show a broad maximum peak. In this specification, the maximum peak refers to a peak with the highest intensity value within the range of 2θ.

[0041] The graphene flakes of the present invention have a maximum peak value in the above 2θ range because when a single-layer film that has been peeled off from graphite is re-laminated, the interlayer spacing between the re-laminated single-layer films increases due to the dispersant adsorbed between the layers or due to the newly formed pore structure. Therefore, it has been confirmed that the graphene flakes according to the present invention have been fully peeled off and formed in a single-layer form.

[0042] Meanwhile, it is observed that the insufficiently exfoliated graphene flakes have a maximum peak at around 26.5°, as in the case of graphite before exfoliation.

[0043] Furthermore, in the data graph obtained by an X-ray diffraction analyzer (Rigaku Ultima IV), the full width at half maximum (FWHM) of the graphene flakes is 0.5° to 5°, and the full width at half maximum (FWHM) of the maximum peak is in the range of 24.5° to 26° in 2θ.

[0044] In the present invention, the full width at half maximum (FWHM) is the value of the peak width at the 1 / 2 position of the maximum peak in the range of 2θ of 24.5° to 26° obtained by X-ray diffraction of a graphene sheet. Even if a film peeled off from graphite is re-laminated during the preparation of a graphene sheet, if the interlayer spacing between the re-laminated films is uneven, the corresponding full width at half maximum value increases. At this time, when the film is re-laminated with an uneven interlayer spacing, the degree of peeling is further increased. Therefore, it is desired that the full width at half maximum value is 0.5° to 5°.

[0045] At the same time, the aspect ratio of the average lateral size of the surface of the graphene flakes to the average thickness of the graphene flakes in the direction perpendicular to the surface of the graphene flakes may be 500 to 50,000, preferably 1,000 to 50,000. This is because, when the graphene flakes exist in the form of plates, the average lateral size of the formed surface is 5 μm to 50 μm, and the average thickness of the graphene flakes is 1 nm to 10 nm.

[0046] At this time, the lateral size and thickness of the graphene flakes can be measured with an atomic force microscope (AFM), and the average lateral size and average thickness can be statistically calculated by direct measurement of the images obtained during the AFM measurement. For example, hundreds or thousands of graphene flakes are observed, and then the lateral size and thickness of the observed graphene flakes are measured respectively. Afterwards, some graphene flakes at the top and some graphene flakes at the bottom are collected according to the order of their lengths. Afterwards, the average lateral size and average thickness of the graphene flakes can be calculated by averaging the lateral size and thickness of the collected graphene flakes, respectively.

[0047] When the aspect ratio is less than 500, the exfoliation of the graphene sheet is not very good, so it may be difficult to form a conductive network that is minimum for the expression of conductivity. When it is greater than 50,000, the diffusion resistance of the electrolytic ions may increase because the area of ​​the graphene sheet is too large for the electrolytic ions to approach the active material.

[0048] In addition, the graphene flakes of the present invention may have an average ratio of 0.06 to 0.5, that is, at 1360±50cm -1 The maximum peak intensity of the D band at 1580±50cm -1 The average ratio of the maximum peak intensity of the G band at , which is obtained by Raman spectroscopy using laser light with a wavelength of 532 nm, is preferably 0.06 to 0.4.

[0049] The Raman spectroscopy analysis method is a method for analyzing the crystallinity of graphene flakes and is a useful method for analyzing the surface state of graphene flakes. In Raman spectroscopy, the wave number 1580±50cm -1 The peak in the vicinity is called the G peak, which represents the sp 2 At the same time, in the Raman spectrum, the wave number is 1360±50cm -1 The peak existing in the region near is called D peak, which represents the sp 3 The peak of the D peak increases when the sp2 bonds with the hexagonal grid surface on the graphite layer are broken and sp3 bonds are formed. Therefore, when the peak at 1360 ± 50 cm -1 The maximum peak intensity of the D band at 1580±50cm -1 When the ratio of the maximum peak intensity of the G band at is within the above range, a significantly exfoliated graphene sheet can be provided while minimizing damage to its intrinsic crystallinity.

[0050] In addition, the oxygen content of the graphene flakes may be 5 to 10 atom%, preferably 5.5 to 10 atom%, and more preferably 6 to 10 atom%. The oxygen content in the graphene flakes is measured by X-ray photoelectron spectroscopy (XPS). The graphene flakes contain oxygen because a surfactant including an oxygen functional group is adsorbed on the surface of the graphene flakes when the graphene flakes are peeled off from graphite. In addition, when the oxygen contained in the graphene flakes is within the above range, electrical repulsion is generated, so that the graphene flakes can be further uniformly dispersed in the slurry for forming the electrode.

[0051] The conductive agent according to the present invention may further include other conductive materials in addition to graphene flakes. For example, conductive materials such as graphite, carbon-based materials such as carbon black, carbon nanotubes, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black may be used; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride powders, aluminum powders, and nickel powders; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or polyphenylene derivatives. Specific examples of commercially available conductive materials may include acetylene black series (products of Chevron Chemical Company), denka black (products of Denka Singapore Private Limited, Gulf Oil Company, etc.), ketjen black, EC series (products of Armak Company), Vulcan XC-72 (products of Cabot Company), and Super P (products of Timcal company).

[0052] Hereinafter, a method for preparing a conductive agent will be described. The conductive agent can be prepared by the following steps: (1) preparing an ion solution; (2) preparing a graphite mixed solution; and (3) obtaining a graphene sheet. Hereinafter, each step will be described.

[0053] (1) Preparation of ionic solution

[0054] The ionic solution can be prepared by mixing an organic solvent, naphthalene, and potassium (K).

[0055] Naphthalene and potassium (K) are used to form a potassium (K) complex. Electrons of potassium (K) are transferred to naphthalene to be ionized, and then coordinated with organic solvent molecules to form a potassium (K) complex. Potassium (K) may be included in the ionic solution at a concentration of 0.1M to 2M, preferably 1M to 2M, to form a complex. When potassium (K) is included within the above range, an insertion reaction of the potassium complex into the middle layer of the mixed graphite may be performed.

[0056] The organic solvent is used to disperse the potassium (K) complex and graphite added to the ionic solution, and is also used as a component of the potassium (K) complex. Any organic solvent can be used without limitation, as long as it does not cause side reactions with the potassium (K) complex and graphite. Preferably, an aprotic organic solvent can be used.

[0057] For example, the organic solvent may include tetrahydrofuran (THF), acetonitrile, dimethylformamide (DMF), dimethylacetamide (DMA), N-methyl-2-pyrrolidone (NMP), methyl ethyl ketone (MEK), pyridine, quinoline, xylene, chloroform, ammonia, toluene, benzene, dimethylsulfoxide (DMSO), propylene carbonate and the like. The above materials may be used alone or in combination. More preferably, the organic solvent may include tetrahydrofuran.

[0058] (2) Preparation of graphite mixed solution

[0059] The graphite mixed solution is prepared by mixing graphite in the ion solution prepared in step (1).

[0060] More specifically, an ion solution is prepared in a glove box of an argon (Ar) atmosphere at a temperature of 25° C. to 40° C., and then graphite is added to the ion solution at a concentration of 30 mg / ml to 150 mg / ml (preferably 35 mg / ml to 150 mg / ml, more preferably 35 mg / ml to 145 mg / ml).

[0061] At this time, natural graphite or artificial graphite can be used as graphite. Graphite can be used in a processed form such as powder, block, or foil. Considering the solubility and viscosity in the ion solution, graphite is added at a concentration within the above range. The concentration of graphite to be added may vary depending on the test conditions.

[0062] When graphite is added to an ion solution, the potassium (K) complex dissolved in the ion solution is inserted between graphite layers, thereby weakening the van der Waals attraction, which can improve the exfoliation of graphite.

[0063] (3) Obtaining graphene sheets

[0064] The graphite mixed solution may be mixed to obtain graphene flakes. The mixing includes processes such as stirring, sonication dispersion, and centrifugation.

[0065] More specifically, the graphene flakes can be obtained through the following steps.

[0066] First, the graphite mixed solution is stirred in a glove box for 5 to 10 hours. Then, the solvent except the solid component (such as graphite) with potassium complex inserted between its layers is removed from the ionic solution, and a non-polar or low-polar solvent capable of dissolving naphthalene can be used for washing. For example, tetrahydrofuran (THF) and cyclohexane (cyclohexane) can be used, and cyclohexane is preferably used to wash the solid component.

[0067] The washed solid component and polyvinylpyrrolidone (PVP) were mixed in a dimethyl sulfoxide (DMSO) solvent, and using a water tank type ultrasonic device, graphite was exfoliated into a single layer structure through sonication dispersion for 10 to 60 minutes.

[0068] In order to separate only the exfoliated single layer structure, centrifugation was performed at 2000 rpm for 30 minutes to 1 hour using a centrifugal separator (Hanil Science Combi-514R). After centrifugation, only the upper layer was separated.

[0069] The material in the separated upper layer portion was centrifuged again at 10000 rpm for 30 minutes to 1 hour using a centrifugal separator (Hanil Science Combi-514R). Thereafter, the residual solvent remaining in the upper layer portion was removed to obtain a graphene sheet.

[0070] Meanwhile, graphene flakes are injected into N-methyl-2-pyrrolidone (NMP) solvent to a concentration of 0.5 mg / ml to 5 mg / ml, and graphene flakes dispersed in the solvent are prepared by performing sonication dispersion using a water tank type ultrasonic device for 5 to 20 minutes.

[0071] Slurry for forming electrodes

[0072] Hereinafter, a slurry for forming an electrode will be described. The slurry for forming an electrode includes an electrode active material, a binder, a dispersion medium, and the conductive agent. Since the conductive agent is the same as the above conductive agent, its detailed description will be omitted.

[0073] Meanwhile, based on 100 parts by weight of the solid components other than the dispersion medium in the slurry for forming the electrode, the conductive agent can be included in an amount of 0.05 to 2.0 parts by weight, preferably 0.3 to 1.5 parts by weight, and more preferably 0.5 to 1.3 parts by weight. When the conductive agent is included within the above range, the conductivity can be improved and the viscosity can be maintained above a predetermined level.

[0074] In the slurry for forming the electrode, the electrode active material can be any electrode active material commonly used as a positive electrode active material or a negative electrode active material of a secondary battery.

[0075] Specifically, when the slurry for forming the electrode is for forming a positive electrode, the electrode active material is a compound capable of reversibly intercalating and deintercalating lithium, and specifically may include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum, and lithium.

[0076] More specifically, the lithium composite metal oxide can be: lithium manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.); lithium cobalt-based oxides (e.g., LiCoO2, etc.); lithium nickel-based oxides (e.g., LiNiO2, etc.); lithium nickel manganese-based oxides (e.g., LiNi 1-Y1 Mn Y1 O2 (where 0 < Y1 < 1), LiMn 2-Z1 Ni Z1 O4 (where 0 < Z1 < 2), etc.); lithium nickel cobalt-based oxides (e.g., LiNi 1-Y2 Co Y2 O2 (where 0 < Y2 < 1)); lithium manganese cobalt-based oxides (e.g., LiCo 1-Y3 Mn Y3 O2 (where 0 < Y3 < 1), LiMn 2- Z2 Co Z2 O4 (where 0 < Z2 < 2), etc.); lithium nickel manganese cobalt-based oxides (e.g., Li(Ni p1 Co q1 Mn r1 )O2 (where 0 < p1 < 1, 0 < q1 < 1, 0 < r1 < 1, p1 + q1 + r1 = 1) or Li(Ni p2 Co q2 Mn r2 )O4 (where 0 < p2 < 2, 0 < q2 < 2, 0 < r2 < 2, p2 + q2 + r2 = 2), etc.); or lithium nickel cobalt transition metal (M) oxides (e.g., Li(Ni p3 Co q3 Mn r3 M s1)O2, where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p3, q3, r3, and s1 are each the atomic fraction of an independent element, where 0 < p3 < 1, 0 < q3 < 1, 0 < r3 < 1, 0 < s1 < 1, and p3 + q3 + r3 + s1 = 1), etc.; and analogs, and may include any one of them or a mixture of two or more of them.

[0077] Among them, since the capacity characteristics and stability of the battery can be improved, the lithium composite metal oxide can be LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (e.g., LiNi 0.8 Co 0.15 Al 0.05 O2, etc.), and analogs. When considering the significant improvement effect according to the control of the type and content ratio of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide can be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, and analogs, and any one of them or a mixture of two or more of them can be used.

[0078] When the slurry for forming the electrode is for forming the negative electrode, the electrode active material is a compound capable of reversibly inserting and extracting lithium, and can be the following negative electrode active materials: composite materials including carbonaceous materials, such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metal compounds that can alloy with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metal oxides that can be doped and undoped with lithium, such as SiO x(0 < x ≤ 2), SnO₂, vanadium oxides, lithium titanium oxides, and lithium vanadium oxides; or composite materials including metal compounds and carbonaceous materials, such as Si-C composite materials or Sn-C composite materials, and any one of them or a mixture of two or more of them can be used. In addition, a thin film of metallic lithium can be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon can be used as the carbon material. Typical examples of low-crystalline carbon can include soft carbon and hard carbon, and typical examples of high-crystalline carbon can include irregular, planar, flaky, spherical, or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature sintered carbon, such as petroleum or coal tar pitch derived cokes.

[0079] Meanwhile, based on 100 parts by weight of the solid components other than the dispersion medium in the slurry for forming the electrode, the electrode active material can be included in an amount of 95.5 parts by weight to 99 parts by weight, preferably 96 parts by weight to 98.7 parts by weight, more preferably 97 parts by weight to 98 parts by weight. When the electrode active material is included within the above range, a capacity at a predetermined level or higher can be maintained, and the binder and the conductive agent are included above a predetermined level, so that the adhesion to the electrode current collector and the conductivity can be improved.

[0080] The binder is a component that helps the binding between the electrode active material, the conductive agent, and the current collector. Examples of the binder can include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, various copolymers thereof, and the like.

[0081] Generally, based on 100 parts by weight of the solid components other than the dispersion medium in the slurry for forming the electrode, the binder can be included in an amount of 0.8 parts by weight to 3.0 parts by weight, preferably 1.0 parts by weight to 2.5 parts by weight, more preferably 1.0 parts by weight to 2.2 parts by weight. When the binder is included within the above range, the adhesion between the electrode active materials and the adhesion between the electrode active material and the conductive agent can be improved. In addition, the adhesion to the current collector can be improved.

[0082] Dispersion medium can be a solvent commonly used in the art. Examples thereof can include organic solvents such as N-methyl-2-pyrrolidine (NMP), dimethyl sulfoxide (DMSO), isopropyl alcohol and acetone, or water, and the like, and any one of them or a mixture of two or more of them can be used. Considering the application thickness and preparation yield of the slurry for forming an electrode, the dispersion medium is used to dissolve or disperse electrode active materials, conductive agents and adhesives. For example, the content of the dispersion medium can make the concentration of the solid components including electrode active materials, conductive agents and optional adhesives be 40% to 80% by weight, preferably 40% to 70% by weight, and more preferably 50% to 65% by weight.

[0083] In addition, when the solid components other than the dispersion medium are included in the slurry for forming an electrode in an amount of 50 to 65 parts by weight based on 100 parts by weight of the slurry for forming an electrode, the viscosity of the slurry for forming an electrode may be 5,000 to 35,000 cPs, preferably 10,000 to 35,000 cPs, and more preferably 10,000 to 30,000 cPs under a temperature condition of 24° C. to 26° C. When the viscosity of the slurry for forming an electrode is within the above range, the solid components other than the dispersion medium are uniformly dispersed, and when the slurry for forming an electrode is applied to a current collector, it can be applied with a uniform thickness.

[0084] electrode

[0085] Hereinafter, the electrodes will be described.

[0086] The electrode of the present invention includes an electrode current collector and an electrode active material layer formed on the electrode current collector. More specifically, the electrode active material layer includes an electrode active material and the conductive agent.

[0087] The electrode may be a positive electrode or a negative electrode, and more specifically a positive electrode. The description of the electrode active material and the conductive agent is the same as above, and thus, a detailed description thereof will be omitted.

[0088] For example, except for forming an electrode active material layer using the slurry for forming an electrode, an electrode may be manufactured by a conventional method for manufacturing an electrode.

[0089] Specifically, the electrode may be manufactured by applying a slurry for forming an electrode on an electrode collector and then drying it, or may be manufactured by casting the slurry for forming an electrode on a separate support and then laminating a film separated from the support on the electrode collector.

[0090] The electrode collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, and the like can be used. In addition, the electrode collector may generally have a thickness of 3 μm to 500 μm, and microscopic irregularities may be formed on the surface of the electrode collector to improve the adhesion of the positive electrode active material. For example, the electrode collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam body, a non-woven fabric body, and the like.

[0091] Lithium secondary battery

[0092] Next, a lithium secondary battery according to the present invention will be described.

[0093] The lithium secondary battery specifically includes a positive electrode, a negative electrode arranged to face the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. At least one of the positive electrode and the negative electrode can be manufactured by using a slurry for forming an electrode including the conductive agent. In addition, the lithium secondary battery may further selectively include a battery container for accommodating an electrode assembly consisting of a positive electrode, a negative electrode and a separator, and a sealing member for sealing the battery container. In addition, the description of the positive electrode and the negative electrode is the same as above, and therefore, a detailed description thereof will be omitted.

[0094] The separator is used to separate the negative electrode and the positive electrode, and provides a mobile path for lithium ions. Any separator can be used without particular limitation, as long as it is generally used as a separator in a secondary battery. In particular, a separator having high moisture retention capacity for electrolytes and low resistance to the movement of electrolyte ions is preferred. Specifically, as a separator, a porous polymer film can be used, for example, a porous polymer film made from polyolefin-based polymers such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or a laminated structure having two or more layers thereof. In addition, typical porous nonwoven fabrics, for example, nonwoven fabrics formed by glass fibers or polyethylene terephthalate fibers with high melting points, and the like can be used as separators. In addition, a coated separator including a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a single-layer structure or a multilayer structure can be selectively used.

[0095] Examples of the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten-type inorganic electrolyte, and the like, which are generally used in the manufacture of a lithium secondary battery.

[0096] Specifically, the electrolyte may include a nonaqueous organic solvent and a lithium salt.

[0097] Any non-aqueous organic solvent can be used as the non-aqueous organic solvent without particular limitation, as long as it can be used as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, as the non-aqueous organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (EPC), etc. can be used. carbonate, PC); alcohol solvents such as ethanol and isopropanol; nitriles such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may include a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolane. Among them, carbonate solvents are preferred, and more preferred is a mixture of cyclic carbonates (such as ethylene carbonate or propylene carbonate) with high ionic conductivity and high dielectric constant and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) that can improve the charge / discharge performance of the battery. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.

[0098] Lithium salts can be used without particular limitation, as long as they are compounds that can provide lithium ions used in lithium secondary batteries. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2 can be used as lithium salts. Lithium salts are preferably used in a concentration range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte properties, and lithium ions can be effectively moved.

[0099] In the electrolyte, in order to improve the life characteristics of the battery, suppress the capacity reduction of the battery, and improve the discharge capacity of the battery, in addition to the electrolyte components, at least one additive may be further added, for example, a halogenated alkylene carbonate-based compound (such as difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, ethylene glycol dimethyl ether (glyme), hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum chloride.

[0100] Therefore, according to another embodiment of the present invention, there are provided a battery module including the lithium secondary battery as a unit battery and a battery pack including the battery module.

[0101] The battery module or battery pack can be used as a power source for at least one medium-sized and large-sized device such as a power tool; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0103] Hereinafter, the present invention will be described in more detail with reference to specific embodiments. However, the following embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. It will be apparent to those skilled in the art that various changes and modifications may be made without departing from the scope and spirit of the present invention, and it is apparent that these changes and modifications fall within the scope of the appended claims.

[0104] [Preparing graphene flakes and preparing graphene]

[0105] 1: Example 1: Preparation of graphene sheets

[0106] 2.56g naphthalene was added to 20ml tetrahydrofuran solvent, and potassium (K) was dissolved therein at a molar concentration of 1mol to prepare an ionic solution. The ionic solution was placed in a glove box and mixed with graphite to a concentration of 100mg / ml to prepare a graphite mixed solution. Afterwards, the graphite mixed solution was stirred at 100rpm to 200rpm at 30°C for 6 hours using a magnetic stirrer. Afterwards, the ionic solution was removed from the stirred graphite mixed solution, and the residual solid components were washed with cyclohexane. 1g of the washed solid components and 1g of polyvinyl pyrrolidone (PVP) were added to 1L dimethyl sulfoxide (DMSO), and a water tank type ultrasonic device (Branson ultrasonic bath) was used to ultrasonically disperse the mixture for 30 minutes. Afterwards, the completely ultrasonically dispersed material was centrifuged at 2000rpm for 1 hour using a centrifugal separator (Hanil Science Combi-514R), and only the upper layer was separated. The separated material of the upper layer portion was centrifuged again at 10000 rpm for 1 hour using a centrifugal separator (Hanil Science Combi-514R) to remove the residual solvent remaining in the upper layer portion, and then a graphene sheet was obtained.

[0107] 2: Comparative Example 1

[0108] Instead of the graphene flakes of Example 1, BTR-(GN-01) as commercially available graphene was prepared.

[0109] 3: Comparative Example 2

[0110] Super C-PAS1003, which is commercially available graphene, was prepared instead of the graphene flakes of Example 1.

[0111] [Preparation of slurry for forming an electrode]

[0112] 1: Example 2

[0113] (1) Preparation of Conductive Agent Dispersion Composition

[0114] 3 g of the graphene flakes prepared according to Example 1 were mixed with N-methyl-2-pyrrolidone (NMP) as a solvent so that the graphene flakes had a concentration of 0.5 mg / ml to 5 mg / ml, and the graphene flakes were dispersed in the solvent by performing sonication dispersion using a water tank type ultrasonic device (Branson ultrasonic bath) for 5 minutes to 20 minutes.

[0115] (2) Preparation of slurry for forming positive electrode

[0116] 250 g of LiNi as a positive electrode active material was added to the conductive agent dispersion composition. 0.6 Mn 0.2 Co 0.2 O2 and 2.5g of polyvinylidene fluoride (PVDF) as a binder were then mixed to prepare a slurry for forming a positive electrode. The graphene flakes were included in an amount of 1.17 parts by weight based on 100 parts by weight of solid components other than the solvent in the slurry for forming a positive electrode.

[0117] 2: Example 3

[0118] A conductive agent dispersion composition and a slurry for forming a positive electrode were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 3.3 g of the graphene flakes prepared according to Example 1 were mixed. The graphene flakes were included in an amount of 1.29 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming a positive electrode.

[0119] 3: Example 4

[0120] A conductive agent dispersion composition and a slurry for forming a positive electrode were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 2.7 g of the graphene flakes prepared according to Example 1 were mixed. The graphene flakes were included in an amount of 1.06 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming a positive electrode.

[0121] 4: Comparative Example 3

[0122] A conductive agent dispersion composition and a slurry for forming a positive electrode were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 3 g of commercially available graphene (BTR-(GN-01)) was used instead of the graphene flakes used in Example 2. The commercially available graphene (BTR-(GN-01)) was included in an amount of 1.17 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming a positive electrode.

[0123] 5: Comparative Example 4

[0124] A conductive agent dispersion composition and a slurry for forming an electrode (positive electrode) were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 3 g of commercially available graphene (Super C-PAS1003) was used instead of the graphene flakes used in Example 2. The commercially available graphene (Super C-PAS1003) was included in an amount of 1.17 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming the positive electrode.

[0125] 6: Comparative Example 5

[0126] A conductive agent dispersion composition and a slurry for forming a positive electrode were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 3 g of carbon nanotubes were used instead of the graphene flakes used in Example 2. The carbon nanotubes were included in an amount of 1.17 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming a positive electrode.

[0127] 7: Comparative Example 6

[0128] A conductive agent dispersion composition and a slurry for forming an electrode (positive electrode) were prepared in the same manner as in Example 2, except that when preparing the conductive agent dispersion composition, 3 g of carbon black was used instead of the graphene flakes used in Example 2. The carbon black was included in an amount of 1.17 parts by weight based on 100 parts by weight of the solid components other than the solvent in the slurry for forming the positive electrode.

[0129] [Manufacturing Example] Manufacturing of Electrode (Positive Electrode) and Lithium Secondary Battery

[0130] 1: Make the positive electrode

[0131] The slurry for forming the positive electrode prepared in Examples 2-4 and Comparative Examples 3-6 was applied to a substrate having a loading of 630 mg / 25 cm 2 The resulting film was placed on an aluminum current collector, dried at 130°C, and then roll-pressed to produce a positive electrode.

[0132] Manufacturing lithium secondary batteries

[0133] Natural graphite as a negative electrode active material, carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder were mixed in a weight ratio of 85:10:5, and then N-methylpyrrolidone as a solvent was added to prepare a slurry for forming a negative electrode. Then, the slurry for forming a negative electrode was applied to a copper current collector to manufacture a negative electrode.

[0134] The porous polyethylene separator is inserted between the positive electrode and the negative electrode prepared as described above to prepare the electrode assembly, and then the electrode assembly is placed in the housing. Afterwards, the electrolyte is injected into the housing to manufacture a lithium secondary battery. At this time, the electrolyte is prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.0M in an organic solvent composed of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate (mixed volume ratio of EC / DMC / EMC = 3 / 4 / 3).

[0135] [Test example]

[0136] 1: Experimental Example 1: X-ray diffraction analysis

[0137] The graphene flakes prepared in Example 1 and the graphene of Comparative Examples 1 and 2 were crushed and measured with an X-ray diffraction analyzer (Bruker AXSD4-Endeavor XRD). The measurement was performed by scanning at intervals of 0.2° with an applied voltage of 40 kV, an applied current of 40 mA, and a 2θ measurement range of 24° to 28°. At this time, a 6 mm variable divergence slit was used as a slit, and a large PMMA holder (diameter = 20 mm) was used to eliminate the background noise caused by the PMMA holder. The intensity ratio of the peak at 25.44° was measured using the EVA program (Bruke Co.). In addition, the crystallinity of the graphene flakes prepared in Example 1 and the graphene of Comparative Examples 1 and 2 was confirmed, and in the data graph obtained by X-ray diffraction (XRD) (see Figure 1 ), the position (°) where the maximum peak appears in the range of 2θ from 24° to 28° and the full width at half maximum (FWHM) of the maximum peak are shown in Table 1 below.

[0138]

Table 1

[0139]

[0140] Figure 1 1 is a data graph obtained by X-ray diffraction (XRD) of the graphene flakes according to Example 1 of the present invention and the graphenes of Comparative Examples 1 and 2. In Example 1, a broad peak was observed at 25.44°, and in Comparative Examples 1 and 2, a narrow peak was observed at 26.51°.

[0141] 2: Test Example 2: Aspect Ratio Analysis

[0142] The average lateral size and average thickness of the graphene flakes of Example 1 and the graphene of Comparative Examples 1 and 2 are measured. First, the conductive agent dispersion composition of Example 2 (wherein the graphene flakes of Example 1 are dispersed) and the conductive agent dispersion composition of Comparative Examples 3 and 4 (wherein the graphene of Comparative Examples 1 and 2 are dispersed) are dripped into a silicon wafer. At this time, the lateral size and thickness of the graphene flakes observed using an atomic force microscope (AFM) are measured respectively. Wherein, the top 50 and the bottom 50 are collected in order of their length to calculate the average lateral size and the average thickness by averaging them, and then the aspect ratio (Aspect ratio) of the calculated average lateral size and the calculated average thickness is measured, and is shown in Table 2 below.

[0143]

Table 2

[0144] Analyze Project Example 1 Comparative Example 1 Comparative Example 2 Average lateral size (μm) 5.04 8.99 6.99 Average thickness (nm) 4.15 790 253.25 Aspect Ratio 1214.46 11.38 27.60

[0145] Referring to Table 2, the aspect ratio of the example is significantly greater than that of the comparative example.

[0146] 3: Experimental Example 3: Raman spectroscopy analysis

[0147] The graphene flakes of Example 1 and the graphene of Comparative Examples 1 and 2 have a wavelength of 1340 cm -1 Up to 1360cm -1 D band within the range (I D ) has the maximum peak intensity at 1575 cm -1 Up to 1600cm -1 G band within the range (I G ) was calculated as an average value based on the ratio of the maximum peak intensities of the wavelength 532 nm obtained by Raman spectroscopy.

[0148]

Table 3

[0149] Analyze Project Example 1 Comparative Example 1 Comparative Example 2 <![CDATA[I D / I G ]]> 0.11 0.056 0.056

[0150] Referring to Table 3, when compared with the comparative example, I D / I G The value is higher than that of Comparative Example 1. D / I G value.

[0151] 4: Experimental Example 4: XPS (X-ray Photoelectron Spectroscopy) Analysis

[0152] The atomic % of the constituent atoms of the graphene sheet of Example 1 and the graphenes of Comparative Examples 1 and 2 obtained by XPS analysis are shown in Table 4 below. Figure 2is a data graph obtained by XPS analysis of the graphene flakes according to Example 1 of the present invention and the graphenes of Comparative Examples 1 and 2.

[0153]

Table 4

[0154] Analyze Project Example 1 Comparative Example 1 Comparative Example 2 Carbon (atomic %) 90.49 96.67 94.77 Oxygen (atomic %) 7.63 3.33 2.89 Nitrogen (atomic %) 1.88 - 2.34

[0155] Refer to Table 4 and Figure 2 , the oxygen atomic % of the graphene sheet of Example 1 is higher than the oxygen atomic % of the graphene of the comparative example.

[0156] 5: Test Example 5: Measurement of Powder Resistance of Slurry for Forming Electrode

[0157] The changes in the compacted density of the slurries for forming electrodes prepared in Examples 2-4 and Comparative Examples 3-6 were measured for powder resistance. The results are shown in Figure 3 middle.

[0158] Each of the prepared slurries for forming an electrode was dried and ground, and then the powder resistivity was measured by changing the compaction density using a powder resistance measuring device (HPRM-A2, Hantec Co.).

[0159]

Table 5

[0160]

[0161] In the case of the examples containing the same content, the powder resistance of the examples was significantly lower than that of all the comparative examples except for Comparative Example 5. Although the powder resistance of Comparative Example 5 was lower than that of the examples, its adhesion and battery capacity retention rate were confirmed to be lower than those of the examples.

[0162] 6: Test Example 6: Measurement of Adhesion of Slurry for Forming Electrode

[0163] Adhesion was measured by applying the slurries for forming electrodes prepared in Examples 2-4 and Comparative Examples 3-6 on a substrate (aluminum foil), and then pulling the dried slurries to 90° at a rate of 100 mm / min to measure the applied force (gf) until the dried slurries fell off. The results are shown in Tables 6 and 7 below. Figure 4 middle.

[0164]

Table 6

[0165]

[0166] Referring to Table 6, the adhesion of the slurry for forming an electrode prepared according to the example is better than that of the comparative example.

[0167] 7: Test Example 7: Evaluation of High-Temperature Cycle Capacity Retention of Lithium Secondary Batteries

[0168] The lithium secondary battery manufactured in the manufacturing example was charged and discharged based on 1 charge and discharge cycle under the conditions of 45°C, SOC 50% and 10C, and the cycle capacity retention rate up to 1800 cycles (300, 600, 900, 1800) was measured. The measured capacity retention rates are shown in Tables 7 and 10 below. Figure 5 middle.

[0169]

Table 7

[0170]

[0171] Refer to Table 7 and Figure 5 , the capacity retention rate of the embodiment is higher than that of the comparative example. Meanwhile, in the case of comparative example 5, it can be confirmed that as the number of cycles increases, its capacity retention rate is further reduced compared with that of embodiment 2.

[0172] 8: Test Example 8: Evaluation of High-Temperature Cycle Capacity Retention of Lithium Secondary Batteries

[0173] The capacity retention rate and resistance increase rate of the lithium secondary battery prepared in the manufacturing example were measured by charging the battery weekly until the fifth week under the conditions of 60°C and SOC 100%. The measured capacity retention rate and resistance increase rate are shown in the following Tables 8 and Figure 6 In. Figure 6 The capacity retention rate can be confirmed by the upper figure, and the resistance increase rate can be confirmed by the lower figure.

[0174]

Table 8

[0175]

[0176] Refer to Table 8 and Figure 6 , the capacity retention rate of the lithium secondary battery according to the embodiment is high, but its resistance increase rate is low. Meanwhile, in the case of Example 2, compared with Comparative Example 5, the capacity retention rate is high and the resistance increase rate is low.

[0177] This application also relates to the following aspects.

[0178] 1. A conductive agent, comprising:

[0179] A graphene sheet, in a data graph obtained by X-ray diffraction (XRD) analysis, a maximum peak of the graphene sheet is observed in the range of 2θ of 24.5° to 26°, wherein

[0180] An aspect ratio of an average lateral dimension of a surface of the graphene flakes to an average thickness of the graphene flakes in a direction perpendicular to the surface of the graphene flakes is 500 to 50,000.

[0181] 2. The conductive agent according to item 1, wherein the average thickness of the graphene flakes is 1 nm to 10 nm.

[0182] 3. The conductive agent according to item 1, wherein the graphene sheet has a full width at half maximum (FWHM) of 0.5° to 5° at a maximum peak in the range of 2θ from 24.5° to 26°.

[0183] 4. The conductive agent according to item 1, wherein the graphene flakes are at 1360±50cm -1 The maximum peak intensity of the D band at 1580±50cm -1 The average ratio of the maximum peak intensities of the G band at is 0.06 to 0.5, which is obtained by Raman spectroscopy using a laser with a wavelength of 532 nm.

[0184] 5. The conductive agent according to item 1, wherein the average oxygen content of the graphene flakes is 5 atomic % to 10 atomic %.

[0185] 6. A slurry for forming an electrode, the slurry comprising:

[0186] Electrode active materials;

[0187] Adhesives;

[0188] dispersion medium; and

[0189] The conductive agent according to item 1.

[0190] 7. The slurry according to item 6, wherein the conductive agent is included in an amount of 0.05 parts by weight to 2.0 parts by weight based on 100 parts by weight of solid components other than the dispersion medium in the slurry for forming an electrode.

[0191] 8. A slurry according to item 6, wherein when the solid components other than the dispersion medium in the slurry for forming an electrode are included in an amount of 50 parts by weight to 65 parts by weight based on 100 parts by weight of the slurry for forming an electrode, the viscosity of the slurry for forming an electrode is 5,000 cPs to 35,000 cPs under temperature conditions of 24°C to 26°C.

[0192] 9. An electrode, comprising:

[0193] an electrode current collector; and

[0194] An electrode active material layer is formed on the electrode current collector, wherein

[0195] The electrode active material layer includes an electrode active material and the conductive agent according to Item 1.

[0196] 10. A lithium secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein

[0197] At least one of the positive electrode and the negative electrode is an electrode according to item 9.

Claims

1. A conductive agent comprising: A graphene sheet, wherein in a data graph obtained by X-ray diffraction analysis, a maximum peak of the graphene sheet is observed in the range of 2θ of 24.5° to 26°, wherein an aspect ratio of an average lateral dimension of the surface of the graphene flakes to an average thickness of the graphene flakes in a direction perpendicular to the surface of the graphene flakes of 500 to 50,000, and The graphene sheet is formed in a single layer; The average oxygen content of the graphene sheet is 5 atomic % to 10 atomic %, The graphene sheet is at 1360±50cm -1 The maximum peak intensity of the D band at 1580 ± 50 cm -1 The average ratio of the maximum peak intensities of the G band at φ is 0.06 to 0.5, which is obtained by Raman spectroscopy using a laser with a wavelength of 532 nm. 2 . The conductive agent according to claim 1 , wherein the average thickness of the graphene flakes is 1 nm to 10 nm. 3 . The conductive agent according to claim 1 , wherein the graphene sheet has a full width at half maximum (FWHM) of 0.5° to 5° at a maximum peak in the range of 2θ of 24.5° to 26°.

4. A slurry for forming an electrode, the slurry comprising: Electrode active materials; Adhesives; dispersion medium; and The conductive agent according to claim 1. The slurry according to claim 4 , wherein the conductive agent is included in an amount of 0.05 parts by weight to 2.0 parts by weight based on 100 parts by weight of solid components excluding the dispersion medium in the slurry for forming an electrode.

6. The slurry according to claim 4, wherein when the solid components other than the dispersion medium in the slurry for forming an electrode are included in an amount of 50 parts by weight to 65 parts by weight based on 100 parts by weight of the slurry for forming an electrode, the viscosity of the slurry for forming an electrode is 5,000 cPs to 35,000 cPs under a temperature condition of 24° C. to 26° C.

7. An electrode comprising: electrode current collector; and An electrode active material layer is formed on the electrode current collector, wherein The electrode active material layer includes an electrode active material and the conductive agent according to claim 1 .

8. A lithium secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein At least one of the positive electrode and the negative electrode is the electrode according to claim 7.