All-solid-state negative-electrode-free sodium ion battery and preparation method thereof
By using hard carbon coating and solid electrolyte layer in all-solid negative electrode-free sodium ion batteries, the chemical reactivity and volume expansion problems of Na metal negative electrodes in sodium ion batteries are solved, high energy density and long cycle life are achieved, and the Battery safety and market application prospects.
Patent Information
- Application Number
- CN202411008994.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
Existing sodium ion batteries have been subjected to branch crystal growth, cycle life and safety due to the high chemical reactivity and volume expansion of Na metal negative electrodes. There are few researches on sodium ion batteries without negative electrodes, especially in liquid conditions due to uneven Na deposition. The SEI layer ruptures and the battery life is reduced.
The all-solid state negative-electrode sodium ion battery structure is adopted, and the hard carbon coating and positive electrode active material are coated on the surface of the metal foil, combined with the solid electrolyte layer, the sodium ion deposition and electrochemical performance are controlled, and the cost is reduced and safety is improved.
It realizes a sodium ion battery with high energy density, long cycle life, high safety and low cost. It buffers sodium ion deposition and expansion, inhibits branch crystal growth, and improves the circulation performance and safety of the battery.
Smart Images

Figure CN118943469A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to an all-solid-state negative-electrode-free sodium-ion battery and a preparation method thereof. Background Art
[0002] The continuous growth of fossil fuel consumption has led to an urgent crisis of energy insecurity and climate change. Cost-effective and reliable energy storage technology is a key enabler for the seamless integration of fluctuating intermittent renewable energy sources to offset fossil fuel consumption. As a viable alternative to the ubiquitous lithium-ion battery, sodium-ion batteries have the advantages of abundant and cheap sodium resources, a wide variety of sodium-based solid phases, and an ultra-high theoretical capacity (1165 mA hg -1 ) and low electrode potential (-2.714Vvs.SHE), and therefore is considered to be an ideal candidate for large-scale, low-cost energy storage systems.
[0003] Sodium-ion batteries using sodium metal anodes can achieve energy densities comparable to those of the most advanced lithium-ion batteries. However, the practical application of Na metal anodes is hampered by two major challenges related to cyclability and safety, mainly due to their high chemical reactivity and huge volume expansion, which ultimately leads to the uncontrolled growth of Na dendrites. At the same time, the high cost of the preparation and coating process of Na metal foil has seriously hindered the promotion and application of sodium-ion batteries. At present, people use hard carbon to replace the direct use of sodium metal as the anode to improve the cycle life and safety of sodium-ion batteries. However, due to the high preparation cost of hard carbon and the high charge and discharge platform of hard carbon, the energy density of the full battery prepared in combination with the positive electrode is greatly reduced. Therefore, the development of highly safe anode-free sodium-ion batteries is imminent. However, there are few studies on anode-free sodium-ion batteries, and all of them focus on liquid anode-free sodium-ion batteries. In liquid anode-free sodium-ion batteries, due to the uneven deposition of Na on the current collector, the internal stress of the electrode increases, resulting in the rupture of the SEI layer. The broken SEI shortens the service life of the battery. The development of all-solid-state negative electrode-free sodium-ion batteries can solve this problem. Summary of the invention
[0004] The object of the present invention is to provide a negative electrode-free sodium ion battery with high battery energy density, controllable sodium volume and dendrite growth, long cycle life, high safety and low cost.
[0005] To achieve the above-mentioned purpose, the present invention proposes an all-solid-state sodium ion battery without negative electrode, comprising a positive electrode collector, a negative electrode collector and a solid electrolyte layer, wherein the solid electrolyte layer is arranged between the positive electrode collector and the negative electrode collector; the positive electrode collector is prepared by coating a positive electrode slurry on the surface of a first current collector, and the negative electrode collector is prepared by coating a hard carbon coating on the surface of a second current collector; the positive electrode slurry comprises a positive electrode active material, and the mass ratio of the hard carbon coating to the positive electrode active material is 1:20-50.
[0006] Furthermore, the first current collector and the second current collector are metal foils; preferably, the first current collector is aluminum foil; preferably, the second current collector is any one of copper foil, zinc foil and aluminum foil.
[0007] Furthermore, the thickness of the first current collector is 6-60 μm, and the thickness of the second current collector is 0.01-1 mm.
[0008] Further, the positive electrode active material, the conductive agent and the binder are mixed evenly in a mass ratio of 7-10:1-2:1-2, and then a solvent is added and mixed to obtain a positive electrode slurry;
[0009] Preferably, the positive electrode active material is Na3V2(PO4)3, Na4Fe3(PO4)2(P2O7), Na3Fe2(PO4)3, Na2Fe(SO4)2 and NaMn 1 / 3 Ni 1 / 3 Cu 1 / 3 Fe 1 / 3 One or more of O2;
[0010] Preferably, the conductive agent is any one or more of acetylene black, Ketjen black, carbon nanotubes, carbon nanofibers, and graphene;
[0011] Preferably, the adhesive is any one or more of sodium carboxymethyl cellulose, polyvinylidene fluoride, polytetrafluoroethylene, fluorinated rubber, polyurethane, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, alginic acid, sodium alginate, and styrene-butadiene rubber;
[0012] Preferably, the solvent is any one or more of N-methylpyrrolidone, dimethylformamide, and dimethyl sulfoxide solvents.
[0013] Furthermore, the hard carbon coating is prepared by mixing hard carbon and polyvinylidene fluoride in a mass ratio of 7-15:1, adding an appropriate amount of N-methylpyrrolidone and dissolving them uniformly.
[0014] Further, the solid electrolyte includes a polymer, an ether molecule, a sodium salt, and a binder;
[0015] Preferably, the polymer is any one or more of polyethylene oxide, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene), and polyethylene glycol;
[0016] Preferably, the ether molecule is one or both of diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether;
[0017] Preferably, the sodium salt is any one or more of NaClO4, sodium hexafluorophosphate or sodium bis(fluorosulfonyl)imide;
[0018] Preferably, the binder is sodium carboxymethylcellulose.
[0019] Furthermore, the hard carbon coating thickness is only 1-10 μm.
[0020] Furthermore, the mass ratio of the polymer, the ether molecule, the sodium salt and the adhesive is 30-90:10-50:1-20:1-20.
[0021] Furthermore, the solid electrolyte has a thickness of 10-120 μm.
[0022] The second aspect of the present invention provides a preparation method for preparing the all-solid-state negative electrode-free sodium ion battery provided in the first aspect of the present invention, comprising the steps of:
[0023] The positive electrode current collector, the solid electrolyte layer and the negative electrode current collector are stacked and packaged in sequence to prepare a sodium ion battery;
[0024] The positive electrode current collector is prepared by soaking the first current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with positive electrode slurry to obtain the positive electrode current collector;
[0025] The negative electrode current collector is prepared by soaking the second current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with a hard carbon coating to obtain the negative electrode current collector;
[0026] Preferably, the concentration of the acid solution is 0.01M-0.5M; preferably, the soaking time is 0.1-10h; preferably 0.5h, and the drying temperature is 50-120°C;
[0027] The solid electrolyte layer is prepared by mixing a polymer, an ether molecule, a sodium salt and an adhesive, adding water and mixing evenly to obtain a mixed solution, pouring the mixed solution on a plate, and drying to obtain a solid electrolyte layer.
[0028] The first current collector and the second current collector are both metal foils, and the purpose of soaking them in acid is to remove the oxide layer on the surface of the metal foil. As a semiconductor, the oxide layer on the surface of the metal foil will reduce the electronic conductivity, increase the polarization of the battery, and affect the safety and service life of the battery. At the same time, acid treatment of the first current collector and the second current collector can increase the surface roughness of the current collector, which can prevent the positive electrode slurry, hard carbon coating and sodium metal from falling off. However, it is not suitable to soak for a long time, and excessive etching of the metal foil will also affect the interface contact.
[0029] A hard carbon coating is applied on the surface of the second current collector to prepare the negative electrode of the battery. The hard carbon is used as a nucleation site instead of as a negative electrode. Compared with using hard carbon directly as a negative electrode, the present invention uses a hard carbon coating with a thickness of only 1-10 μm applied on the surface of the metal foil, which reduces the cost and improves the energy density of the battery. The second current collector is a metal foil, which can be any one of zinc foil, copper foil and aluminum foil. Through the adsorption energy generated between the second current collector and the sodium ions, the sodium ions can be evenly deposited on the surface of the negative electrode current collector during the battery cycle. Among them, the capacity, cycle life and safety of the battery are the best when zinc foil is used as the second current collector.
[0030] The full battery prepared in the present invention, which is composed of a negative electrode current collector, a negative electrode side hard carbon coating, a positive electrode current collector, a positive electrode active material coating and a low-cost solid electrolyte layer, can provide excellent electrochemical performance. The negative electrode side of the battery does not need to be placed with sodium metal in advance. During the battery cycle, a sodium metal layer with a thickness of 0.5-10 μm is uniformly deposited on the surface of the hard carbon coating on the negative electrode current collector, so a separate sodium plating process is not required, which can effectively reduce the mass of the negative electrode side and improve the energy density and power density of the negative electrode-free sodium ion battery.
[0031] By formulating and combining the solid electrolyte, the negative electrode current collector and the positive electrode material, the all-solid-state negative electrode-free sodium ion battery of the present invention performs well in terms of capacity, cycle life and safety, effectively buffers the volume expansion caused by the deposition of sodium ions on the surface of the negative electrode current collector during the cycle, improves the cycle performance of the battery, and effectively inhibits the growth of sodium metal dendrites, solving the problem of reduced battery cycle life and safety caused by the growth of dendrites in sodium ion batteries.
[0032] The all-solid-state negative electrode-free sodium ion battery of the present invention has a capacity retention rate of 70-95% after 100 charge and discharge cycles at 1C.
[0033] In summary, the preparation method of the negative electrode-free all-solid-state sodium ion battery provided by the present invention is easy to realize industrial production. The prepared negative electrode-free all-solid-state sodium ion battery has excellent cycle performance, energy density and power density, and its safety is improved, and it has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the charge and discharge curve of the all-solid-state sodium ion battery at 0.1C in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those who do not indicate the manufacturer of the reagents or instruments used are all conventional products that can be obtained commercially. In the following embodiments, if not clearly stated, "%" refers to weight percentage.
[0036] The preparation method of the all-solid-state negative electrode-free sodium ion battery in the present invention is:
[0037] The positive electrode current collector, the solid electrolyte layer and the negative electrode current collector are stacked and packaged in sequence to prepare a sodium ion battery.
[0038] The positive electrode current collector is prepared by soaking the first current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with positive electrode slurry to obtain the positive electrode current collector;
[0039] The negative electrode current collector is prepared by soaking the second current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with a hard carbon coating to obtain the negative electrode current collector;
[0040] The solid electrolyte layer is prepared by mixing polymer, ether molecules, sodium salt and adhesive in proportion, adding water to mix well to obtain a mixed solution, pouring the mixed solution on a plate, and drying to obtain a solid electrolyte layer.
[0041] Preferably, the acid concentration is 0.01M-0.5M.
[0042] Preferably, the soaking time is 0.5-10h.
[0043] Preferably, the drying temperature is 50-120°C.
[0044] The plate is a corrosion-resistant and high-temperature-resistant material, which is commercially available. The present invention selects a polytetrafluoroethylene plate as the casting plate.
[0045] Hard carbon is carbon that is difficult to graphitize even at 2500° C. or higher. The hard carbon in the present invention is any commercially available hard carbon.
[0046] Embodiment 1:
[0047] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0048] After mixing hard carbon and polyvinylidene fluoride at a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, coated on the surface of the second current collector, and vacuum dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0049] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The thickness of the prepared solid electrolyte film is 95μm.
[0050] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0051] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0052] The sodium ion battery prepared in Example 1 was tested, and the results were as follows: Figure 1 As shown, Figure 1 The charge and discharge curve of the all-solid-state sodium ion battery in Example 1 of the present invention at 0.1C. The discharge capacity at 0.1C is 98.5 mAh g -1 , after 100 charge and discharge cycles at 1C, the capacity retention rate is 94.2%;
[0053] Embodiment 2:
[0054] A copper foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0055] After mixing hard carbon and polyvinylidene fluoride at a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100°C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0056] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The thickness of the prepared solid electrolyte film is 95μm.
[0057] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0058] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0059] Embodiment 3:
[0060] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0061] After mixing hard carbon and polyvinylidene fluoride at a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100°C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0062] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0063] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0064] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0065] Embodiment 4:
[0066] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 0.05 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0067] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0068] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, the preset time range being 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0069] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0070] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0071] Embodiment 5:
[0072] Aluminum foil with a thickness of 0.1 mm was selected as the second current collector, and aluminum foil with a thickness of 50 μm was selected as the first current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. Then, after ultrasonically cleaning with distilled water for 30 minutes, it was ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0073] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0074] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0075] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0076] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0077] Embodiment 6:
[0078] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0079] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0080] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 50:30:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0081] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0082] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0083] Embodiment 7:
[0084] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0085] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0086] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 70:10:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0087] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0088] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0089] Embodiment 8:
[0090] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0091] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0092] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, the preset time range being 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0093] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 7:1:2, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0094] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0095] Embodiment 9:
[0096] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0097] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0098] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, the preset time range being 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0099] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 7:2:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0100] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0101] Embodiment 10:
[0102] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0103] After mixing hard carbon and polyvinylidene fluoride in a ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0104] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, the preset time range being 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0105] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 20 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0106] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0107] Embodiment 11:
[0108] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0109] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0110] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0111] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 30 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0112] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0113] Embodiment 12:
[0114] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0115] After mixing hard carbon and polyvinylidene fluoride in a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, and then coated on the surface of the second current collector and dried in a vacuum drying oven at 100 °C to control the surface loading of hard carbon to 1 mg cm -2 , and obtain the negative electrode current collector.
[0116] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. The temperature in the vacuum drying oven is then adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The prepared solid electrolyte film has a thickness of 95μm.
[0117] NaMn 1 / 3 Ni 1 / 3 Cu 1 / 3 Fe 1 / 3 O2, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the active material surface loading was controlled to be 25 mg cm-2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0118] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0119] The negative electrodes prepared in the above embodiments were assembled into batteries for testing. Using the LAND CT2001A battery testing system of Wuhan Landian Electronics Co., Ltd., the sodium ion batteries prepared in Examples 1-5 were subjected to constant current charge and discharge tests at 0.1C and 1C current densities at 2.5 to 4.0V, and the cycles were greater than 100 times. The test results are shown in Table 1. From the test results, it can be seen that the energy capacity of the all-solid-state sodium-free battery prepared by the present invention is considerable, and the cycle can be stably cycled for 100 times. Therefore, the present invention can be effectively applied in the preparation of all-solid-state sodium-free batteries with high energy density. Comparative Example 1:
[0120] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0121] Ethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The thickness of the prepared solid electrolyte film is 95μm.
[0122] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0123] On the negative electrode side, the treated zinc foil is directly used as the negative electrode current collector.
[0124] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0125] Comparative Example 2:
[0126] A zinc foil with a thickness of 0.1 mm was selected as the second current collector, and an aluminum foil with a thickness of 50 μm was selected as the first current collector. The first current collector was ultrasonically cleaned with distilled water at 25 kHz for 30 minutes, and then immersed in a 0.05 M hydrochloric acid solution for 8 hours. After ultrasonically cleaned with distilled water for 30 minutes, anhydrous alcohol was used for ultrasonic cleaning at 25 kHz for 30 minutes, and the surfaces of the first and second current collectors were wiped clean, and vacuum dried at 100°C.
[0127] After mixing hard carbon and polyvinylidene fluoride at a mass ratio of 9:1, a small amount of N-methylpyrrolidone was added to dissolve evenly, coated on the surface of the second current collector, and vacuum dried in a vacuum drying oven at 100°C to control the surface loading of hard carbon to 0.1 mg cm -2 , and obtain the negative electrode current collector.
[0128] Polyethylene oxide (PEO), diethylene glycol dimethyl ether, NaClO4 and sodium carboxymethyl cellulose (Na-CMC) are fully mixed in warm water at a mass ratio of 60:20:9:9. Then stir at 80°C until clear and uniform to obtain a mixed solution. The mixed solution is cast on a polytetrafluoroethylene plate and placed in a vacuum drying oven. Then the temperature in the vacuum drying oven is adjusted to 25°C and maintained for a preset time to obtain a solid electrolyte membrane, and the preset time range is 24h. The thickness of the prepared solid electrolyte film is 95μm.
[0129] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and then a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry, which was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and the surface loading of the active material was controlled to be 25 mg cm -2 , and dried in a vacuum drying oven at 80°C to obtain the positive electrode sheet.
[0130] Battery assembly: In a glove box, the zinc foil, solid electrolyte film and positive electrode sheet prepared above are cut into suitable sizes, and solid-state sodium-ion battery cells are prepared by stacking. After packaging, a sodium-ion battery is obtained.
[0131] Table 1. Performance data of negative electrode-free all-solid-state sodium ion battery
[0132]
[0133]
[0134] The battery in Comparative Example 1 uses only the treated zinc foil as the negative electrode current collector. The capacity retention rate of the battery after 100 cycles at 1C is only 10.4%. The battery in Comparative Example 2 controls the surface loading of the hard carbon in the negative electrode current collector to 0.1 mg cm -2 , the capacity retention rate after 100 cycles at 1C is only 23.5%.
[0135] It can be concluded from the above embodiments and comparative examples that when the surface of the negative electrode current collector is not coated with a hard carbon coating or is coated with only a small amount of a hard carbon coating, the capacity retention rate of the battery after 100 cycles at 1C will be greatly reduced, thereby reducing the safety and service life of the battery.
[0136] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. An all-solid-state negative electrode-free sodium ion battery, characterized in that: It includes a positive electrode collector, a negative electrode collector and a solid electrolyte layer, wherein the solid electrolyte layer is arranged between the positive electrode collector and the negative electrode collector; the positive electrode collector is prepared by coating a positive electrode slurry on the surface of a first current collector, and the negative electrode collector is prepared by coating a hard carbon coating on the surface of a second current collector; the positive electrode slurry includes a positive electrode active material, and the mass ratio of the hard carbon coating to the positive electrode active material is 1:20-50.
2. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The first current collector and the second current collector are both metal foils; preferably, the first current collector is aluminum foil; preferably, the second current collector is any one of copper foil, zinc foil and aluminum foil.
3. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The thickness of the first current collector is 30-60 μm, and the thickness of the second current collector is 0.01-1 mm.
4. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The positive electrode active material, the conductive agent and the binder are mixed evenly in a mass ratio of 7-10:1-2:1-2, and then a solvent is added and mixed to obtain a positive electrode slurry; Preferably, the positive electrode active material is Na3V2(PO4)3, Na4Fe3(PO4)2(P2O7), Na3Fe2(PO4)3, Na2Fe(SO4)2 and NaMn 1 / 3 Ni 1 / 3 Cu 1 / 3 Fe 1 / 3 One or more of O2; Preferably, the conductive agent is any one or more of acetylene black, Ketjen black, carbon nanotubes, carbon nanofibers, and graphene; Preferably, the adhesive is any one or more of sodium carboxymethyl cellulose, polyvinylidene fluoride, polytetrafluoroethylene, fluorinated rubber, polyurethane, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, alginic acid, sodium alginate, and styrene-butadiene rubber; Preferably, the solvent is any one or more of N-methylpyrrolidone, dimethylformamide, and dimethyl sulfoxide solvents.
5. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The hard carbon coating is prepared by mixing hard carbon and polyvinylidene fluoride at a mass ratio of 7-15:1, adding a proper amount of N-methylpyrrolidone and dissolving them uniformly.
6. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The solid electrolyte includes a polymer, an ether molecule, a sodium salt and a binder; Preferably, the polymer is any one or more of polyethylene oxide, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene), and polyethylene glycol; Preferably, the ether molecule is one or both of diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; Preferably, the sodium salt is any one or more of NaClO4, sodium hexafluorophosphate or sodium bis(fluorosulfonyl)imide; Preferably, the binder is sodium carboxymethyl cellulose.
7. The all-solid-state negative electrode-free sodium ion battery according to claim 6, characterized in that: The mass ratio of the polymer, the ether molecule, the sodium salt and the adhesive is 30-90:10-50:1-20:1-20.
8. The all-solid-state negative electrode-free sodium ion battery according to claim 1, characterized in that: The solid electrolyte has a thickness of 10-120 μm.
9. A method for preparing the all-solid-state negative electrode-free sodium ion battery according to any one of claims 1 to 8, characterized in that: Includes steps: The positive electrode current collector, the solid electrolyte layer and the negative electrode current collector are stacked and packaged in sequence to prepare a sodium ion battery; The positive electrode current collector is prepared by soaking the first current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with positive electrode slurry to obtain the positive electrode current collector; The negative electrode current collector is obtained by soaking the second current collector in an acid solution, treating it with water and ethanol solution in sequence, drying it, and then coating it with a hard carbon coating; Preferably, the concentration of the acid solution is 0.1M-0.5M; preferably, the soaking time is 0.1-10h; preferably 0.5h, and the drying temperature is 50-120°C; The solid electrolyte layer is prepared by mixing a polymer, an ether molecule, a sodium salt and an adhesive, adding water and mixing evenly to obtain a mixed solution, pouring the mixed solution on a plate, and drying to obtain a solid electrolyte layer.
Citation Information
Cited By
Preparation method of polymer solid electrolyte and negative-electrode-free solid sodium battery
CN119890467A