Negative-electrode-free sodium ion battery and preparation method thereof
By uniformly depositing a sodium metal layer on the metal current collector in an all-solid negative electrode-free sodium ion battery, combining low-cost positive electrode and polymer electrolyte, the cycleability and safety of sodium ion battery are solved, and high energy density and long Life-long battery design reduces cost and improves safety.
Patent Information
- Application Number
- CN202411009009.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The practical application of sodium ion batteries is challenged by cycleability and safety, especially the problems of branch crystal growth caused by the high chemical reactivity and volume expansion of sodium metal negative electrodes. The high preparation cost of hard carbon leads to reduced energy density and short service life. .
Designed with all-solid negative electrode sodium ion battery, by uniformly deposition of sodium metal layer on metal current collector, combining the low-cost Na3V2(PO4)3 positive electrode and polymer electrolyte, buffering volume expansion and inhibiting branch crystal growth, avoiding sodium plating alone Process to improve energy density and power density.
It has achieved high energy density, long cycle life, low cost and high safety negative electrode sodium ion batteries, which are easy to be industrialized and enhance the market application prospects of batteries.
Smart Images

Figure CN118943470A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a negative electrode-free sodium ion battery and a preparation method thereof. Background Art
[0002] The continuous growth of fossil fuel consumption has led to an urgent crisis of energy insecurity and climate change. Cost-effective and reliable energy storage technology is a key enabler for the seamless integration of fluctuating intermittent renewable energy sources to offset fossil fuel consumption. As a viable alternative to the ubiquitous lithium-ion battery, sodium-ion batteries have the advantages of abundant and cheap sodium resources, a wide variety of sodium-based solid phases, and an ultra-high theoretical capacity (1165 mA hg -1 ) and low electrode potential (-2.714Vvs.SHE), and therefore is considered to be an ideal candidate for large-scale, low-cost energy storage systems.
[0003] Sodium-ion batteries using sodium metal anodes can achieve energy densities comparable to those of the most advanced lithium-ion batteries. However, the practical application of Na metal anodes is hampered by two major challenges related to cyclability and safety, mainly due to their high chemical reactivity and huge volume expansion, which ultimately leads to the uncontrolled growth of Na dendrites. At the same time, the high cost of the preparation and coating process of Na metal foil has seriously hindered the promotion and application of sodium-ion batteries. At present, people use hard carbon to replace the direct use of sodium metal as the anode to improve the cycle life and safety of sodium-ion batteries. However, due to the high preparation cost of hard carbon and the high charge and discharge platform of hard carbon, the energy density of the full battery prepared in combination with the positive electrode is greatly reduced. Therefore, the development of highly safe anode-free sodium-ion batteries is imminent. However, there are few studies on anode-free sodium-ion batteries, and all of them focus on liquid anode-free sodium-ion batteries. In liquid anode-free sodium-ion batteries, due to the uneven deposition of Na on the current collector, the internal stress of the electrode increases, resulting in the rupture of the SEI layer. The broken SEI shortens the service life of the battery. The development of all-solid-state negative electrode-free sodium-ion batteries can solve this problem. Summary of the invention
[0004] The object of the present invention is to provide a negative electrode-free sodium ion battery with high battery energy density, controllable sodium volume and dendrite growth, long cycle life, high safety and low cost.
[0005] To achieve the above purpose, a negative electrode-free sodium ion battery comprises a positive electrode and a metal current collector, wherein the positive electrode and the metal current collector are combined to obtain a battery; the positive electrode comprises a positive electrode current collector, a positive electrode slurry and an electrolyte layer, the surface of the positive electrode current collector is pretreated, the positive electrode slurry is coated, and then a layer of electrolyte layer is coated after drying; the electrolyte layer comprises 1wt% of an initiator, 40-55wt% of an epoxy resin monomer, 10-30wt% of an ether molecular monomer, 4wt% of a curing agent and 20-30wt% of a sodium salt.
[0006] Furthermore, the positive electrode current collector and the metal current collector are any one of copper foil, zinc foil and aluminum foil.
[0007] Furthermore, the thickness of the positive electrode current collector and the metal current collector are both 0.01-1 mm.
[0008] Furthermore, the thickness of the electrolyte layer is 10-200 μm.
[0009] Further, the positive electrode slurry includes a positive electrode active material, a conductive agent and a binder in a mass ratio of 7-10:1-2:1-2;
[0010] Preferably, the positive electrode active material is Na3V2(PO4)3, Na4Fe3(PO4)2(P2O7), Na3Fe2(PO4)3, Na2Fe(SO4)2, and NaMn 1 / 3 Ni 1 / 3 Cu 1 / 3 Fe 1 / 3 At least one of O2;
[0011] Preferably, the conductive agent is at least one of acetylene black, Ketjen black, carbon nanotubes, carbon nanofibers, and graphene;
[0012] Preferably, the adhesive is at least one of sodium carboxymethyl cellulose, polyvinylidene fluoride, polytetrafluoroethylene, fluorinated rubber, polyurethane, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, alginic acid, sodium alginate, and styrene-butadiene rubber; more preferably, the adhesive is sodium carboxymethyl cellulose.
[0013] Further, the initiator is at least one of dialkoxyacetophenone, α-hydroxyalkylphenone, acylphosphine oxide, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone or 2-hydroxy-2-methylphenylpropane-1-one;
[0014] The epoxy resin monomer is at least one of bisphenol A epoxy resin, epoxidized ethylene epoxy resin, glycidyl epoxy resin and derivatives thereof;
[0015] The ether molecular monomer is one or both of diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether;
[0016] The curing agent is at least one of ethylenediamine, diethylenetriamine, dimethylaminopropylamine or polyetheramine;
[0017] The sodium salt is at least one of NaClO4, sodium hexafluorophosphate or sodium bis(fluorosulfonyl)imide;
[0018] The second aspect of the present invention provides a method for preparing a negative electrode-free sodium ion battery, which is used to prepare the negative electrode-free sodium ion battery provided in the first aspect of the present invention, comprising:
[0019] The positive electrode slurry is applied to the surface of the positive electrode current collector after cleaning and drying, and the first positive electrode sheet is obtained after curing; then an initiator, an epoxy resin monomer, an ether molecular monomer, a curing agent and a sodium salt are mixed to prepare an electrolyte solution, the electrolyte solution is applied to the surface of the first positive electrode sheet to form an electrolyte layer, and the positive electrode is obtained after curing;
[0020] The positive electrode is combined with the cleaned and dried metal current collector and packaged to obtain a negative electrode-free sodium ion battery.
[0021] Furthermore, the acid washing is to place the positive electrode current collector and the metal current collector in an acidic solution for washing; preferably, the concentration of the acidic solution is 0.1M-0.5M; preferably, the washing is an ultrasonic treatment for 0.5-1.5h.
[0022] Furthermore, the drying is vacuum drying at 70-85°C.
[0023] Further, the curing is performed by heating at 50-150° C. under vacuum conditions for 0.5-5 h.
[0024] The battery prepared in the present invention does not need to place sodium metal in advance on the negative electrode side. During the battery cycle, a sodium metal layer is evenly deposited on the negative electrode metal current collector, so no separate sodium plating process is required, which can effectively improve the energy density of the sodium ion battery. The full battery consisting of a sodium metal negative electrode, a low-cost Na3V2(PO4)3 positive electrode, and a low-cost all-solid polymer electrolyte can provide excellent electrochemical performance. At the same time, the thickness of the deposited sodium metal is only 0.5-10μm, which effectively reduces the mass of the negative electrode side and can improve the energy density and power density of the solid-state sodium ion battery.
[0025] The negative electrode-free sodium ion solid-state battery system composed of a polymer electrolyte, a metal current collector and a positive electrode can effectively buffer the volume expansion of sodium when it is deposited on the negative electrode current collector during the cycle, improve the cycle performance, and effectively inhibit the growth of sodium metal dendrites.
[0026] In summary, the preparation method of the negative electrode-free all-solid-state sodium ion battery provided by the present invention is easy to realize industrial production. The prepared negative electrode-free all-solid-state sodium ion battery has excellent cycle performance, energy density and power density, and its safety is improved, and it has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the charge and discharge curve of the battery in Example 1 of the present invention at 0.1C. DETAILED DESCRIPTION
[0028] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those who do not indicate the manufacturer of the reagents or instruments used are all conventional products that can be obtained commercially. In the following embodiments, if not clearly stated, "%" refers to weight percentage.
[0029] The thickness of the positive electrode collector and the metal current collector is 0.01-1mm, not limited to 0.02mm, 0.03mm, 0.04mm, 0.05mm, 0.06mm, 0.07mm, 0.08mm, 0.09mm, 0.10mm, 0.15mm, 0.20mm, 0.25mm, 0.30mm, 0.35mm, 0.40mm, 0.45mm, 0.50mm, 0.55mm, 0.60mm, 0.65mm, 0.70mm, 0.75mm, 0.80mm, 0.85mm, 0.90mm, and 0.95mm.
[0030] The thickness of the electrolyte layer is 10-200μm, but not limited to 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, and 190μm.
[0031] The concentration of the acid solution is 0.1M-0.5M, not limited to 0.2M, 0.3M, 0.4M;
[0032] The cleaning is performed by ultrasonic treatment for 0.5-1.5 h, but not limited to 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1.0 h, 1.1 h, 1.2 h, 1.3 h, and 1.4 h.
[0033] Drying is vacuum drying at 70-85°C, but not limited to 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, and 84°C.
[0034] The curing is carried out by heating under vacuum conditions at 50-150°C for 0.5-5h. The curing temperature is not limited to 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145°C; the heating time is not limited to 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h.
[0035] The preparation method of the negative electrode-free sodium ion battery in the present invention is as follows:
[0036] The positive electrode slurry is applied to the surface of the positive electrode current collector after cleaning and drying, and the first positive electrode sheet is obtained after curing; then an initiator, an epoxy resin monomer, an ether molecular monomer, a curing agent and a sodium salt are mixed to prepare an electrolyte solution, the electrolyte solution is applied to the surface of the first positive electrode sheet to form an electrolyte layer, and the positive electrode is obtained after curing;
[0037] The positive electrode is combined with the cleaned and dried metal current collector and packaged to obtain a negative electrode-free sodium ion battery.
[0038] Preferably, the concentration of the acidic solution is 0.1M-0.5M;
[0039] Preferably, the cleaning is performed by ultrasonic treatment for 0.5-1.5 h.
[0040] Preferably, the drying is vacuum drying at 70-85°C.
[0041] Preferably, the curing is performed by heating at 50-150° C. under vacuum conditions for 0.5-5 h.
[0042] Embodiment 1:
[0043] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0044] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0045] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, epoxidized olefin epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:50:20:4:25.
[0046] The preparation method of the solution layer is as follows:
[0047] (1) Dialkoxyacetophenone, epoxidized olefin-based epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80° C. for 12 h.
[0048] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:50:15) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0049] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 20:4:10) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0050] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0051] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0052] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0053] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0054] The sodium ion battery prepared in Example 1 was tested, and the results were as follows: Figure 1As shown, the abscissa is the specific capacity of the battery and the ordinate is the voltage. The discharge specific capacity at 0.1C is 89.7 mAh g -1 , after 100 charge and discharge cycles at 1C, the capacity retention rate is 90.5%.
[0055] Embodiment 2:
[0056] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0057] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0058] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, epoxidized olefin epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:40:25:4:30.
[0059] The preparation method of the solution layer is as follows:
[0060] (1) Dialkoxyacetophenone, epoxidized olefin-based epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80° C. for 12 h.
[0061] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:40:15) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0062] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 25:4:15) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0063] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0064] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0065] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0066] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0067] Embodiment 3:
[0068] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0069] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0070] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, epoxidized olefin epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:20:40:4:35.
[0071] The preparation method of the solution layer is as follows:
[0072] (1) Dialkoxyacetophenone, epoxidized olefin-based epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80° C. for 12 h.
[0073] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:20:20) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0074] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 40:4:15) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0075] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0076] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0077] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0078] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0079] Embodiment 4:
[0080] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0081] Na3V2(PO4)3, acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0082] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, epoxidized olefin epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:50:20:4:25.
[0083] The preparation method of the solution layer is as follows:
[0084] (1) Dialkoxyacetophenone, epoxidized olefin-based epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80° C. for 12 h.
[0085] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:50:15) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0086] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 20:4:10) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0087] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0088] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0089] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0090] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0091] Embodiment 5:
[0092] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0093] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0094] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, glycidyl epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:50:20:4:25.
[0095] The preparation method of the solution layer is as follows:
[0096] (1) Dialkoxyacetophenone, glycidyl epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80°C for 12 h.
[0097] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:50:15) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0098] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 20:4:10) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0099] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0100] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0101] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0102] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0103] A zinc foil with a thickness of 0.1 mm was used as a metal current collector. It was ultrasonically cleaned with distilled water for 30 minutes at 25 kHz, then immersed in a 0.5 M hydrochloric acid solution for 8 hours, then ultrasonically cleaned with distilled water for 30 minutes, and then ultrasonically cleaned with anhydrous alcohol at 25 kHz for 30 minutes to wipe the surface of the zinc foil substrate. The surface was vacuum dried at 100 °C.
[0104] Na4Fe3(PO4)2(P2O7), acetylene carbon black and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and a small amount of N-methylpyrrolidone was dissolved in the mixture and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was coated on a positive electrode current collector aluminum foil with a thickness of 15 μm, and dried in a vacuum drying oven at 80°C to obtain the first positive electrode sheet.
[0105] The initiator in the electrolyte solution is dialkoxyacetophenone; dialkoxyacetophenone, epoxidized olefin epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF6 are mixed in a mass ratio of 1:65:20:4:10.
[0106] The preparation method of the solution layer is as follows:
[0107] (1) Dialkoxyacetophenone, epoxidized olefin-based epoxy resin, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 were dried in a vacuum oven at 80° C. for 12 h.
[0108] (2) In a glove box, add dialkoxyacetophenone, epoxidized olefinic epoxy resin and NaPF4 (mass ratio of 1:50:15) into a reagent bottle and stir in an oil bath at 55°C for 8 h (speed of 400 r / min) until the sodium salt is completely dissolved to form a uniform solution.
[0109] (3) Similarly, diethylene glycol dimethyl ether, dimethylaminopropylamine and NaPF4 (mass ratio of 20:4:10) were added to a reagent bottle and stirred in an oil bath at 55°C for 8 h (speed of 500 r / min) until the sodium salt was completely dissolved to form a uniform solution.
[0110] (4) The solutions of step (2) and (3) were added into a reagent bottle at a mass ratio of 2:1, and stirred in an oil bath at 55° C. for 1 h (speed of 600 r / min) until the system was uniformly mixed to obtain an electrolyte solution.
[0111] (5) The electrolyte solution was placed in a glove box transition chamber and evacuated, and ultrasonically treated for 0.5 h to remove bubbles in the electrolyte solution.
[0112] (6) The electrolyte solution after bubbles are removed is evenly coated on the surface of the first positive electrode sheet with a scraper, and then placed under vacuum conditions at 100° C. for curing for more than 3 hours to ensure that it is fully cured on the surface of the first positive electrode sheet to form an electrolyte layer to obtain a positive electrode.
[0113] The positive electrode was cut into discs with a diameter of 16 mm and assembled into a battery with the treated zinc foil in a glove box filled with argon.
[0114] The negative electrodes prepared in the above embodiments and comparative examples were assembled into batteries for testing. Using the LAND CT2001A battery testing system of Wuhan Landian Electronics Co., Ltd., the sodium ion batteries prepared in the above embodiments and comparative examples were subjected to constant current charge and discharge tests at 0.1C and 1C current densities at 2.5 to 4.0V, and the cycles were greater than 100 times. The test results are shown in Table 1. It can be seen from the test results that the energy capacity of the all-solid-state sodium-free battery prepared by the present invention is considerable, and the cycle can be stably cycled for 100 times. Therefore, the present invention can be effectively applied in the preparation of all-solid-state sodium-free batteries with high energy density.
[0115] Table 1. Performance data of negative electrode-free all-solid-state sodium ion battery
[0116]
[0117] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A negative electrode-free sodium ion battery, characterized in that: The invention comprises a positive electrode and a metal current collector, and the positive electrode and the metal current collector are combined to obtain a battery; the positive electrode comprises a positive electrode current collector, a positive electrode slurry and an electrolyte layer, and the surface of the positive electrode current collector is pretreated, and then coated with the positive electrode slurry, and then coated with an electrolyte layer after drying; the electrolyte layer comprises 1wt% of an initiator, 40-55wt% of an epoxy resin monomer, 10-30wt% of an ether molecular monomer, 4wt% of a curing agent and 20-30wt% of a sodium salt.
2. The negative electrode-free sodium ion battery according to claim 1, characterized in that: The positive electrode current collector and the metal current collector are any one of copper foil, zinc foil and aluminum foil.
3. The negative electrode-free sodium ion battery according to claim 1, characterized in that: The thickness of the positive electrode current collector and the metal current collector are both 0.01-1 mm.
4. The negative electrode-free sodium ion battery according to claim 1, characterized in that: The thickness of the electrolyte layer is 10-200 μm.
5. The negative electrode-free sodium ion battery according to claim 1, characterized in that: The positive electrode slurry comprises a positive electrode active material, a conductive agent and a binder, and the mass ratio thereof is 7-10:1-2:1-2; Preferably, the positive electrode active material is Na3V2(PO4)3, Na4Fe3(PO4)2(P2O7), Na3Fe2(PO4)3, Na2Fe(SO4)2, and NaMn 1 / 3 Ni 1 / 3 Cu 1 / 3 Fe 1 / 3 At least one of O2; Preferably, the conductive agent is at least one of acetylene black, Ketjen black, carbon nanotubes, carbon nanofibers, and graphene; Preferably, the adhesive is at least one of sodium carboxymethyl cellulose, polyvinylidene fluoride, polytetrafluoroethylene, fluorinated rubber, polyurethane, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, alginic acid, sodium alginate, and styrene-butadiene rubber; more preferably, the adhesive is sodium carboxymethyl cellulose.
6. The negative electrode-free sodium ion battery according to claim 1, characterized in that: The initiator is at least one of dialkoxyacetophenone, α-hydroxyalkyl phenone, acylphosphine oxide, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholine-1-propanone or 2-hydroxy-2-methylphenylpropane-1-one; The epoxy resin monomer is at least one of bisphenol A epoxy resin, epoxidized olefin epoxy resin, glycidyl epoxy resin and derivatives thereof; The ether molecular monomer is one or both of diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; The curing agent is at least one of ethylenediamine, diethylenetriamine, dimethylaminopropylamine or polyetheramine; The sodium salt is at least one of NaClO4, sodium hexafluorophosphate or sodium bis(fluorosulfonyl)imide.
7. A method for preparing a negative electrode-free sodium ion battery, characterized in that: For preparing the negative electrode-free sodium ion battery according to any one of claims 1 to 6, comprising: The positive electrode slurry is applied to the surface of the positive electrode current collector after cleaning and drying, and the first positive electrode sheet is obtained after curing; then an initiator, an epoxy resin monomer, an ether molecular monomer, a curing agent and a sodium salt are mixed to prepare an electrolyte solution, the electrolyte solution is applied to the surface of the first positive electrode sheet to form an electrolyte layer, and the positive electrode is obtained after curing; The positive electrode is combined with the cleaned and dried metal current collector and packaged to obtain a negative electrode-free sodium ion battery.
8. The preparation method according to claim 7, characterized in that: The acid washing is to place the positive electrode current collector and the metal current collector in an acidic solution for washing; preferably, the concentration of the acidic solution is 0.1M-0.5M; preferably, the washing is an ultrasonic treatment for 0.5-1.5h.
9. The preparation method according to claim 7, characterized in that: The drying is vacuum drying at 70-85°C.