Preparation method and application of cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst
By using core-shell MOFs materials in fuel cells to prepare cobalt ferroalloy/nitrogen co-doped carbon-based catalysts, the problem of poor stability of noble metal-based catalysts is solved, and high-efficiency oxygen reduction catalysis and stability are achieved, with performance close to that of commercial precious metal catalysts.
Patent Information
- Application Number
- CN202411400501.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-12
AI Technical Summary
Existing precious metal-based catalysts have poor stability in oxygen reduction reactions in fuel cells, are susceptible to toxicity by small organic molecules, and have limited reserves, making it difficult to meet the needs of large-scale applications. It is necessary to develop new, green and efficient heteroatom-doped porous carbon-based catalyst materials.
Core-shell metal organic frame materials (MOFs) are used as precursors, and co-doped co-doped carbon-based catalysts are prepared through sonication and pyrolysis to form multi-stage pore structures and metal-nitrogen-carbon active sites to enhance Catalytic activity and stability.
The catalytic activity and stability of high oxygen reduction under alkaline conditions were achieved. The current retention rate of the catalyst was as high as 94% after 40,000 seconds, the performance was close to that of commercial precious metal catalysts, and the methanol resistance was good.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of novel nanocomposite materials, and in particular relates to a novel cobalt-iron alloy / nitrogen co-doped carbon-based catalytic material. Background Art
[0002] During the electrochemical reaction, fuel cells can directly convert the chemical potential energy stored in the fuel into electrical energy with high efficiency. The conversion process does not require any intermediate links, which significantly improves the efficiency of energy conversion. Through this innovative technology, fuel cells not only optimize the way of energy utilization, but also provide strong support for sustainable energy development. Due to its clean and efficient performance, it has attracted much attention from the scientific community. The development of efficient oxygen electrode catalysts is the key to promoting major breakthroughs in new energy conversion devices such as fuel cells. Commercial precious metal-based catalysts have good oxygen reduction reaction (ORR) properties, but due to their poor stability, susceptibility to organic small molecule poisoning, and limited reserves, it is difficult to meet the needs of large-scale applications. Therefore, the development of green and efficient synthesis methods to prepare new heteroatom-doped porous carbon-based catalytic materials has important scientific significance and application value. Heteroatom-doped porous carbon materials are expected to replace commercial precious metal catalysts and be used in related fields such as fuel cells because of their good oxygen electrocatalytic activity and stability. Multi-level pore structure carbon materials have special morphological advantages, such as large specific surface area, good conductivity and easy doping. They have high active site density and fast material transfer, which can significantly improve the oxygen reduction catalytic activity. In terms of composition, nitrogen atom doping will introduce new active sites, further enhancing the catalytic activity of carbon materials. Since the electronegativity of nitrogen atoms (χ=3.04) is greater than that of carbon atoms (χ=2.55), when they are doped into the carbon layer, electron transfer sites will be generated, which is beneficial to promote electron transfer and mass transfer during oxygen reduction. On the other hand, the metal-nitrogen-carbon composite center is beneficial to the kinetic process of the catalytic reaction. The key to preparing efficient carbon-based nanocatalytic materials with multi-level pore structure loaded with cobalt-iron alloy is to make nitrogen atoms evenly distributed on the surface of the material and convert them into metal-nitrogen-carbon active sites after high-temperature treatment. To achieve this goal, core-shell metal organic framework materials (MOFs) are widely used in the preparation of carbon-based nanocatalytic materials with multi-level pore structure loaded with cobalt-iron alloy.
[0003] Core-shell MOFs are metal organic framework materials with special structures and properties. The material consists of two parts, usually a core (core) composed of a central metal ion and a shell (shell) formed by an outer layer of organic ligands. This structure gives MOFs an internal cavity and an external surface, which is conducive to the storage and release of molecules. MOFs have a very high specific surface area due to their porous structure, which makes them advantageous in applications such as gas adsorption, separation and catalysis. The core-shell structure allows the properties of MOFs to be adjusted by selecting appropriate metal ions and organic ligands, thereby changing their pore size, chemical activity and stability. Therefore, the introduction of phthalocyanine iron molecules on the surface of core-shell MOFs materials can not only provide iron and nitrogen sources for the system, but also induce subsequent heat treatment to form a highly efficient oxygen electroactive site cobalt-iron alloy and improve the local carbon migration efficiency through metallothermic action to promote the formation of new pores. Due to its porous structure and adjustability, it is simpler to use core-shell MOFs materials as catalyst precursors. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a preparation method of a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst, thereby realizing the study of oxygen reduction performance.
[0005] One of the purposes of the present invention is to provide a method for preparing a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst.
[0006] The second purpose of the present invention is to use the prepared cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst for oxygen reduction performance research.
[0007] The technical solution of the present invention comprises the following steps: 1. A preparation method of a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst, comprising the following steps: 290.0~310.0 mg of core-shell MOFs material was dispersed in 40.0 mL of acetone and ultrasonicated for 30 min; Then, 10.0 mL of acetone solution containing 90.0-110.0 mg of iron phthalocyanine was added to (1), and the mixture was heated to 60 °C and refluxed for 8 h. The precipitate was washed with acetone, and then the precipitate was dried in a vacuum oven at 50 °C overnight to obtain the iron phthalocyanine / core-shell MOFs composite (ZIF-8@ZIF-67-FePc). The quartz boat containing the ZIF-8@ZIF-67-FePc composite was placed in a tubular heating furnace and heated at 5 °C min under a nitrogen atmosphere. -1 Heating to 900°C and keeping the temperature constant for 2h to obtain CoFe / NCC; In addition, referring to the above ratio, 1, 2 and 4 times molar amounts of iron phthalocyanine were used to prepare CoFe / NCC-x (x=1, 2 and 4) composites with different iron phthalocyanine binding amounts. CoFe / NCC-x (x=1, 2 and 4) were prepared using CoFe / NCC-x as a precursor to compare the properties of catalysts with different loading amounts of iron phthalocyanine, and the pyrolysis treatment steps were the same as above.
[0008] 2. The method for preparing a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst according to claim 1, characterized in that the preparation of the core-shell MOFs material comprises the following steps: (1) Weigh 9.0-11.0 g of 2-methylimidazole and dissolve it in 100 mL of methanol to obtain solution 1. Weigh 8.0-10.0 g of zinc nitrate and dissolve it in 300.0 mL of methanol to obtain solution 2. Mix solution 1 and solution 2, stir for 15 minutes until the reactants are completely dissolved, seal the solution with a sealing film, and let it stand at room temperature for 24 hours. (2) After standing, the precipitate was washed with methanol and deionized water in the reaction solution, and then the precipitate was placed in a vacuum oven at 60°C and dried overnight to obtain the ZIF-8 material; (3) Weigh 1.0-3.0 g of the synthesized ZIF-8 material and dissolve it in 300 mL of methanol solution. Ultrasonicate for 15 minutes and then stir for 5 minutes to obtain solution 1. Weigh 3.0-5.0 g of 2-methylimidazole and 800.0-1000.0 mg of cobalt nitrate hexahydrate and dissolve them in 100 mL of methanol solution to obtain solution 2. Mix solution 1 and solution 2 and stir for 24 hours. (4) After the stirring is completed, the precipitate is washed with methanol and deionized water in the reaction solution, and then the precipitate is placed in a vacuum oven and dried at 60°C overnight to obtain the ZIF-8@ZIF-67 material.
[0009] 3. A cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst prepared by the preparation method according to claim 1 is used for studying the catalytic performance of oxygen reduction reaction, and the detection steps are as follows: (1) 5.0 mg of the catalyst was dispersed in 1.0 mL of a mixed solvent of water-isopropanol-Nafion (V / V / V = 15 / 4 / 1) and ultrasonically dispersed to obtain a uniform suspension (5.0 mg mL -1 ); (2) The working electrode was a rotating ring-disk electrode loaded with catalyst. 4.0 µL of the suspension was transferred using a pipette and spin-coated onto a previously polished ring-disk electrode and allowed to stand and dry. The electrode catalyst loading was 0.16 mg cm -2 ; (3) All electrochemical experiments, including cyclic voltammetry (CV) and linear voltammetry (LSV), were performed in 0.1 M KOH solution saturated with oxygen or nitrogen at room temperature; (4) CV scan rate is 50 mV s -1 , LSV scan rate is 5 mV s -1 , the ring disk electrode speed range is 400-2250rpm.
[0010] (1) The present invention prepares a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst. The core-shell MOFs material is used as the binding part of the precursor complex. After carbonization, it still maintains a good porous structure and has uniformly dispersed cobalt-nitrogen and iron-nitrogen active sites. At the same time, it provides a graphitized carbon layer of appropriate thickness for the iron phthalocyanine material, effectively preventing excessive aggregation of particles and improving its catalytic stability. Thanks to the synergistic optimization of the catalyst composition and structure, CoFe / N-CNCC exhibits catalytic activity comparable to that of commercial precious metal catalysts under alkaline conditions, with higher stability and methanol resistance; (2) A cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst was used to study oxygen reduction performance and to test its electrocatalytic oxygen reduction reaction. Under alkaline conditions, the catalyst has good oxygen reduction catalytic properties; its half-wave potential can reach 0.87V in 0.1M KOH solution; the number of reaction electron transfers can be calculated by the KL equation to be 3.86-3.94, approximately 4 electron transfers; through long-cycle stability tests, the catalyst showed good stability, and after 40,000s, the current retention rate was still as high as 94%. DETAILED DESCRIPTION
[0011] The present invention will now be further described by way of specific embodiments, but is not limited thereto.
[0012] Example 1 A method for preparing a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst (1) Disperse 290.0 mg of core-shell MOFs material in 40.0 mL of acetone and ultrasonicate for 30 min; (2) Then, 10.0 mL of acetone solution containing 90.0 mg of iron phthalocyanine was added to (1), the temperature was raised to 60 °C and refluxed with stirring for 8 h, and then the precipitate was washed with acetone, and then the precipitate was placed in a vacuum oven at 50 °C and dried overnight to obtain the iron phthalocyanine / core-shell MOFs composite (ZIF-8@ZIF-67-FePc); (3) The quartz boat containing the ZIF-8@ZIF-67-FePc composite was placed in a tubular heating furnace, and the temperature was raised to 900 °C at 5 °C min-1 under a nitrogen atmosphere and kept at this temperature for 2 h to obtain CoFe / NCC; (4) In addition, referring to the above ratio, 1, 2 and 4 times the molar amount of iron phthalocyanine were used to prepare CoFe / NCC-x (x = 1, 2 and 4) composites with different iron phthalocyanine binding amounts. CoFe / NCC-x (x = 1, 2 and 4) were prepared using CoFe / NCC-x as a precursor to compare the properties of catalysts with different iron phthalocyanine loadings. The pyrolysis treatment steps were the same as above.
[0013] Example 2 Preparation method of cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst (1) Disperse 300.0 mg of core-shell MOFs material in 40.0 mL of acetone and treat with ultrasound for 30 min; (2) Then, 10.0 mL of acetone solution containing 100.0 mg of iron phthalocyanine was added to (1), the temperature was raised to 60 °C and refluxed with stirring for 8 h, and then the precipitate was washed with acetone, and then the precipitate was placed in a vacuum oven at 50 °C and dried overnight to obtain the iron phthalocyanine / core-shell MOFs composite (ZIF-8@ZIF-67-FePc); (3) The quartz boat containing the ZIF-8@ZIF-67-FePc composite was placed in a tubular heating furnace, and the temperature was raised to 900 °C at 5 °C min-1 under a nitrogen atmosphere and kept at this temperature for 2 h to obtain CoFe / NCC; (4) In addition, referring to the above ratio, 1, 2 and 4 times the molar amount of iron phthalocyanine were used to prepare CoFe / NCC-x (x = 1, 2 and 4) composites with different iron phthalocyanine binding amounts. CoFe / NCC-x (x = 1, 2 and 4) were prepared using CoFe / NCC-x as a precursor to compare the properties of catalysts with different iron phthalocyanine loadings. The pyrolysis treatment steps were the same as above.
[0014] Example 3 Preparation method of cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst (1) Disperse 310.0 mg of core-shell MOFs material in 40.0 mL of acetone and treat with ultrasound for 30 min; (2) Then, 10.0 mL of acetone solution containing 110.0 mg of iron phthalocyanine was added to (1), the temperature was raised to 60 °C and refluxed with stirring for 8 h, and then the precipitate was washed with acetone, and then the precipitate was placed in a vacuum oven at 50 °C and dried overnight to obtain the iron phthalocyanine / core-shell MOFs composite (ZIF-8@ZIF-67-FePc); (3) The quartz boat containing the ZIF-8@ZIF-67-FePc composite was placed in a tubular heating furnace, and the temperature was raised to 900 °C at 5 °C min-1 under a nitrogen atmosphere and kept at this temperature for 2 h to obtain CoFe / NCC; (4) In addition, referring to the above ratio, 1, 2 and 4 times the molar amount of iron phthalocyanine were used to prepare CoFe / NCC-x (x = 1, 2 and 4) composites with different iron phthalocyanine binding amounts. CoFe / NCC-x (x = 1, 2 and 4) were prepared using CoFe / NCC-x as a precursor to compare the properties of catalysts with different iron phthalocyanine loadings. The pyrolysis treatment steps were the same as above.
[0015] Example 4 Preparation of the core-shell MOFs material (1) Weigh 9.0 g of 2-methylimidazole and dissolve it in 100 mL of methanol to obtain solution 1. Weigh 8.0 g of zinc nitrate and dissolve it in 300.0 mL of methanol to obtain solution 2. Mix solution 1 and solution 2, stir for 15 minutes until the reactants are completely dissolved, seal the solution with a sealing film, and let it stand at room temperature for 24 hours. (2) After standing, the precipitate was washed with methanol and deionized water in the reaction solution, and then the precipitate was placed in a vacuum oven at 60°C and dried overnight to obtain the ZIF-8 material; (3) Weigh 1.0 g of the synthesized ZIF-8 material and dissolve it in 300 mL of methanol solution. Ultrasonicate for 15 minutes and then stir for 5 minutes to obtain solution 1. Weigh 3.0 g of 2-methylimidazole and 800.0 mg of cobalt nitrate hexahydrate and dissolve them in 100 mL of methanol solution to obtain solution 2. Mix solution 1 and solution 2 and stir for 24 hours. (4) After the stirring is completed, the precipitate is washed with methanol and deionized water in the reaction solution, and then the precipitate is placed in a vacuum oven and dried at 60°C overnight to obtain the ZIF-8@ZIF-67 material.
[0016] Example 5 Preparation of the core-shell MOFs material (1) Weigh 10.0 g of 2-methylimidazole and dissolve it in 100 mL of methanol to obtain solution 1. Weigh 9.0 g of zinc nitrate and dissolve it in 300.0 mL of methanol to obtain solution 2. Mix solution 1 and solution 2, stir for 15 minutes until the reactants are completely dissolved, seal the solution with a sealing film and let it stand at room temperature for 24 hours; (2) After standing, the precipitate was washed with methanol and deionized water in the reaction solution, and then the precipitate was placed in a vacuum oven at 60°C and dried overnight to obtain the ZIF-8 material; (3) Weigh 2.0 g of the synthesized ZIF-8 material and dissolve it in 300 mL of methanol solution. Ultrasonicate for 15 minutes and then stir for 5 minutes to obtain solution 1. Weigh 4.0 g of 2-methylimidazole and 900.0 mg of cobalt nitrate hexahydrate and dissolve them in 100 mL of methanol solution to obtain solution 2. Mix solution 1 and solution 2 and stir for 24 hours. (4) After the stirring is completed, the precipitate is washed with methanol and deionized water in the reaction solution, and then the precipitate is placed in a vacuum oven and dried at 60°C overnight to obtain the ZIF-8@ZIF-67 material.
[0017] Example 6 Preparation of the core-shell MOFs material (1) Weigh 11.0 g of 2-methylimidazole and dissolve it in 100 mL of methanol to obtain solution 1. Weigh 10.0 g of zinc nitrate and dissolve it in 300.0 mL of methanol to obtain solution 2. Mix solution 1 and solution 2, stir for 15 minutes until the reactants are completely dissolved, seal the solution with a sealing film and let it stand at room temperature for 24 hours; (2) After standing, the precipitate was washed with methanol and deionized water in the reaction solution, and then the precipitate was placed in a vacuum oven at 60°C and dried overnight to obtain the ZIF-8 material; (3) Weigh 3.0 g of the synthesized ZIF-8 material and dissolve it in 300 mL of methanol solution. Ultrasonicate for 15 minutes and then stir for 5 minutes to obtain solution 1. Weigh 5.0 g of 2-methylimidazole and 1000.0 mg of cobalt nitrate hexahydrate and dissolve them in 100 mL of methanol solution to obtain solution 2. Mix solution 1 and solution 2 and stir for 24 hours. (4) After the stirring is completed, the precipitate is washed with methanol and deionized water in the reaction solution, and then the precipitate is placed in a vacuum oven and dried at 60°C overnight to obtain the ZIF-8@ZIF-67 material.
[0018] Example 7 Study on the catalytic performance of the cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction catalyst for oxygen reduction reaction (1) 5.0 mg of the catalyst was dispersed in 1.0 mL of a mixed solvent of water-isopropanol-Nafion (V / V / V = 15 / 4 / 1) and ultrasonically dispersed to obtain a uniform suspension (5.0 mg mL -1 ); (2) For the oxygen reduction reaction test, the working electrode was a rotating ring disk electrode loaded with catalyst. 4.0 µL of the suspension was transferred using a pipette and spin-coated onto a previously polished ring disk electrode and allowed to stand and dry. The electrode catalyst loading was 0.16 mg cm -2 All electrochemical experiments, including cyclic voltammetry (CV) and linear voltammetry (LSV), were performed in 0.1 M KOH solution saturated with oxygen or nitrogen at room temperature; the CV scan rate was 50 mV s -1 , LSV scan rate is 5 mV s -1 , the ring disk electrode speed range is 400-2250rpm.
Claims
1. A method for preparing a cobalt-iron alloy / nitrogen co-doped carbon-based oxygen reduction electrocatalyst, It is characterized in that The following steps are involved: Preparation of core-shell MOFs materials; Preparation of iron phthalocyanine / core-shell MOFs composite-derived carbon-based oxygen reduction electrocatalysts for the study of catalytic performance of oxygen reduction reaction; The preparation steps of the core-shell MOFs material are as follows: ① Weigh 9.0-11.0 g of 2-methylimidazole and dissolve it in 100 mL of methanol to obtain solution 1, weigh 8.0-10.0 g of zinc nitrate and dissolve it in 300.0 mL of methanol to obtain solution 2, mix solution 1 and solution 2, stir for 15 minutes until the reactants are completely dissolved, seal the solution with a sealing film and let it stand at room temperature for 24 hours; ② After standing, the precipitate was washed with methanol and deionized water in the reaction solution, and then the precipitate was placed in a vacuum oven at 60°C and dried overnight to obtain the ZIF-8 material; ③ Weigh 1.0-3.0 g of the synthesized ZIF-8 material and dissolve it in 300 mL of methanol solution. Ultrasonicate for 15 minutes and then stir for 5 minutes to obtain solution 1. Weigh 3.0-5.0 g of 2-methylimidazole and 800.0-1000.0 mg of cobalt nitrate hexahydrate and dissolve them in 100 mL of methanol solution to obtain solution 2. Mix solution 1 and solution 2 and stir for 24 hours. ④ After the stirring is completed, the precipitate is washed with methanol and deionized water in the reaction solution, and then the precipitate is placed in a vacuum oven and dried at 60°C overnight to obtain the ZIF-8@ZIF-67 material.
2. Preparation of Cobalt-Iron Alloy / Nitrogen Co-doped Carbon-based Oxygen Reduction Catalyst, the steps are as follows: ① Disperse 290.0~310.0 mg of core-shell MOFs material in 40.0 mL of acetone and treat with ultrasound for 30 min; ② Then, 10.0 mL of acetone solution containing 90.0-110.0 mg of phthalocyanine iron was added to (1), the temperature was raised to 60 °C and refluxed with stirring for 8 h, and then the precipitate was washed with acetone, and then the precipitate was placed in a vacuum oven at 50 °C and dried overnight to obtain the phthalocyanine cobalt / core-shell MOFs composite (ZIF-8@ZIF-67-FePc); ③Put the quartz boat containing the ZIF-8@ZIF-67-FePc composite into a tubular heating furnace and heat it at 5℃min under nitrogen atmosphere. -1 Heating to 900°C and keeping the temperature constant for 2h to obtain CoFe / NCC; ④ In addition, referring to the above ratio, 1, 2 and 4 times the molar amount of iron phthalocyanine were used to prepare CoFe / NCC-x (x=1, 2 and 4) complexes with different iron phthalocyanine binding amounts. CoFe / NCC-x (x=1, 2 and 4) was prepared using CoFe / NCC-x as a precursor to compare the properties of iron phthalocyanine catalysts with different loading amounts, and the pyrolysis treatment steps were the same as above.
3. The catalytic performance of the catalyst for oxygen reduction reaction is tested in the following steps: ① 5.0 mg of the catalyst was dispersed in 1.0 mL of a mixed solvent of water-isopropanol-Nafion (V / V / V=15 / 4 / 1) and ultrasonically dispersed to obtain a uniform suspension (5.0 mg mL -1 ); ② The working electrode is a rotating ring disk electrode loaded with catalyst. Use a pipette to transfer 4.0 µL of the suspension onto the previously polished ring disk electrode and let it stand to dry. The electrode catalyst loading is 0.16 mg cm -2 ; ③ All electrochemical experiments, including cyclic voltammetry (CV) and linear sweep voltammetry (LSV), were performed in 0.1 M KOH solution saturated with oxygen or nitrogen at room temperature; ④CV scan rate is 50mV s -1 , LSV scan rate is 5 mV s -1 , the ring disk electrode speed range is 400-2250rpm.
Citation Information
Cited By
Cobalt-zinc bimetal modified lignin-based catalyst as well as preparation method and application thereof