Sulfide solid electrolyte and preparation method thereof

Through high-energy microwave sintering technology, the problem of low preparation efficiency of sulfide electrolytes is solved, and the ionic conductivity and material properties of the electrolyte are significantly improved, achieving a more efficient preparation process.

CN118943473APending Publication Date: 2024-11-12HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202410993453.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing preparation methods of sulfide electrolytes have the problem of low preparation efficiency, especially the sintering process takes a long time, which affects the ionic conductivity and material properties of the electrolyte.

Method used

The sulfide electrolyte is prepared by high-energy microwave sintering technology. Through high-speed powder mixing and rotary microwave sintering, the preparation time is significantly shortened and the ionic conductivity of the electrolyte is improved.

Benefits of technology

The ionic conductivity of the sulfide electrolyte is significantly improved, while reducing the preparation temperature and time, and improving the purity and preparation efficiency of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943473A_ABST
    Figure CN118943473A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and particularly relates to a sulfide solid electrolyte and a preparation method thereof. The chemical composition of the sulfide solid electrolyte is Li < 6-m > PS < 5-m > X < 1 + m >, wherein 0 lt; mlt; mlt; x is selected from one or more of F, Cl, Br and I. The preparation method comprises the following steps: (1) weighing raw materials for preparing the sulfide solid electrolyte according to a stoichiometric ratio of a chemical formula, crushing and mixing, and uniformly mixing to obtain an electrolyte precursor; and (2) placing the electrolyte precursor in microwave equipment, and carrying out rotary microwave sintering. Compared with the existing conventional LPSX sulfide electrolyte, the sulfide electrolyte provided by the invention has higher halogen content and remarkably higher ionic conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium - ion batteries, and particularly relates to a sulfide solid electrolyte and a preparation method thereof. Background Art

[0002] Under the background of carbon neutrality, lithium - ion batteries, as a portable energy storage device, have been widely used in fields such as electric vehicles and energy storage. However, due to the use of flammable liquid electrolytes in lithium - ion batteries, there are safety problems, and the energy density is close to the theoretical value. All - solid - state lithium batteries, with higher safety performance and energy density, are considered the most important next - generation electrochemical energy storage technology. Solid electrolytes, as the core components of all - solid - state batteries, have been widely studied. Among them, sulfide solid electrolytes are considered more suitable materials due to their high ionic conductivity and appropriate mechanical properties.

[0003] Currently, the preparation of sulfide electrolytes is mostly carried out by solid - phase mixing combined with annealing sintering. An addition reaction occurs during the sintering process to form the electrolyte material. Mixing is generally carried out by ball - milling. There are the following problems in preparing sulfide electrolytes by a similar method: (1) The amount of primary mixing is limited, and the ball - milling time is more than 20 h; (2) The sintering method is generally sintering in a muffle furnace. Limited by the heating method and the thermal conductivity of the electrolyte material, the sintering process of sulfide electrolytes requires a long time, generally 12 - 48 hours, seriously affecting the preparation efficiency of sulfide electrolytes.

[0004] Based on this, it is necessary to develop a method for quickly preparing sulfide solid electrolytes in large quantities. Summary of the Invention

[0005] The purpose of the present invention is to provide a sulfide solid electrolyte and a preparation method thereof.

[0006] According to the first aspect of the present invention, the present invention provides a sulfide solid electrolyte, and the chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5-m X 1+m ; wherein, 0 < m < 1, and X is selected from one or more of F, Cl, Br, and I.

[0007] Compared with the existing method of preparing sulfide electrolytes by ball - milling combined with muffle furnace annealing sintering, heating and sintering the electrolyte precursor with high - energy microwaves can make the heating of sulfide electrolytes more uniform. However, the present invention unexpectedly finds through research that when using the high - energy microwave sintering method for the chemical composition of Li 6 PS 5 Cl 0.5 Br 0.5When the sulfide electrolyte is prepared, it is found that the ionic conductivity of the prepared sulfide electrolyte is not significantly improved. For example, the ionic conductivity of the sulfide electrolyte obtained in Comparative Example 4 of the present invention is only 5mS / cm. Thus, the present invention has further studied and found that when a high-energy microwave sintering method is used to prepare the sulfide solid electrolyte with the chemical composition provided by the present invention, that is, the chemical composition of the sulfide solid electrolyte provided by the present invention contains a higher halogen content, it is found that the ionic conductivity of the prepared sulfide electrolyte can be as high as 15mS / cm, that is, increasing the halogen content in the sulfide electrolyte to a certain extent can significantly improve the ionic conductivity of the sulfide electrolyte. The sulfide solid electrolyte provided by the present invention can cause the S and X elements in the crystalline structure to have a higher degree of disorder at the 4a and 4d positions due to the high content of halogen element X replacing the S element, which helps to promote Li + transitions in the crystal lattice, thereby increasing the ionic conductivity of the electrolyte.

[0008] Specifically, the chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5-m X 1+m ; Wherein, m can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 or a range consisting of any two of the above values. It is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0009] In some embodiments of the present invention, the chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5- m X 1+m ; Wherein, 0.3≤m≤0.8. Specifically, the chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5-m X 1+m ; Wherein, m can be 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or a range consisting of any two of the above values. Not limited to the listed values, other values ​​not listed in the numerical range are also applicable. By controlling m in the chemical composition structural formula of the sulfide solid electrolyte within the above range, the content distribution of the halogen in the sulfide electrolyte can be further improved, thereby achieving a more significant effect of improving the ionic conductivity of the sulfide electrolyte.

[0010] In some embodiments of the present invention, the raw material source of the sulfide solid electrolyte is Li 2 S.P. 2 S 5and LiX, wherein X is selected from one or more of F, Cl, Br, and I.

[0011] In some embodiments of the present invention, the sulfide solid electrolyte is prepared by microwave sintering. The sulfide solid electrolyte provided by the present invention, due to the high content of halogen element X replacing the position of S element, can cause the S and X elements in the crystalline structure to have a higher degree of disorder at the 4a and 4d positions, which helps to promote the transition of Li+ in the lattice, thereby improving the ionic conductivity of the electrolyte. And because the sulfide solid electrolyte provided by the present invention has a higher content of halogen X, the raw materials for preparing the sulfide solid electrolyte are prepared by microwave sintering, which can make it better coupled with microwaves and better reduce the sintering temperature of the electrolyte, so as to achieve the improvement of the ionic conductivity of the electrolyte while reducing the sintering temperature required for preparation and improving the preparation efficiency of the electrolyte.

[0012] In some embodiments of the present invention, the microwave frequency of the microwave sintering is 5-35 GHz; preferably, the microwave frequency of the microwave sintering is 15-30 GHz. Specifically, the microwave frequency of the microwave sintering can be 5 GHz, 6 GHz, 7 GHz, 8 GHz, 9 GHz, 10 GHz, 11 GHz, 12 GHz, 13 GHz, 14 GHz, 15 GHz, 16 GHz, 17 GHz, 18 GHz, 19 GHz, 20 GHz, 21 GHz, 22 GHz, 23 GHz, 24 GHz, 25 GHz, 26 GHz, 27 GHz, 28 GHz, 29 GHz, 30 GHz, 31 GHz, 32 GHz, 33 GHz, 34 GHz, 35 GHz or a range consisting of any two of the above values. Not limited to the listed values, other values ​​not listed in the numerical range are also applicable. By controlling the microwave frequency of microwave sintering within the above range, better uniformity of the sintered electrolyte can be achieved, the electrolyte can be heated more evenly, and the effect of impurities will not be produced, so that the prepared sulfide electrolyte has higher purity and higher ionic conductivity.

[0013] According to the second aspect of the present invention, the present invention further provides a method for preparing the sulfide solid electrolyte as described in any one of the first aspects of the present invention, comprising the following steps:

[0014] (1) Mixing: weighing the raw materials for preparing the sulfide solid electrolyte according to the stoichiometric ratio, crushing and mixing, and mixing evenly to obtain an electrolyte precursor;

[0015] (2) Sintering: placing the electrolyte precursor in a microwave device and performing rotary microwave sintering to obtain the sulfide solid electrolyte.

[0016] As shown in the background technology section, the existing preparation of sulfide electrolytes is generally carried out by ball milling mixing combined with muffle furnace annealing and sintering. Due to the limitations of the mixing method, heating means and thermal conductivity of the electrolyte material, the sulfide electrolyte mixing and sintering processes require a long time, which seriously affects the preparation efficiency of the sulfide electrolyte. Based on this, the present invention provides a method for preparing a sulfide solid electrolyte, which prepares the sulfide electrolyte by high-speed powder mixing combined with high-energy microwave sintering, significantly shortening the time required for the preparation process, improving the preparation efficiency, and significantly improving the ionic conductivity of the prepared sulfide electrolyte.

[0017] In some embodiments of the present invention, the raw materials for preparing the sulfide solid electrolyte include Li 2 S.P. 2 S 5 and LiX, wherein X is selected from one or more of F, Cl, Br, and I.

[0018] In some embodiments of the present invention, the ratio of each raw material is: Li 2 S:P 2 S 5:LiX=3.2~4.9:1:2.1~3.8. Specifically, according to the stoichiometric ratio, the ratio of each raw material can be 3.2:1:2.1, 3.3:1:2.1, 3.4:1:2.1, 3.5:1:2.1, 3.6:1:2.1, 3.7:1:2.1, 3.8:1:2.1, 3.9:1:2.1, 4.0:1:2.1, 4.1:1:2.1, 4.2:1:2.1, 4.4:1:2.1, 4.5:1:2.1, 4.6:1:2.1, 4.7:1:2.1, 4.8:1:2.1, 4.9:1:2.1, 3.2:1:2.2, 3.3:1:2.2, 3.4:1:2.2, 3.5:1:2.2, 3.6:1:2.2, 3.7:1:2.1 .7:1:2.2, 3.8:1:2.2, 3.9:1:2.2, 4.0:1:2.2, 4.1:1:2.2, 4.2:1:2.2, 4.4:1:2.2, 4.5:1:2.2, 4.6:1:2.2, 4.7:1:2.2, 4.8:1:2.2, 4.9:1:2.2, 3.2:1:2.3, 3.3:1:2.3, 3.4:1:2.3, 3.5:1:2.3, 3.6:1:2.3, 3.7:1:2.3, 3.8:1:2.3, 3.9:1:2.3, 4.0:1:2.3, 4.1:1:2.3, 4.2:1:2.3, 4.4:1:2.3, 4.5:1 :2.3, 4.6:1:2.3, 4.7:1:2.3, 4.8:1:2.3, 4.9:1:2.3, 3.2:1:2.4, 3.3:1:2.4, 3.4:1:2.4, 3.5:1:2.4, 3.6:1:2.4, 3.7:1:2.4, 3.8:1:2.4, 3.9:1:2.4, 4.0:1:2.4, 4.1:1:2.4, 4.2:1:2.4, 4.4:1:2.4, 4.5:1:2.4, 4.6:1:2.4, 4.7:1:2.4, 4.8:1:2.4, 4.9:1:2.4, 3.2:1:2.5, 3.3:1:2.5, 3.4:1:2. 5, 3.5:1:2.5, 3.6:1:2.5, 3.7:1:2.5, 3.8:1:2.5, 3.9:1:2.5, 4.0:1:2.5, 4.1:1:2.5, 4.2:1:2.5, 4.4:1:2.5, 4.5:1:2.5, 4.6:1:2.5, 4.7:1:2.5, 4.8:1:2.5, 4.9:1:2.5, 3.2:1:2.6, 3.3:1:2.6, 3.4:1:2.6, 3.5:1:2.6, 3.6:1:2.6, 3.7:1:2.6, 3.8:1:2.6, 3.9:1:2.6, 4.0:1:2.6, 4.1:1:2.6, 4.2:1:2.6、4.4:1:2.6、4.5:1:2.6、4.6:1:2.6、4.7:1:2.6、4.8:1:2.6、4.9:1:2.6、3.2:1:2.8、3.3:1:2.8、3.4:1:2.8、3.5:1:2.8、3.6:1:2.8、3.7:1:2.8、3.8:1:2.8、3.9:1:2.8、4.0:1:2.8、4.1:1:2.8、4.2:1:2.8、4.4:1:2.8、4.5:1:2.8、4.6:1:2.8、4.7:1:2.8、4.8:1:2.8、4.9:1:2.8、3.2:1:3.0、3.3:1:3.0、3.4:1:3.0、3.5:1:3.0、3.6:1:3.0、3.7:1:3.0、3.8:1:3.0、3.9:1:3.0、4.0:1:3.0、4.1:1:3.0、4.2:1:3.0、4.4:1:3.0、4.5:1:3.0、4.6:1:3.0、4.7:1:3.0、4.8:1:3.0、4.9:1:3.0、3.2:1:3.2、3.3:1:3.2、3.4:1:3.2、3.5:1:3.2、3.6:1:3.2、3.7:1:3.2、3.8:1:3.2、3.9:1:3.2、4.0:1:3.2、4.1:1:3.2、4.2:1:3.2、4.4:1:3.2、4.5:1:3.2、4.6:1:3.2、4.7:1:3.2、4.8:1:3.2、4.9:1:3.2、3.2:1:3.5、3.3:1:3.5、3.4:1:3.5、3.5:1:3.5、3.6:1:3.5、3.7:1:3.5、3.8:1:3.5、3.9:1:3.5、4.0:1:3.5、4.1:1:3.5、4.2:1:3.5、4.4:1:3.5、4.5:1:3.5、4.6:1:3.5、4.7:1:3.5、4.8:1:3.5、4.9:1:3.5、3.2:1:3.6、3.3:1:3.6、3.4:1:3.6、3.5:1:3.6、3.6:1:3.6、3.7:1:3.6、3.8:1:3.6、3.9:1:3.6、4.0:1:3.6、4.1:1:3.6、4.2:1:3.6、4.4:1:3.6、4.5:1:3.6、4.6:1:3.6、4.7:1:3.6、4.8:1:3.6、4.9:1:3.6 or a range consisting of any two of the above ratios. Not limited to the listed values, other values ​​not listed in the numerical range are also applicable. By controlling the ratio of each raw material within the above range, the prepared electrolyte can contain a higher and more suitable halogen content, so that it can better couple with microwaves and significantly improve the ionic conductivity of the electrolyte. .

[0019] In some embodiments of the present invention, the ratio of each raw material is: Li 2 S:P 2 S 5 :LiX=3.4~4.4:1:2.6~3.6. When the ratio of each raw material is controlled within the above range, the ionic conductivity of the electrolyte can be more significantly improved. When the ratio of each raw material is controlled within the above range, the ionic conductivity of the electrolyte can be more significantly improved.

[0020] In some embodiments of the present invention, in step (1), the pulverizing and mixing is performed in a powder pulverizer. Combining powder pulverization with microwave sintering can prepare sulfide electrolytes more quickly and efficiently, and the synthesized electrolyte has higher uniformity due to microwave sintering, which is conducive to element diffusion.

[0021] In some embodiments of the present invention, the rotating speed of the crushing and mixing / or powdering machine is 20000~50000rpm / min. Specifically, the rotating speed of the crushing and mixing / or powdering machine can be 20000rpm / min, 25000rpm / min, 26000rpm / min, 27000rpm / min, 28000rpm / min, 29000rpm / min, 30000rpm / min, 31000rpm / min, 32000rpm / min, 33000rpm / min, 34000rpm / min, 35000rpm / min, 36000rpm / min, 37000rpm / min, 38000rpm / min, 39000rpm / min, 4000rpm / min, 45000rpm / min, 50000rpm / min or the range composed of any two of the above values. Not limited to the listed values, other unlisted values ​​in the numerical range are also applicable.

[0022] In some embodiments of the present invention, the mixing time is 0.1 to 2 hours; preferably, the mixing time is 0.1 to 0.5 hours. Specifically, the mixing time can be 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1.0h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h or a range consisting of any two of the above values. Not limited to the listed values, other values ​​not listed in the numerical range are also applicable. Controlling the parameters of the crushing mixer / or powdering machine within the above range can achieve uniform mixing of raw materials more quickly and better, and prepare sulfide electrolytes faster and more efficiently.

[0023] In some embodiments of the present invention, in step (2), the electrolyte precursor is placed in a microwave device for rotary microwave sintering, which includes the following steps: the electrolyte precursor is sealed in a low-absorption and high-temperature resistant container, the container sealed with the electrolyte precursor is placed on a rotatable base of the microwave device, the microwave device is started, and the container rotates with the rotatable base to perform microwave sintering. The rotary microwave sintering can make the electrolyte more evenly heated, make the electrolyte material better react with microwaves, improve the uniformity of microwave sintering, speed up the sintering process, and will not produce impurities.

[0024] In some embodiments of the present invention, the low-absorption and high-temperature resistant container is selected from alumina or quartz crucible.

[0025] In some embodiments of the present invention, the microwave sintering conditions are: heating to 100-450°C at a rate of 60-150°C / min, and sintering for 0.1-1h. Specifically, in the above microwave sintering conditions, the sintering temperature after heating can be 100°C, 150, 200°C, 250°C, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C or a range consisting of any two of the above values. Not limited to the listed values, other values ​​not listed in the numerical range are also applicable. Specifically, in the above microwave sintering conditions, the sintering time can be 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h or a range consisting of any two of the above values. Not limited to the listed values, other unlisted values ​​within the numerical range are also applicable. Specifically, in the above microwave sintering conditions, the heating rate can be 60℃ / min, 65℃ / min, 70℃ / min, 75℃ / min, 80℃ / min, 85℃ / min, 90℃ / min, 95℃ / min, 100℃ / min, 105℃ / min, 110℃ / min, 115℃ / min, 120℃ / min, 125℃ / min, 130℃ / min, 135℃ / min, 140℃ / min, 145℃ / min, 150℃ / min or a range consisting of any two of the above values. The present invention is not limited to the numerical values ​​listed, and other numerical values ​​not listed within the numerical range are also applicable.

[0026] In some embodiments of the present invention, the microwave sintering conditions are preferably: heating to 250-450° C. at a rate of 60-150° C. / min, and sintering for 20-40 min.

[0027] In some embodiments of the present invention, the microwave sintering conditions are preferably: heating to 100-450° C. at a rate of 80-130° C. / min, and sintering for 0.1-1 h.

[0028] In some embodiments of the present invention, the microwave sintering conditions are preferably: heating to 250-450° C. at a rate of 80-120° C. / min, and sintering for 20-40 min.

[0029] By controlling the microwave sintering conditions within the above range, the electrolyte material can better react with microwaves, improve the uniformity of microwave sintering, speed up the sintering process, and avoid generating impurities.

[0030] In some embodiments of the present invention, the microwave frequency of the microwave sintering is 5-35GHz; preferably, the microwave frequency of the microwave sintering is 15-30GHz. Specifically, the microwave frequency of the microwave sintering can be 5GHz, 6GHz, 7GHz, 8GHz, 9GHz, 10GHz, 11GHz, 12GHz, 13GHz, 14GHz, 15GHz, 16GHz, 17GHz, 18GHz, 19GHz, 20GHz, 21GHz, 22GHz, 23GHz, 24GHz, 25GHz, 26GHz, 27GHz, 28GHz, 29GHz, 30GHz, 31GHz, 32GHz, 33GHz, 34GHz, 35GHz or a range consisting of any two of the above values. Not limited to the listed values, other unlisted values ​​within the numerical range are also applicable. Controlling the microwave frequency of microwave sintering within the above range can make the electrolyte material better interact with microwaves, improve the uniformity of microwave sintering, accelerate the sintering process, and will not produce impurities.

[0031] According to the third aspect of the present invention, the present invention further provides a lithium-ion battery, which comprises a sulfide solid electrolyte as described in any one of the first aspect of the present invention / or a sulfide solid electrolyte prepared by any one of the preparation methods described in any one of the second aspect of the present invention.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention provides a new sulfide electrolyte. Compared with the existing conventional LPSX sulfide electrolyte, the sulfide electrolyte provided by the present invention has a higher halogen content and significantly higher ionic conductivity.

[0034] (2) The present invention also provides a method for preparing the sulfide electrolyte. In the preparation method provided by the present invention, the sulfide electrolyte is prepared by high-speed powder mixing combined with high-energy microwave sintering, which significantly shortens the time required for the preparation process, improves the preparation efficiency, and significantly improves the ionic conductivity of the prepared sulfide electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is an appearance diagram of the electrolyte prepared in Example 1 of the present invention;

[0036] Figure 2 This is a SEM image of the electrolyte prepared in Example 1 of the present invention;

[0037] Figure 3 The XRD structure diagrams of the electrolytes prepared in various embodiments and comparative examples of the present invention are shown below;

[0038] Figure 4 The impedance diagrams of the electrolytes prepared in the embodiments and comparative examples of the present invention are shown in FIG. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further described below by specific embodiments, which do not limit the protection scope of the present invention. Some non-essential modifications and adjustments made by others based on the concept of the present invention still fall within the protection scope of the present invention.

[0040] Hereinafter, the present invention will be described in more detail by way of specific examples.

[0041] Example 1

[0042] This embodiment provides a method for preparing a sulfide solid electrolyte, comprising the following steps:

[0043] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 3.8:1:1.6:1.6, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 minutes to obtain a uniformly mixed electrolyte precursor;

[0044] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started, and the quartz crucible rotated with the base to absorb microwaves more evenly. The temperature was raised to 300°C and sintered for 30 minutes (the heating rate was 100°C / min), and Li 5.4 PS 4.4 Cl 0.8 Br 0.8 Electrolyte; wherein the microwave frequency is 28 GHz.

[0045] The appearance of the electrolyte prepared in this example is as follows Figure 1 The SEM image of its microstructure is shown in Figure 2 As shown, the XRD pattern is Figure 3 The impedance diagram is shown as Figure 4 In summary, the electrolyte prepared in this embodiment has high crystallinity and purity.

[0046] Example 2

[0047] This embodiment provides a method for preparing a sulfide solid electrolyte, comprising the following steps:

[0048] The electrolyte raw material Li 2 S:P2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 4:1:1.8:1.2, put into a powder grinder, and crushed and mixed at a speed of 50000 rpm / min for 6 minutes to obtain a uniformly mixed electrolyte precursor;

[0049] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started, and the quartz crucible rotated with the base to absorb microwaves more evenly. The temperature was raised to 350°C and sintered for 30 minutes (the heating rate was 100°C / min) to prepare Li 5.5 PS 4.5 Cl 0.9 Br 0.6 Electrolyte; wherein the microwave frequency is 28 GHz.

[0050] Example 3

[0051] This embodiment provides a method for preparing a sulfide solid electrolyte, comprising the following steps:

[0052] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 4.4:1:1.4:1.2, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 minutes to obtain a uniformly mixed electrolyte precursor;

[0053] The mixed electrolyte precursor was sealed in an alumina crucible, and the alumina crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started, and the quartz crucible rotated with the base to absorb microwaves more evenly. The temperature was raised to 400°C and sintered for 30 minutes (the heating rate was 100°C / min) to prepare Li 5.7 PS 4.7 Cl 0.7 Br 0.6 Electrolyte; wherein the microwave frequency is 28 GHz.

[0054] Example 4

[0055] This embodiment provides a method for preparing a sulfide solid electrolyte, comprising the following steps:

[0056] The electrolyte raw material Li 2 S:P 2 S 5:LiCl was weighed according to the stoichiometric ratio of 3.8:1:3.2, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 min to obtain a uniformly mixed electrolyte precursor;

[0057] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started, and the quartz crucible rotated with the base to absorb microwaves more evenly. The temperature was raised to 300°C and sintered for 30 minutes (the heating rate was 100°C / min), and Li 5.4 PS 4.4 Cl 1.6 Electrolyte; wherein the microwave frequency is 28 GHz.

[0058] Example 5

[0059] This embodiment provides a method for preparing a sulfide solid electrolyte, comprising the following steps:

[0060] The electrolyte raw material Li 2 S:P 2 S 5 :LiBr was weighed according to the stoichiometric ratio of 3.8:1:3.2, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 min to obtain a uniformly mixed electrolyte precursor;

[0061] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started, and the quartz crucible rotated with the base to absorb microwaves more evenly. The temperature was raised to 300°C and sintered for 30 minutes (the heating rate was 100°C / min), and Li 5.4 PS 4.4 Br 1.6 Electrolyte; wherein the microwave frequency is 28 GHz.

[0062] Comparative Example 1

[0063] This comparative example provides a method for preparing a sulfide solid electrolyte based on Example 1. The difference from Example 1 is that the mixing method and sintering method of the electrolyte raw materials are different, as follows:

[0064] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 3.8:1:1.6:1.6, put into a ball mill, and ball milled for 20 h at a speed of 500 rpm / min to obtain a uniformly mixed electrolyte precursor;

[0065] The mixed electrolyte precursor was sealed in a quartz crucible, placed in a muffle furnace for annealing, and sintered at 450 ° C for 20 h to prepare Li 5.4 PS 4.4 Cl 0.8 Br 0.8 Electrolytes.

[0066] The XRD pattern of the electrolyte prepared in this comparative example is as follows: Figure 3 As shown, although it has a high crystallinity, there is Li 2 S mixed phase.

[0067] Comparative Example 2

[0068] This comparative example provides a method for preparing a sulfide solid electrolyte based on Example 1, and the specific steps are as follows:

[0069] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 3.8:1:1.6:1.6, put into a ball mill, and ball milled for 20 h at a speed of 500 rpm / min to obtain a uniformly mixed electrolyte precursor;

[0070] The mixed electrolyte precursor was sealed in a quartz crucible, placed in a muffle furnace for annealing, and sintered at 350 ° C for 30 min to prepare Li 5.5 PS 4.5 Cl 0.8 Br 0.8 Electrolytes.

[0071] The XRD pattern of the electrolyte prepared in this comparative example is as follows: Figure 3 As shown, the electrolyte prepared by this method has low crystallinity and contains a large amount of raw material impurities.

[0072] Comparative Example 3

[0073] This comparative example provides a method for preparing a sulfide solid electrolyte based on Example 1. The difference from Example 1 is that the microwave frequency in the microwave sintering step is different, as follows:

[0074] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr was weighed according to the stoichiometric ratio of 3.8:1:1.6:1.6, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 minutes to obtain a uniformly mixed electrolyte precursor;

[0075] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started. The quartz crucible rotated with the base, which could absorb microwaves more evenly. The temperature was raised to 300°C and sintered for 1h (the heating rate was 50°C / min) to prepare Li 5.4 PS 4.4 Cl 0.8 Br 0.8 Electrolyte; wherein the microwave frequency is 2.45 GHz.

[0076] The XRD pattern of the electrolyte prepared in this comparative example is as follows: Figure 3 As shown, although the electrolyte prepared by this method has high crystallinity, it has a small amount of impurities of the raw materials due to poor sintering uniformity.

[0077] Comparative Example 4

[0078] This comparative example provides a method for preparing a sulfide solid electrolyte based on Example 1. The difference from Example 1 is that the mixing ratio of the electrolyte raw materials is different, as follows:

[0079] The electrolyte raw material Li 2 S:P 2 S 5 :LiCl:LiBr were weighed according to the stoichiometric ratio of 5:1:1:1, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 min to obtain a uniformly mixed electrolyte precursor;

[0080] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started. The quartz crucible rotated with the base to absorb microwaves more evenly. The microwave frequency was 28 GHz, and the temperature was raised to 450 ° C for 30 min (the heating rate was 100 ° C / min), and Li 6 PS 5 Cl 0.5 Br 0.5 Electrolytes.

[0081] Comparative Example 5

[0082] This comparative example provides a method for preparing a sulfide solid electrolyte based on Example 1. The difference from Example 1 is that the mixing ratio of the electrolyte raw materials is different, as follows:

[0083] The electrolyte raw material Li 2 S:P 2 S 5:LiCl:LiBr is weighed according to the stoichiometric ratio of 3:1:2:2, put into a powder grinder, and crushed and mixed at a speed of 30000 rpm / min for 15 minutes to obtain a uniformly mixed electrolyte precursor;

[0084] The mixed electrolyte precursor was sealed in a quartz crucible, and the quartz crucible containing the electrolyte precursor was placed on a rotatable base in a microwave device. The microwave sintering furnace was started. The quartz crucible rotated with the base to absorb microwaves more evenly. The microwave frequency was 28 GHz, and the temperature was raised to 450 ° C for 30 min (the heating rate was 100 ° C / min), and Li 5 PS 4 Cl 1 Br 1 Electrolytes.

[0085] Performance Testing

[0086] The EIS impedance of the blocked battery assembled with carbon-coated aluminum foil on both sides of the electrolyte prepared in the above Examples 1-5 and Comparative Examples 1-5 was measured. The test method is as follows: the assembled blocked battery is placed in a 25°C constant temperature box for 1 hour to make the temperature of the electrolyte inside the battery reach 25°C, and the battery is connected to the electrochemical workstation of Su Liqiang to measure the constant voltage AC impedance at a frequency range of 1MHz to 1Hz. After conversion, the ionic conductivity of the electrolyte prepared in each example and comparative example is obtained. Among them, the ionic conductivity impedance spectra of the electrolyte prepared by Examples 1-5 and Comparative Examples 1-5 are as follows: Figure 4 As shown, the impedance (Ω) and ionic conductivity (mS / cm) of the electrolytes prepared in each embodiment and comparative example are shown in Table 1:

[0087] Table 1 Impedance and ionic conductivity data of electrolytes prepared in each group and comparison of the disorder of S and halogen X at lattice sites 4a and 4d obtained by XRD refinement

[0088]

[0089]

[0090] According to the results shown in Table 1, the room temperature ionic conductivity of the electrolyte obtained in Example 1 is 15 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Example 2 is 13 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Example 3 is 10 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Example 4 is 14 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Example 5 is 13.5 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Comparative Example 1 is 11 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Comparative Example 2 is 2 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Comparative Example 3 is 9 mS / cm, the room temperature ionic conductivity of the electrolyte obtained in Comparative Example 4 is 5 mS / cm, and the room temperature ionic conductivity of the electrolyte obtained in Comparative Example 5 is 6.5 mS / cm.

[0091] By comparing the disorder of Examples 1, 2, and 3 with that of Comparative Example 4, it can be found that when not doped, S mainly occupies the 4d position and X mainly occupies the 4a position. As the content of the X element increases, the S content at the 4a position gradually increases, and the X element at the 4d position increases, that is, the disorder of S and X at the 4a / 4d position increases, thereby improving the ionic conductivity of the electrolyte. As shown in Comparative Example 5, when the X content is too high, the crystal structure of the electrolyte cannot be maintained, and X cannot be successfully doped, so the ionic conductivity decreases.

[0092] By comparing the results of Example 1 with those of Comparative Example 1, it can be found that the sulfide solid electrolyte can be prepared faster and more efficiently by using the powder pulverizer in Example 1 combined with microwave sintering, and the synthesized electrolyte has higher uniformity due to microwave sintering, which is conducive to element diffusion. Therefore, the electrolyte prepared in Example 1 does not have impurities, has a lower sintering temperature, and has a higher ionic conductivity of 15 mS / cm. In Comparative Example 1, when a muffle furnace is used for heating and sintering, not only does the heating time take a long time, but the prepared electrolyte also has Li 2 The ionic conductivity of the S impurity phase is also significantly lower. Further comparison of the results of Example 1 and Comparative Example 2 further shows that when the sulfide electrolyte precursor is heated and sintered in a muffle furnace, the heating effect is poor. If the sintering time is too short, the electrolyte will not have time to crystallize, resulting in the prepared electrolyte having too low ionic conductivity.

[0093] Comparing the results of Example 1 with Comparative Example 3, it can be found that the electrolyte is sintered using the conventional microwave frequency of 2.45 GHz. In addition to the presence of a small amount of impurities in the raw materials, the ionic conductivity of the electrolyte obtained is also significantly lower. Compared with the conventional microwave frequency of 2.45 GHz, the present invention uses a microwave frequency of 28 GHz to sinter the electrolyte, so that the electrolyte is heated more evenly, and the prepared electrolyte has no impurities, better uniformity, and significantly higher ionic conductivity. Further comparing the results of Example 1 with Comparative Example 4, it can be found that even if the sulfide electrolyte is microwave sintered based on the same microwave frequency (28 GHz), the ionic conductivity of the electrolyte obtained in Comparative Example 4 is significantly reduced, and the electrolyte obtained in Example 1 has a higher halogen content, and achieves a better coupling effect with high-frequency microwaves, so that the prepared electrolyte achieves a higher ionic conductivity. Further comparing Example 1 with Comparative Example 5, it can be found that excessive halogen substitution for sulfur element will cause the crystal structure of the electrolyte to be destroyed and generate impurities, so that the ionic conductivity is reduced.

[0094] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of the present invention are within the scope of protection of the present invention.

Claims

1. A sulfide solid electrolyte, characterized in that: The chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5-m X 1+m ; wherein, 0 < m < 1, and X is selected from one or more of F, Cl, Br, and I.

2. The sulfide solid electrolyte according to claim 1, characterized in that The chemical composition of the sulfide solid electrolyte is: Li 6-m PS 5-m X 1+m ; Among them, 0.3≤m≤0.

8.

3. The sulfide solid electrolyte according to claim 1, characterized in that The raw material sources of the sulfide solid electrolyte are Li2S, P2S5 and LiX, wherein X is selected from one or more of F, Cl, Br and I.

4. A method for preparing a sulfide solid electrolyte as claimed in any one of claims 1 to 3, characterized in that: The steps include: (1) Mixing: weighing the raw materials for preparing the sulfide solid electrolyte according to the stoichiometric ratio, crushing and mixing, and mixing evenly to obtain an electrolyte precursor; (2) Sintering: placing the electrolyte precursor in a microwave device and performing rotary microwave sintering to obtain the sulfide solid electrolyte.

5. The preparation method according to claim 4, characterized in that: The raw materials for preparing the sulfide solid electrolyte include Li2S, P2S5 and LiX, wherein X is selected from one or more of F, Cl, Br and I.

6. The preparation method according to claim 5, characterized in that: According to the stoichiometric ratio, the ratio of each raw material is: Li2S:P2S5:LiX=3.2~4.9:1:2.1~3.8; preferably, Li2S:P2S5:LiX=3.4~4.4:1:2.6~3.

6.

7. The preparation method according to claim 4, characterized in that: Step (1), the crushing and mixing is carried out in a powder grinder; Preferably, the speed of the powdering machine is 20000-50000 rpm / min; Preferably, the mixing time is 0.1 to 2 hours; Preferably, the mixing time is 0.1 to 0.5 h.

8. The preparation method according to claim 4, characterized in that: In step (2), placing the electrolyte precursor in a microwave device and performing rotary microwave sintering comprises the following steps: The electrolyte precursor is sealed in a low-absorption and high-temperature resistant container, the container sealed with the electrolyte precursor is placed on a rotatable base of the microwave device, the microwave device is started, and the container rotates with the rotatable base to perform microwave sintering; Preferably, the low-absorption and high-temperature resistant container is selected from alumina or quartz crucible.

9. The preparation method according to claim 4, characterized in that: The microwave sintering conditions include: heating to 100-450°C at a rate of 60-150°C / min, and sintering for 0.1-1h; Preferably, the microwave frequency of the microwave sintering is 5-35 GHz.

10. A lithium ion battery, characterized in that: It comprises the sulfide solid electrolyte as described in any one of claims 1 to 3 / or the sulfide solid electrolyte prepared by the preparation method as described in any one of claims 4 to 9.

Citation Information

Patent Citations

  • Sulfide-based solid electrolyte for lithium ion battery

    CN105229841A

  • Preparation method of sulfide solid electrolyte

    CN111908437A

  • Sulfide solid-state electrolyte, preparation method thereof, solid-state electrolyte sheet and solid-state battery

    CN113839086A

  • Sulfide solid electrolyte and preparation method and application thereof

    CN114976220A

  • High-performance sulfide solid electrolyte material, preparation method thereof and application of high-performance sulfide solid electrolyte material in all-solid-state battery

    CN115377483A

Cited By

  • Composite silicon negative electrode material and preparation method and application thereof

    CN120727806A

  • High-entropy all-solid-state electrolyte and preparation method and application thereof

    CN121355360A

  • Sulfide electrolyte, preparation method thereof and solid-state battery

    CN121812764A

  • Sulfide solid-state electrolyte and preparation method therefor, battery, and electric device

    WO2026218792A1