LiNi0. 8Co0. 1Mn0. 1O2-delta-SnO2-based composite electrolyte material and semiconductor ion fuel cell
The composite electrolyte material of LiNi0.8Co0.1Mn0.1O2-δ and SnO2 is formed, and the lithium embedded characteristics of SnO2 and the conductivity of LiNi0.8Co0.1Mn0.1O2-δ are used to solve the problem of low temperatures in SIFC electrolyte materials. The problem of insufficient ion conductivity has achieved the improvement of high power density and electrochemical performance.
Patent Information
- Application Number
- CN202411092997.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to increase the ionic conductivity of semiconductor ionic fuel cell (SIFC) electrolyte materials at low temperatures, especially non-ceria-based electrolytes, resulting in a power density of less than 1100 mW/cm2.
The composite electrolyte material of LiNi0.8Co0.1Mn0.1O2-δ and SnO2 was synthesized by high-temperature solid phase method and sol-gel method to form a P-N heterostructure. The lithium-embedded characteristics of SnO2 and LiNi0.8Co0.1Mn0.1O2- The oxygen ion conductivity of δ generates molten Li2CO3/LiOH complexes, improving the density and ionic conductivity of the electrolyte.
At 550°C, the maximum power density reached 1169 mW/cm2, the open circuit voltage was 1.15 V, and the ohmic impedance was 0.14 Ω·cm2, which significantly improved the power density than that used LiNi0.8Co0.1Mn0.1O2-δ electrolyte alone, solving the problem of solving Battery short circuit problem.
Smart Images

Figure CN118943439A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid oxide fuel cells, and more specifically to a LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2-based composite electrolyte materials and semiconductor ion fuel cells. Background Art
[0002] As global energy and environmental issues become increasingly severe, it is a general trend to vigorously develop high-efficiency, pollution-free solid oxide fuel cells (SOFCs). SOFC is one of the electrochemical energy conversion devices, with the advantages of all components being solid, high energy conversion efficiency and no pollution. Traditional SOFCs have a high operating temperature of 600-1000℃, which leads to problems such as long startup time and poor stability.
[0003] Semiconductor ion fuel cell (SIFC) is a SOFC that uses a semiconductor and ion conductor composite as the electrolyte. The internal heterogeneous structure of the electrolyte improves the electrochemical performance of the battery at low temperatures (450-600°C) and is considered to be a potential battery for commercialization.
[0004] In recent years, researchers have found that CeO2-based materials mixed with traditional SOFC cathode materials as electrolytes can form a junction with a rectifying effect that can suppress electronic conductivity and effectively increase the battery's opening voltage and MPD. Nie et al. used Sm 3+ and Ca 2+ Co-doped CeO2(SCDC) and SrCo 0.8 Nb 0.1 Ta 0.1 O 3−δ The SIFC was fabricated by using SCNT as electrolyte and NCAL as symmetrical electrode in a mass ratio of 9:1. The SIFC obtained a higher opening voltage and nearly twice the MPD (1016 mW / cm2) than SCDC at an operating temperature of 550°C. 2 ).
[0005] However, it is difficult to achieve a battery power of 1100 mW / cm 2 The above power density is especially for batteries with non-ceria-based electrolytes.
[0006] How to improve the ionic conductivity of SIMFC electrolyte materials at low temperatures and at the same time make SIFC have ultra-high electrochemical performance is an urgent problem that needs to be solved. Summary of the invention
[0007] In view of this, one of the purposes of the present invention is to provide a composite electrolyte material suitable for semiconductor ion fuel cells. The composite electrolyte material provided by the present invention has ultra-high electrochemical performance at low temperatures, and an excellent maximum power density of 1169 mW / cm2 is obtained at 550°C. 2 , which ranks among the best in non-ceria-based electrolytes.
[0008] To achieve the above object, the technical solution of the present invention is as follows: A LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2-based composite electrolyte material, the composite electrolyte material is used as an electrolyte for a semiconductor ion fuel cell, the composite electrolyte material is composed of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2, the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mass ratio of SnO2 is 6~9:1~4.
[0009] Here, δ is a value that allows the compound to maintain electrical neutrality.
[0010] In the present invention, on the one hand, LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ It is a kind of 2- / H + / e - The conductive triple conductive material, whose excellent oxygen ion and proton conductivity meets the requirements of SIFC electrolyte, but has a higher electronic conductivity and increases the possibility of battery short circuit. Therefore, in the prior art, it is usually used as a lithium battery positive electrode material.
[0011] On the other hand, tin dioxide is a wide bandgap N-type semiconductor. Due to its specific conductivity, tin dioxide is a new negative electrode material for lithium-ion batteries in the prior art.
[0012] In the present invention, a Li-containing + LiNi 0.8 Co 0.1 Mn 0.1 O 2-δWith wide bandgap N-type semiconductor SnO2-based composite electrolyte, as the electrolyte of semiconductor ion fuel cell, the unique lithium insertion property of SnO2 is used to convert Li + Directly introduced into the electrolyte, when the semiconductor ion fuel cell is running, a large amount of molten Li2CO3 / LiOH complex will be directly generated in the electrolyte, which greatly improves the density and ion conductivity of the electrolyte. 0.8 Co 0.1 Mn 0.1 O 2-δ The PN heterostructure formed at the interface with SnO2, the space charge layer of the PN junction can effectively promote the 2- and H + The conduction of electrons is inhibited.
[0013] Furthermore, the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mass ratio of SnO2 is 6~8:2~4.
[0014] Furthermore, the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mass ratio of SnO2 is 7:3.
[0015] Wherein, the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2 were synthesized by high temperature solid phase method and sol-gel method respectively.
[0016] A second object of the present invention is to provide a method for preparing the above-mentioned composite electrolyte material, comprising the following steps: (1) Weigh LiNi according to the mixing mass ratio 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2; (2) LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2 are placed in a ball mill, anhydrous ethanol is added for ball milling and mixing to obtain a mixed slurry; (3) drying the mixed slurry to remove anhydrous ethanol to obtain a dried mixed slurry; (4) The dried mixed slurry is subjected to primary grinding, sintering, and secondary grinding to obtain LiNi 0.8 Co 0.1Mn 0.1 O 2-δ -SnO2-based composite electrolyte materials.
[0017] Furthermore, in step (1), the rotation speed of the ball mill is 150-200 r / min, and the ball milling time is 5-7 h; in step (3), the mixed slurry is placed under a heating lamp for drying, and the drying time is 2-4 h; in step (4), the first grinding time is 30-60 min, the sintering temperature is 550-650°C, the sintering time is 4-6 h, and the second grinding time is 30-60 min.
[0018] Furthermore, in step (1), the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The preparation method comprises: S1. Weigh the raw materials Li2CO3, NiO, Co3O4 and Mn2O3 according to the element ratio and place them in a ball mill. Add anhydrous ethanol and set the speed and time to 180-280 r / min and 5-7 h respectively. S2. Suck out the mixed raw materials in the ball mill, place them under a heating lamp to dry the anhydrous ethanol; after drying, grind them in a mortar for 30-60 min, and then pre-calculate them in a muffle furnace at 450-550°C for 4-6 h; S3, after pre-sintering, grind again in a mortar for 30-60 min, then sinter at 700-1000 °C for 8-12 h; grind again in a mortar for 30-60 min after sintering to obtain a P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ powder; Preferably, in step S3, the sintering temperature is 800-900°C.
[0019] Furthermore, in step (1), the method for preparing SnO2 comprises: S1. Add tin nitrate into a container, and then place it on a magnetic stirrer to fully stir and dissolve it in water, wherein the solid-liquid ratio of tin nitrate to water is 1g: 20-40 mL, and then add citric acid CA and continue stirring; then add a certain amount of EDTA, and add ammonia water to adjust the pH value to 6.5-7; wherein the molar ratio of EDTA to citric acid CA and metal cation is 1:1.5:1.
[0020] S2. Place the beaker in a water bath at a constant temperature of 70-90°C and a rotation speed of 10 r / min. After the solution becomes gelatinous, place the beaker in a 210°C drying oven for 2-4 hours until it is completely dry.
[0021] S3. Grind the dried material in a mortar for 45 min, then put it into a ceramic crucible, and place it in a muffle furnace for pre-sintering at 550°C for 5-7 h. After pre-sintering, grind it again in a mortar for 30-60 min, and then sinter it at 500°C-800°C for 8-12 h, preferably, sinter it at 500°C-600°C. After sintering, grind it again in a mortar for 30-60 min to obtain SnO2 powder.
[0022] The present invention also aims to provide a LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -Semiconductor ion fuel cells based on SnO2-based composite electrolyte materials.
[0023] In the present invention, the electrode material of the semiconductor ion fuel cell is LiNi 0.8 Co 0.15 Al 0.05 O2(NCAL), the LiNi 0.8 Co 0.15 Al 0.05 O2 is obtained by a solid phase mixing method, wherein the sintering temperature after mixing is 810°C and the sintering time is 10 h.
[0024] Specifically, LiNi 0.8 Co 0.15 Al 0.05 The preparation method of O2 includes: (1) According to the ion molar ratio of Li: Ni: Co: Al = 1: 0.8: 0.15: 0.05, weigh a certain amount of lithium hydroxide monohydrate, nickel hydroxide, cobalt oxide and aluminum oxide respectively; put the weighed materials into a ball mill, add an appropriate amount of alcohol so that the grinding balls in the ball mill are submerged by the liquid, and set the speed and time of the ball mill to 280 r / min and 6 h respectively; after the ball milling is completed, absorb the liquid in the ball mill with a syringe and transfer it to a large beaker, clean the residual material in the ball mill with alcohol again and absorb it into the large beaker, and place the large beaker under a drying lamp for drying, and the drying time is 2-4 h; (2) Grind the dried solid material in a mortar manually for about 30 to 60 minutes, then pour the ground material into a clean crucible and pre-sinter it in a muffle furnace; the pre-sintering temperature and pre-sintering time are 450 to 550 °C and 4 to 6 hours, respectively; (3) The pre-sintered material was placed in a mortar and ground manually again. After 30 to 60 min, the powder was placed in a crucible again and sintered again using a muffle furnace. The sintering temperature and time were set to 810 °C and 10 h, respectively.
[0025] Compared with the prior art, the present invention has the following advantages: In the present invention, the lithium battery positive electrode material LiNi is firstly 0.8 Co 0.1 Mn 0.1 O 2-δ By introducing SIFC electrolyte and utilizing the unique lithium insertion properties of SnO2, Li + Directly introduced into the electrolyte, when the battery is working, H2 will reduce the NCAL anode and the LiNi on the anode side. 0.8 Co 0.1 Mn 0.1 O 2-δ , and eventually a large amount of Li2CO3 / LiOH complex is generated in the electrolyte; since the battery operating temperature is greater than the melting point of the Li2CO3 / LiOH complex 419°C, the complex is in a molten state, which can greatly improve the ionic conductivity and density of the electrolyte.
[0026] At the same time, LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The PN heterostructure formed at the interface with SnO2, the space charge layer of the PN junction can effectively promote the 2- and H + while inhibiting the conduction of electrons.
[0027] The P-type semiconductor LiNi with the best ratio designed by the present invention 0.8 Co 0.1 Mn 0.1 O 2-δ The SnO2-based electrolyte composite material with an N-type semiconductor is used as the electrolyte for a solid fuel cell, which achieves an excellent maximum power density of 1169 mW / cm at 550°C. 2 , open circuit voltage (OCV) is 1.15 V, ohmic resistance (R0) is 0.14 Ω·cm 2 , than pure LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The single cell power of the electrolyte (433 mW·cm -2 ) increased by 2.7 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is LiNi0.8 Co 0.1 Mn 0.1 O 2-δ XRD patterns of (NCML811) sintered at 700℃, 800℃, 900℃ and 1000℃ for 10h respectively.
[0029] Figure 2 (a) LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ (NCML811), SnO2 and 7 LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -3SnO2 XRD spectrum; (b) XRD spectrum of mixed electrolytes with different proportions.
[0030] Figure 3 (a) IV / IP curve of a single cell with SnO2 as electrolyte after multiple reverse connection at a test temperature of 550℃; (b) EIS curve.
[0031] Figure 4 (a) is LiNi with different mass ratios 0.8 Co 0.1 Mn 0.1 O 2-δ IV / IP curves of the battery with (NCML811) and SnO2-based electrolyte composite at 550℃; (b) 7LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ :3IV / IP curve of a single cell with SnO2 as electrolyte at a test temperature of 400-550℃; (c) 0.8 Co 0.1 Mn 0.1 O 2-δ The IV / IP of the single cell made of electrolyte is tested at a temperature of 450-550°C.
[0032] Figure 5 LiNi with different mass ratios 0.8 Co 0.1 Mn 0.1 O 2-δ EIS curves of the battery composed of (NCML811) and SnO2-based electrolyte at 550℃.
[0033] Figure 6 It is LiNi with a mass ratio of 7:3 0.8 Co 0.1 Mn 0.1 O2-δ (NCML811): Ionic conductivity of SnO2 electrolyte and NCML811 electrolyte.
[0034] Figure 7 TG and DSC diagrams of 7NCML811:3SnO2 before and after the test, (a) before the test; (b) after the test.
[0035] Figure 8 It is LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ UV spectra and band gap diagrams of (NCML811) and SnO2, where (a) LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ ; (b) SnO2.
[0036] Fig. 9 It is LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Energy band diagram of PN heterojunction of (NCML811) and SnO2. DETAILED DESCRIPTION
[0037] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0039] Example 1 1. Synthesize P-type semiconductor LiNi using high temperature solid phase method 0.8 Co 0.1 Mn 0.1 O 2-δ Electrolyte material, the specific preparation method is as follows: (1) Weigh a certain amount of Li2CO3, NiO, Co3O4 and Mn2O3 according to the element ratio and place them in a ball mill. Add an appropriate amount of anhydrous ethanol to the ball mill so that the grinding balls in the ball mill are submerged in the liquid. Set the speed and time to 260 r / min and 6 h respectively.
[0040] (2) Use a needle to suck out the mixed raw materials in the ball mill into a beaker and place it under a heating lamp to dry the anhydrous ethanol. After drying, grind it in a mortar for 45 minutes and then pre-calculate it in a muffle furnace at 500℃ for 5 hours.
[0041] (3) After pre-sintering, grind it again in a mortar for 1 h, and then sinter it at 700℃, 800℃, 900℃, and 1000℃ for 10 h. After sintering, grind it again in a mortar for 1 h to obtain P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Electrolyte powder.
[0042] like Figure 1 LiNi is prepared by high temperature solid phase method 0.8 Co 0.1 Mn 0.1 O 2-δ XRD patterns of sintering at 700℃, 800℃, 900℃, and 1000℃ for 10 h. As shown in the figure, when the sintering temperature is 700℃, there are more impurities compared with the standard card PDF#85-1966. When the sintering temperature is 800℃, the impurities disappear. At this time, the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The crystallinity is good, forming an α-NaFeO type layered structure. When the sintering temperature is further increased to 900 ° C, the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The crystallinity of LiNi was further improved. The sintering temperature was raised to 1000℃ again, and a complete P-type semiconductor LiNi was formed. 0.8 Co 0.1 Mn 0.1 O 2-δ phase, but the crystallinity of the material is lower than that at 900℃, so LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The minimum and optimal phase formation temperatures are 800℃ and 900℃ respectively.
[0043] 2. Prepare N-type semiconductor SnO2. The preparation method is as follows: S1. Add tin nitrate into a container, and then place it on a magnetic stirrer to fully stir and dissolve it in water, wherein the solid-liquid ratio of tin nitrate to water is 1g:30 mL, and then add citric acid CA and continue stirring; then add a certain amount of EDTA, and add ammonia water to adjust the pH value to 7; wherein the molar ratio of EDTA to citric acid CA and metal cation is 1:1.5:1.
[0044] S2. Place the beaker in a water bath at a constant temperature of 80°C and a rotation speed of 10 r / min. After the solution becomes gelatinous, place the beaker in a drying oven at 210°C for 3 hours until it is completely dry.
[0045] S3. Grind the dried material in a mortar for 45 min, then put it into a ceramic crucible and pre-sinter it in a muffle furnace at 550°C for 6 h. Grind it again in a mortar for 45 min after pre-sintering, and then sinter it at 600°C for 10 h. Grind it again in a mortar for 45 min after sintering to obtain SnO2 powder.
[0046] 3. Synthesize P-type semiconductor LiNi by solid-phase solid-phase mixing method 0.8 Co 0.1 Mn 0.1 O 2-δ The specific preparation method of the composite electrolyte with N-type semiconductor SnO2 is as follows: (1) Weigh LiNi with a balance according to different mass ratios (9:1, 8:2, 7:3, 6:4) 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2 and placed in a ball mill respectively; add an appropriate amount of anhydrous ethanol to the ball mill so that the grinding balls in the ball mill are submerged by the liquid, and set the speed and time to 180 r / min and 6 h respectively.
[0047] (2) Use a syringe to suck out the evenly mixed raw materials in the ball mill into a beaker, and place it under a baking lamp to dry the anhydrous ethanol; after drying, grind it in a mortar for 45 minutes and then place it in a muffle furnace for sintering at 600℃ for 5 hours.
[0048] (3) After sintering, grind again in a mortar for 45 min to obtain P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Electrolyte and N-type semiconductor SnO2-based composite electrolyte materials.
[0049] like Figure 2 It is a P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O2-δ , SnO2 and LiNi with different mass ratios 0.8 Co 0.1 Mn 0.1 O 2-δ The XRD spectrum of SnO2 and P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The XRD patterns of the two materials after mechanical mixing in a ball mill and sintering at 600℃ for 5 h in a muffle furnace completely correspond to those of the single material, with no new peaks and obvious phase structure changes, indicating that the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ It has good chemical compatibility and does not react with SnO2 in air at 600℃. 4. Synthesis of LiNi by high temperature solid phase method 0.8 Co 0.15 Al 0.05 O2 (NCAL) electrode material, the specific preparation method is as follows: (1) According to the ion molar ratio of Li: Ni: Co: Al = 1: 0.8: 0.15: 0.05, weigh a certain amount of lithium hydroxide monohydrate, nickel hydroxide, cobalt oxide and aluminum oxide respectively. Put the weighed materials into a ball mill, add an appropriate amount of alcohol so that the grinding balls in the ball mill are submerged by the liquid, and set the speed and time to 260 r / min and 6 h respectively. After the ball milling is completed, the liquid in the ball mill is sucked out with a syringe and transferred to a large beaker. The residual material in the ball mill is properly cleaned with alcohol again and sucked into the large beaker. The large beaker is placed under a drying lamp for drying for 3 hours.
[0050] (2) Grind the dried solid material in a mortar manually for about 45 min, then pour the ground material into a clean crucible and pre-sinter it in a muffle furnace at a temperature of 500 °C and a time of 5 h.
[0051] (3) The pre-sintered material was placed in a mortar and ground manually again. After 45 min, the powder was placed in a crucible again and sintered again in a muffle furnace at a sintering temperature of 810 °C and a sintering time of 10 h. NCAL powder was obtained by grinding again.
[0052] 5. Preparation of electrodes. The specific steps are as follows: (1) According to a certain ratio, weigh 10 g of NCAL powder and 0.05 g of PVB in a mortar, mix thoroughly, and then add 2 mL of anhydrous ethanol and 3 mL of pinene alcohol; (2) Use a punch to punch out a nickel foam disc, and evenly apply the slurry prepared in (1) on the nickel foam disc; the area of the punch is 0.64 cm 2 , the thickness of nickel foam is 1.2 mm.
[0053] (3) Wrap the coated nickel foam with tin foil and place it in a 120°C drying oven for 24 min. Repeat the above operation twice, brush the surface of the nickel foam to give it a metallic luster, and then place it in a drying oven to dry, finally obtaining a porous symmetrical electrode material Ni-NCAL, wherein the drying temperature and drying time are 120°C and 30 min, respectively.
[0054] 6. Preparation of single cell In this example, Ni–NCAL|LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2|Ni–NCAL single cell preparation, the specific steps are as follows: (1) Place the prepared electrode into the bottom of the mold for making the battery. The effective working area of the electrode is 0.64 cm 2 .
[0055] (2) Weigh an appropriate amount (0.32 g) of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ or LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2 is the electrolyte placed on the bottom NCAL electrode and compacted with a mold.
[0056] (3) Then place an NCAL electrode on top of the mold to make the battery.
[0057] (4) Place the mold into a tablet press to connect the electrodes and electrolyte together to obtain a single cell.
[0058] (5) Place the prepared single cell into the test battery fixture and start testing.
[0059] 7. Performance Testing Figure 3(a) IV / IP curve (b) EIS curve of a single cell with SnO2 as electrolyte at 550℃. The maximum output power density of the battery at 550℃ increases with the number of tests, while the impedance decreases. To our surprise, the maximum output power density of the battery reached 800 mW / cm after the third test. 2 This should be the result of the unique lithium insertion property of SnO2. At 550℃, H2 will reduce NCAL to generate Li + Due to the potential difference between the electrode and the electrolyte, Li + It will diffuse into the SnO2 electrolyte and react with SnO2 to form lithium oxide. Lithium oxide then reacts with CO2 and H2O to form Li2CO3 / LiOH complex. At 550°C, the Li2CO3 / LiOH complex is in a molten state, which greatly improves the ionic conductivity of the electrolyte and reduces the activation energy and polarization resistance of the electrode reaction, thereby greatly improving the MPD of the battery.
[0060] Figure 4 (c) shows the fuel cell preheated at 550 °C for 30 min to perform a single-cell Ni-NCAL|LiNi 0.8 Co 0.1 Mn 0.1 O 2−δ |Ni-NCAL electrochemical performance (IV / IP) test and electrochemical impedance spectroscopy (EIS) test Figure 5 As shown in the figure, the open circuit voltages of 0.676 V, 0.756 V, 0.657 V and the open circuit voltage of 432.81 mW / cm2 were obtained at 550℃, 500℃, and 450℃, respectively. 2 、325.00 mW / cm 2 、285.94 mW / cm 2 MPD, it is obvious that the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ As an electrolyte alone, the open circuit voltage is low at several temperatures, which is attributed to the 0.8 Co 0.1 Mn 0.1 O 2-δ The electrolyte has a certain electronic conductivity, which ultimately leads to a relatively low MPD. From the EIS test results, the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The impedance of the electrolyte is relatively large, so the P-type semiconductor LiNi 0.8Co 0.1 Mn 0.1 O 2-δ It is less feasible as a SOFC electrolyte alone.
[0061] In order to reduce the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The electronic conductivity in the electrolyte was designed with different mass ratios of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Composite with SnO2-based electrolyte, using LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The PN heterostructure formed between SnO2 and O 2− and H + Then, in order to explore the different mass ratios of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Electrochemical performance (IV / IP) test of batteries with SnO2-based composite as electrolyte at 550°C ( Figure 4 (a)), electrochemical impedance spectroscopy (EIS) Figure 5 As shown. 0.8 Co 0.1 Mn 0.1 O 2-δ Compared with electrolyte, P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The MPD of SnO2 composite electrolytes has been significantly improved. With the increase of the mass proportion of SnO2 in the composite electrolyte, the MPD shows a trend of first increasing and then decreasing. Figure 4 (ac) and Figure 5 As shown, the optimal ratio of 7LiNi designed by the invention 0.8 Co 0.1 Mn 0.1 O 2-δ -3SnO2-based electrolyte composite material, single cell achieved an excellent maximum power density of 1169 mW / cm at 550°C 2 , open circuit voltage (OCV) is 1.15 V, ohmic resistance (R0) is 0.14Ω·cm 2 , compared with LiNi 0.8 Co 0.1 Mn 0.1O 2-δ The single cell power of the electrolyte (433 mW·cm -2 ) increased by 169%, the optimal ratio of 7LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -3SnO2 composite electrolyte values rank among the best in non-ceria-based electrolytes. This shows that in the P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The composite with N-type semiconductor SnO2-based electrolyte in different mass ratios can effectively increase the open circuit voltage and solve the battery short circuit problem.
[0062] Figure 6 It is 7LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ : The conductivity of 3SnO2 and NCML811 electrolyte at 550-400℃. The conductivity here is derived from the slope of the I-V curve. We all know that the linear part of the I-V curve belongs to the ohmic loss of the electrolyte, so the ohmic resistance of the electrolyte can be obtained by calculating the slope, and then the 7LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ :3SnO2 and NCML811 electrolyte battery total ionic conductivity. The above formula is used to calculate the 7LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The ionic conductivity of 3SnO2 electrolyte at 550℃, 500℃, 450℃ and 400℃ are 0.162 S / cm, 0.117 S / cm, 0.107 S / cm and 0.022 S / cm respectively, and that of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The ionic conductivity of the electrolyte at 550℃, 500℃, 450℃, and 400℃ are 0.060 S / cm, 0.041 S / cm, 0.030 S / cm, and 0.016 S / cm, respectively. 0.8 Co 0.1 Mn 0.1 O 2-δ :3SnO2 electrolyte ion conductivity is significantly higher than LiNi 0.8 Co 0.1 Mn 0.1 O2-δ Electrolytes.
[0063] Figure 7 7LiNi before and after the test 0.8 Co 0.1 Mn 0.1 O 2-δ :3SnO2 electrolyte was subjected to TG-DSC test, and combined with the above analysis of Li2CO3 / LiOH complex, Li2CO3 / LiOH complex was in molten state above 419℃, and the molten Li2CO3 / LiOH complex could significantly improve the ionic conductivity of the electrolyte. However, when the temperature dropped from 450℃ to 400℃, the molten Li2CO3 / LiOH complex gradually turned into solid state, and the solid Li2CO3 / LiOH complex was an insulator that blocked the conduction of ions in the electrolyte, resulting in a sudden drop in MPD, while the open circuit voltage and the electrolyte ohmic impedance both rose sharply.
[0064] Figure 8 (a, b) are LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ UV spectrum and band gap diagram of LiNi and SnO2. 0.8 Co 0.1 Mn 0.1 O 2-δ It belongs to P-type semiconductor and SnO2 belongs to N-type semiconductor. When the two materials are compounded, charge redistribution will occur at the contact interface of the two materials at the battery operating temperature to form a PN junction. The space charge layer of the PN junction can effectively promote the conduction of oxygen ions and protons while inhibiting the conduction of electrons.
[0065] For LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ UV test with SnO2, the results are as follows Figure 8 shown.
[0066] According to the following formula, we can calculate LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The band gaps of SnO2 are 1.60 eV and 3.86 eV respectively.
[0067] LiNi is plotted based on the bandgap width of the two materials. 0.8 Co 0.1 Mn 0.1 O 2-δThe PN heterojunction energy band diagram with SnO2 and the model schematic diagram are as follows Fig. 9 shown.
[0068] Comparative Example 1 In this embodiment, the single cell is Ni-NCAL|SrFe 0.2 Ti 0.8 O 3-δ -ZnO|Ni-NCAL.
[0069] The preparation methods of the electrolyte, the electrode and the single cell are the same as those in Example 1.
[0070] The only difference is that in this embodiment, the electrolyte material is SrFe 0.2 Ti 0.8 O 3-δ Composite materials with ZnO, in which SrFe 0.2 Ti 0.8 O 3-δ The mixing ratio with ZnO is 1:1.
[0071] After testing, the maximum power density of the single cell prepared in this embodiment at 520°C is 650 mW·cm -2 .
[0072] Comparative Example 2 In this embodiment, the single cell is Ni-NCAL|SrFe 0.2 Ti 0.8 O 3−δ -SnO2|Ni-NCAL.
[0073] The preparation methods of the electrolyte, the electrode and the single cell are the same as those in Example 1.
[0074] The only difference is that in this embodiment, the electrolyte material is SrFe 0.2 Ti 0.8 O 3−δ Composite materials with SnO2, in which SrFe 0.2 Ti 0.8 O 3−δ The mixing ratio with SnO2 is 6:4.
[0075] After testing, the maximum power density of the single cell prepared in this embodiment can reach 1004 mW / cm at 550°C. 2 .
[0076] Comparative Example 3 In this embodiment, the single cell is Ni-NCAL|Gd 0.15 Ni 0.05 Ce 0.8 O 2-δ-SnO2|Ni-NCAL. The preparation methods of the electrolyte, the electrode and the single cell are the same as those in Example 1.
[0077] The difference is that in this embodiment, the electrolyte material is LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ Composite materials with SnO2, in which LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mixing ratio with SnO2 is 7:3.
[0078] After testing, the maximum power density of the single cell prepared in this embodiment at 550°C is 879.4 mW cm -2 .
[0079] Comparative Example 4 In this embodiment, the single cell is Ni-NCAL|LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2|Ni–NCAL.
[0080] The preparation methods of the electrolyte, electrodes and single cells are basically the same as those in Example 1.
[0081] The difference is that in this embodiment, the SnO2 used in the electrolyte material is prepared by thermal decomposition: S1. Weigh a certain amount of tin nitrate (Sn(NO3)2) into an alumina ceramic crucible. S2. Place in a Ma Furnace and calcine at 500~600℃ for 3~6 hours.
[0082] S3. Then grind in a mortar for 1 h to obtain SnO2 powder.
[0083] In this embodiment, LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mixing ratio with SnO2 is 7:3.
[0084] After testing, the maximum power density of the single cell prepared in this embodiment at 550°C is 1021 mW·cm -2 .
[0085] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0086] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2-based composite electrolyte material, characterized in that The composite electrolyte material is used as an electrolyte for a semiconductor ion fuel cell. The composite electrolyte material is composed of LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2, the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mass ratio of SnO2 is 6~9:1~4.
2. LiNi according to claim 1 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2-based composite electrolyte material, characterized in that The LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The mass ratio of SnO2 is 6~8:2~4.
3. LiNi according to claim 1 0.8 Co 0.1 Mn 0.1 O 2-δ , SnO2 electrolyte material, characterized in that, The LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2 were synthesized by high temperature solid phase method and sol-gel method respectively.
4. LiNi according to any one of claims 1 to 3 0.8 Co 0.1 Mn 0.1 O 2-δ -A method for preparing a SnO2-based composite electrolyte material, characterized in that: The following steps are involved: (1) Weigh LiNi according to the mixing mass ratio 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2; (2) LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ and SnO2 are placed in a ball mill, and anhydrous ethanol is added for ball milling and mixing to obtain a mixed slurry; (3) drying the mixed slurry to remove anhydrous ethanol to obtain a dried mixed slurry; (4) The dried mixed slurry is subjected to primary grinding, sintering, and secondary grinding to obtain LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ -SnO2-based composite electrolyte materials.
5. The preparation method according to claim 4, characterized in that: In step (1), the rotation speed of the ball mill is 150-200 r / min, and the ball milling time is 5-7 h. In step (3), the mixed slurry is placed under a heating lamp for drying, and the drying time is 2-4 h. In step (4), the first grinding time is 30-60 min, the sintering temperature is 550-650°C, the sintering time is 4-6 h, and the second grinding time is 30-60 min.
6. The preparation method according to claim 4, characterized in that: In step (1), the LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ The preparation method comprises: S1. Weigh the raw materials Li2CO3, NiO, Co3O4 and Mn2O3 according to the element ratio and place them in a ball mill. Add anhydrous ethanol and set the speed and time to 180-280 r / min and 5-7 h respectively. S2. Suck out the evenly mixed raw materials in the ball mill, place them under a heating lamp to dry the anhydrous ethanol; after drying, grind them in a mortar for 30-60 min, and then pre-calculate them in a muffle furnace at 500-550°C for 4-6 h; S3, after pre-sintering, grind again in a mortar for 30-60 min, then sinter at 700-1000 °C for 8-12 h; grind again in a mortar for 30-60 min after sintering to obtain a P-type semiconductor LiNi 0.8 Co 0.1 Mn 0.1 O 2-δ powder.
7. A LiNi containing any one of claims 1 to 3 0.8 Co 0.1 Mn 0.1 O 2-δ -Semiconductor ion fuel cells based on SnO2-based composite electrolyte materials.
8. The semiconductor ion fuel cell according to claim 7, characterized in that: The electrode material of the battery is LiNi 0.8 Co 0.15 Al 0.05 O 2-δ , the LiNi 0.8 Co 0.15 Al 0.05 O 2-δ It is obtained by a solid phase mixing method, wherein the sintering temperature after mixing is 810°C and the time is 10 h.