Electrolyte and battery

By using -OLi-containing quinoline compounds and carbonate additives in the lithium-ion battery electrolyte, combined with sulfur-containing additives, a uniform and dense membrane structure is formed, the problem of insufficient oxidation resistance of lithium-ion batteries at high voltages is solved. , significantly improves the battery's circulation and storage performance.

CN118943489APending Publication Date: 2024-11-12EVE ENERGY CO LTD

Patent Information

Application Number
CN202410994555.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have insufficient oxidation resistance at high voltages, resulting in reduced performance. Existing methods such as increasing lithium salt concentration, using new high-voltage electrolyte solvents or additives have high costs, low-temperature performance or poor negative electrode compatibility. Good and other problems, there is a lack of practical high-pressure positive electrode film forming additives.

Method used

Introduce quinoline compounds containing -OLi as the first functional additive, combining carbonate additives and sulfur-containing additives to form uniform and dense positive electrode CEI and negative electrode SEI films, enhancing interface stability, reducing side reactions, and improving high-voltage batteries loop and storage performance.

Benefits of technology

It effectively improves the room temperature, high temperature circulation and high temperature storage characteristics of high voltage batteries, enhances the stability and lithium conductivity of positive and negative electrode interfaces, optimizes the cycling performance of the battery, especially the performance under high temperature conditions is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943489A_ABST
    Figure CN118943489A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte and a battery. The electrolyte comprises a lithium salt, an organic solvent, a carbonic ester additive and a first functional additive, according to the electrolyte, the quinoline compound additive containing-OLi is introduced, so that the electrolyte can directly participate in film formation of a positive electrode CEI, the uniformity and compactness of positive electrode film formation are effectively promoted, and the stability of a positive electrode interface is improved; and in addition, the electrolyte can act together with other additives such as a sulfur-containing additive and a carbonic ester additive, so that negative electrode SEI film formation is further promoted, and the interface stability of the negative electrode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to an electrolyte and a battery. Background Art

[0002] Lithium-ion batteries are the most widely used secondary batteries at present. They have many advantages such as high energy density, low self-discharge rate, and high potential difference. Their application fields include electronic equipment, electric vehicles, satellites, etc. However, with the continuous increase in human needs, the requirements for the energy density and safety performance of lithium-ion batteries are also getting higher and higher. Especially in special environments, the energy density of existing lithium-ion batteries can hardly meet people's current needs. High working voltage is one of the effective ways to improve the energy density of lithium-ion batteries. Under high working voltage, the electrolyte needs to have good oxidation resistance so that the electrolyte can ensure that the lithium-ion battery maintains a stable cycle under high voltage.

[0003] However, commercial lithium-ion battery electrolytes are generally composed of carbonate organic solvents and lithium hexafluorophosphate (LiPF6). Carbonate solvents are mainly composed of chain carbonates DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), DEC (diethyl carbonate), and cyclic carbonates PC (propylene carbonate), EC (ethylene carbonate), etc. Because they have low oxidation potentials, they cannot stably exist after oxidative decomposition under high voltage, which will reduce the performance of lithium-ion batteries. The pressure resistance of commercial electrolytes can usually be improved in the following ways:

[0004] (1) Increasing the lithium salt concentration in carbonate electrolytes increases the number of complexes between lithium ions and solvent molecules, which enhances the antioxidant properties of the complexed solvent molecules and the stability of the electrolyte. In addition, compared with traditional electrolytes, high-concentration electrolytes have enhanced flame retardancy and improved battery safety.

[0005] (2) Use new high-voltage electrolyte solvents to replace carbonate solvents. The new solvents include sulfones, nitriles, ionic liquids and fluorinated electrolytes. These new system electrolytes can meet the high voltage requirements to a certain extent.

[0006] (3) By adding high-voltage electrolyte additives to traditional carbonate electrolytes, the additives can preferentially decompose on the positive electrode surface to form a CEI film during battery cycling, which can protect the integrity of the high-voltage electrode material to a certain extent and reduce the side reactions caused by the contact between the high-voltage positive electrode and the electrolyte.

[0007] Although the first two methods can improve the high voltage resistance of the electrolyte to a certain extent, they both have certain limitations. High lithium salt concentration will lead to high cost of the electrolyte. Sulfone solvents and ionic liquids have relatively high melting points, which reduces their performance at low temperatures. The poor compatibility of nitrile with graphite negative electrodes also limits the practical application of new solvent system electrolytes. In comparison, the third method, high-voltage electrolyte positive electrode additives, can simply and effectively improve the high voltage resistance of the electrolyte. However, there are currently few types of high-voltage positive electrode film-forming additives that can be used on the market. Therefore, the development of new practical positive electrode film-forming high-voltage electrolyte positive electrode additives is still an urgent problem to be solved. Summary of the invention

[0008] In order to solve the problems and deficiencies in the prior art, the present invention provides an electrolyte and a battery. The electrolyte can not only directly participate in the film formation of the positive electrode CEI by introducing a quinoline compound additive containing -OLi, effectively promote the uniformity and compactness of the positive electrode film formation, and improve the positive electrode interface stability, but also can work together with other additives such as sulfur-containing additives and carbonate additives to further promote the negative electrode SEI film formation and improve the negative electrode interface stability. Therefore, the electrolyte provided by the present invention can form uniform and dense CEI and SEI films at the positive and negative interfaces, effectively inhibit the side reactions at the positive and negative electrode interfaces, and thus effectively improve the normal temperature, high temperature cycle and high temperature storage characteristics of the high-voltage battery system.

[0009] According to a first aspect of the present invention, an electrolyte is provided, comprising a lithium salt, an organic solvent, a carbonate additive, and a first functional additive; the structural formula of the first functional additive is as follows: Wherein R1, R2, R3, R4, R5, and R6 are each independently selected from hydrogen, C1-C10 straight chain or branched alkyl or alkoxy, C1-C10 straight chain or branched alkyl or alkoxy substituted with halogen, C3-C10 straight chain or branched alkenyl, C3-C10 straight chain or branched alkynyl, C6-C26 unsubstituted aryl, C6-C26 aryl substituted with alkyl, and / or hydroxyl, and / or halogen, C7-C27 unsubstituted aryl, and C7-C27 benzyl substituted with alkyl, and / or hydroxyl, and / or halogen.

[0010] In the electrolyte provided by the present invention, the first functional additive introduced is a quinoline compound containing -OLi. Compared with other hydroxyquinoline additives (containing benzyl hydroxyl groups in the structure and easy to oxidize), the additive participates in the dense and uniform film formation of the positive electrode CEI, which can effectively improve the interfacial stability of the CEI film, and will not introduce active hydrogen protons (if it is a compound similar to 8-hydroxyquinoline, containing hydroxyl groups, it will introduce active hydrogen protons, increase the interfacial reaction activity, deteriorate the interfacial stability, and be detrimental to the high-temperature cycle performance of the battery), which can effectively improve the room temperature and high temperature cycle and storage performance of the high-voltage system. In addition, the -OLi group contained in the first functional additive can indirectly supplement lithium from the positive electrode to the negative electrode to compensate for the lithium loss caused by the formation of the SEI film on the negative electrode, thereby further improving the stability of the negative electrode SEI film and further optimizing the cycle performance of the battery.

[0011] At the same time, the electrolyte provided by the present invention also contains carbonate additives, which mainly participate in the formation of a good SEI film at the negative electrode. The carbonate additives work together with the first functional additive to not only further improve the stability of the negative electrode interface, but also have a significant effect on further improving the stability of the positive electrode interface. Therefore, the two additives are used together to form a dense and uniform CEI and SEI film at the positive and negative electrode interfaces, further optimize the positive and negative electrode interface stability, reduce the positive and negative electrode interface side reactions, and further optimize the cycle stability of the battery using it, especially for the normal temperature, high temperature cycle and high temperature storage characteristics of the battery.

[0012] Preferably, the mass proportion of the first functional additive in the electrolyte is 0.8-1.5%. If the first additive is too little, the interface film formed at the positive electrode interface will be dense and uniform, and it will not be able to effectively improve the positive electrode interface stability with other additives. At the same time, because the positive and negative poles have a certain mutual influence, the stability of the negative electrode interface will also decrease, resulting in a decrease in the degree of optimization of the battery performance. Too much first additive, on the one hand, will limit the role of other electrolyte additives or other components of the electrolyte, and deteriorate the overall performance of the electrolyte. Therefore, if the first functional additive is too much, it will also deteriorate the stability of the electrolyte, that is, it will not be conducive to further improving the stability of the positive and negative electrode interfaces, and the cycle performance of the battery will be reduced. At the same time, too much first additive will also transition into a film, which is not conducive to the deintercalation and insertion of lithium ions, and therefore is not conducive to the cycle performance of the battery.

[0013] Preferably, the electrolyte provided by the present invention also includes a second functional additive, which is a sulfur-containing additive, and the sulfur-containing additive includes at least one of vinyl sulfate, 1,3-propane sultone, and propenyl-1,3-sultone; the mass proportion of the sulfur-containing additive in the electrolyte is 0.3-0.9%. The above-mentioned sulfur-containing additives assist film formation at the negative electrode and have high thermal stability. Too little addition is not conducive to the formation of a dense SEI film at the negative electrode, and too much addition will cause transitional film formation, which is not conducive to the deintercalation of lithium ions, resulting in decreased cycle performance. And too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte.

[0014] Preferably, the sulfur additive includes vinyl sulfate and 1,3-propane sultone; or, the sulfur-containing additive includes vinyl sulfate and propenyl-1,3-sultone; or, the sulfur-containing additive includes vinyl sulfate, 1,3-propane sultone and propenyl-1,3-sultone. In the combination of the above sulfur-containing additives, these combinations and the first additive will not only not have obvious adverse reactions, but also can produce certain synergistic effects when used in such a combination, thereby further enhancing the interfacial stability and lithium conductivity of the CEI and SEI membranes, and effectively improving the room temperature and high temperature cycle and storage performance of high-voltage battery systems such as ternary systems.

[0015] Preferably, the first functional additive comprises at least one of the following structural formulas:

[0016]

[0017] Preferably, the carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; the mass proportion of the carbonate additive in the electrolyte is 0.2-0.6%. Carbonate additives such as vinylene carbonate (VC) and fluoroethylene carbonate (FEC) form a film at the negative electrode, but too little addition will not form a dense SEI film, and too much addition will lead to high impedance and high-temperature gas production. At the same time, too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte, which is not conducive to the comprehensive performance of the electrolyte.

[0018] Preferably, the electrolyte provided by the present invention also includes a lithium salt additive, and the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); the mass proportion of the lithium salt additive in the electrolyte is 0.5-1.0%. The lithium salt additive also has the function of forming positive and negative electrodes, and can further improve the density of the generated CEI film and SEI film, inhibit the dissolution of positive electrode metal ions, reduce the damage of metal ions to the negative electrode SEI film, and improve the thermal stability of the film. If the amount of addition is too small, a dense SEI film cannot be formed, and if the amount of addition is too large, gas production and electrical performance will be reduced.

[0019] Preferably, the lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

[0020] Preferably, the organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0021] Preferably, when the organic solvent includes ethylene carbonate and ethyl methyl carbonate, calculated by volume fraction, the volume fractions of ethylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate in the organic solvent are 20-40%, 0-20%, 0-20% and 30-50%, respectively.

[0022] According to the second aspect of the present invention, a battery is provided, comprising the above-mentioned electrolyte. By using the electrolyte provided by the present invention, a uniform and dense CEI film and SEI film can be formed on both sides of the positive and negative electrodes of the battery, which greatly optimizes the stability of the positive and negative electrode interfaces, while enhancing the lithium conductivity of the positive and negative electrodes, and improving the lithium ion transmission efficiency, thereby significantly optimizing the normal temperature and high temperature cycle and storage performance of the battery using the electrolyte. In particular, the introduction of the quinoline compound additive of -OLi plays a key role in further improving the compactness and uniformity of the positive electrode CEI film, greatly improving the stability of the positive electrode interface, and making the cycle performance optimization effect of the battery more obvious. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0024] The quinoline compounds containing -OLi used in the following examples and comparative examples are

[0025] They are denoted as A1, A2, A3, and A4 respectively. The synthesis method of A1-A4 is as follows: add the corresponding quinoline of A1-A4 quinoline lithium to acetonitrile (acetonitrile = 1g: 5ml), heat the solution to 40°C-50°C and keep the temperature constant for 2-4 hours, add lithium hydride in an amount 1.5 times the mass of A1-A4 quinoline in batches during the constant temperature period, and the addition rate is 1 / 20 of the total mass of lithium hydride added every 10 minutes, and it takes 3 hours to complete the feeding; after the addition is completed, keep the temperature at 40°C-50°C for 5 hours, filter the reaction solution, and the obtained yellow filter cake is the crude product of A1-A4 quinoline lithium, and then obtain A1-A4 quinoline lithium with higher purity through static crystallization.

[0026] Example 1

[0027] 1. Electrolyte and preparation of electrolyte

[0028] The electrolyte in this embodiment is composed of an organic solvent, a lithium salt and an additive, wherein the lithium salt is an electrolyte salt. The additives are carbonate additives, lithium salt additives, first functional additives, and second functional additives (sulfur-containing additives). The carbonate additive is fluoroethylene carbonate (FEC), and its mass fraction in the electrolyte is 0.4%. The lithium salt additive is lithium difluorophosphate (LiPO2F2), and its mass fraction in the electrolyte is 1.0%. The sulfur-containing additive is 1,3-propane sultone (PS), and its mass fraction in the electrolyte is 0.6%. The first additive is The mass fraction in the electrolyte is 1.1%. The lithium salt is lithium hexafluorophosphate (LiPF6), and its concentration in the electrolyte is 1.0 mol / L. The organic solvent is composed of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate. Taking the total volume of the organic solvent as 100%, the volume fraction of ethylene carbonate is 30%, the volume fraction of diethyl carbonate is 20%, and the volume fraction of ethyl methyl carbonate is 50%.

[0029] The preparation of the electrolyte follows the following steps: in an argon atmosphere, add the carbonate additive, lithium salt additive, first additive and sulfur-containing additive to an organic solvent, and finally add lithium hexafluorophosphate (lithium salt) and stir at low temperature to mix evenly.

[0030] 2. Preparation of batteries

[0031] The battery of this embodiment includes a positive electrode, a negative electrode, an electrolyte, and a separator.

[0032] In the preparation of the positive electrode sheet, the positive electrode active material is a nickel-cobalt-manganese ternary material (Li(Ni x Co y Mn z)O2) (where 0.5 ≤ x < 0.8, 0 < y ≤ 0.3, 0 < z ≤ 0.3 and x + y + z = 1). And the preparation method of the positive electrode sheet is as follows: Prepare a slurry by mixing the positive electrode active material (NCM523 in this embodiment), the conductive agent acetylene black, and the binder PVDF according to a mass ratio of 94:3:3, coat it on an aluminum foil current collector, and dry it in vacuum to obtain the positive electrode sheet.

[0033] In the preparation of the negative electrode sheet, the negative electrode active material is graphite. And the preparation method of the negative electrode sheet is as follows: Prepare a slurry by mixing the negative electrode active material graphite, the conductive agent acetylene black, and the binders CMC and SBR according to a mass percentage of 94:1:2:3, coat it on a copper foil current collector, and dry it in vacuum to obtain the negative electrode sheet.

[0034] After assembling the positive and negative electrode sheets prepared above with a Celgard 2400 separator to obtain an electric core, transfer the electric core into a casing, and then inject the electrolyte prepared in this embodiment, and perform formation and constant volume to obtain the battery of this embodiment.

[0035] Example 2

[0036] 1. Electrolyte and preparation of electrolyte

[0037] The electrolyte in this embodiment is different from that in Example 1 in that: Adjust the mass fraction of the first functional additive in the electrolyte to 0.8%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Example 1.

[0038] And the preparation of the electrolyte in this embodiment is the same as that in Example 1.

[0039] 2. Preparation of battery

[0040] The preparation of the battery in this embodiment is the same as that in Example 1.

[0041] Example 3

[0042] 1. Electrolyte and preparation of electrolyte

[0043] The electrolyte in this embodiment is different from that in Example 1 in that: Adjust the mass fraction of the first functional additive in the electrolyte to 1.4%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Example 1.

[0044] And the preparation of the electrolyte in this embodiment is the same as that in Example 1.

[0045] 2. Preparation of battery

[0046] The preparation of the battery in this embodiment is the same as that in Example 1.

[0047] Example 4

[0048] 1. Electrolyte and preparation of electrolyte

[0049] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 0.6%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0050] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0051] 2. Preparation of batteries

[0052] The preparation of the battery in this example is consistent with that in Example 1.

[0053] Example 5

[0054] 1. Electrolyte and preparation of electrolyte

[0055] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 1.7%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0056] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0057] 2. Preparation of batteries

[0058] The preparation of the battery in this example is consistent with that in Example 1.

[0059] Example 6

[0060] 1. Electrolyte and preparation of electrolyte

[0061] The electrolyte in this embodiment is different from that in the embodiment 1 in that the sulfur-containing additive is adjusted to diethyl sulfate (DTD). The rest is the same as that in the embodiment 1.

[0062] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0063] 2. Preparation of batteries

[0064] The preparation of the battery in this example is consistent with that in Example 1.

[0065] Example 7

[0066] 1. Electrolyte and preparation of electrolyte

[0067] The electrolyte in this embodiment is different from that in Embodiment 1 in that the sulfur-containing additive is adjusted to be vinyl sulfate (DTD) and 1,3-propane sultone (PS), and the mass fractions of DTD and PS in the electrolyte are 0.4% and 0.2% respectively. The rest is the same as that in Embodiment 1.

[0068] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0069] 2. Preparation of batteries

[0070] The preparation of the battery in this example is consistent with that in Example 1.

[0071] Example 8

[0072] 1. Electrolyte and preparation of electrolyte

[0073] The electrolyte in this embodiment is different from that in Embodiment 1 in that the sulfur-containing additive is adjusted to vinyl sulfate (DTD), 1,3-propane sultone (PS) and propenyl-1,3-sultone (PST), and the mass fractions of DTD, PS and PST in the electrolyte are 0.3%, 0.2% and 0.1% respectively. The rest is the same as that in Embodiment 1.

[0074] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0075] 2. Preparation of batteries

[0076] The preparation of the battery in this example is consistent with that in Example 1.

[0077] Example 9

[0078] 1. Electrolyte and preparation of electrolyte

[0079] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to The rest is consistent with Example 1.

[0080] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0081] 2. Preparation of batteries

[0082] The preparation of the battery in this example is consistent with that in Example 1.

[0083] Example 10

[0084] 1. Electrolyte and preparation of electrolyte

[0085] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to The rest is consistent with Example 1.

[0086] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0087] 2. Preparation of batteries

[0088] The preparation of the battery in this example is consistent with that in Example 1.

[0089] Embodiment 11

[0090] 1. Electrolyte and preparation of electrolyte

[0091] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to The rest is consistent with Example 1.

[0092] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0093] 2. Preparation of batteries

[0094] The preparation of the battery in this example is consistent with that in Example 1.

[0095] Example 12

[0096] 1. Electrolyte and preparation of electrolyte

[0097] The electrolyte in this embodiment is different from that in Embodiment 9 in that the sulfur-containing additives are adjusted to be vinyl sulfate (DTD) and 1,3-propane sultone (PS), and the mass fractions of DTD and PS in the electrolyte are 0.4% and 0.2%, respectively. The rest is the same as that in Embodiment 9.

[0098] The preparation of the electrolyte in this embodiment is consistent with that in Example 9.

[0099] 2. Preparation of batteries

[0100] The preparation of the battery in this example is consistent with that in Example 9.

[0101] Example 13

[0102] 1. Electrolyte and preparation of electrolyte

[0103] The electrolyte in this embodiment is different from that in embodiment 11 in that the sulfur-containing additive is adjusted to be vinyl sulfate (DTD) and 1,3-propane sultone (PS), and the mass fractions of DTD and PS in the electrolyte are 0.4% and 0.2%, respectively. The rest is the same as that in embodiment 11.

[0104] The preparation of the electrolyte in this embodiment is consistent with that in Example 9.

[0105] 2. Preparation of batteries

[0106] The preparation of the battery in this example is consistent with that in Example 11.

[0107] Embodiment 14

[0108] 1. Electrolyte and preparation of electrolyte

[0109] The electrolyte in this embodiment is different from that in embodiment 11 in that the sulfur-containing additive is adjusted to vinyl sulfate (DTD), 1,3-propane sultone (PS) and propenyl-1,3-sultone (PST), and the mass fractions of DTD and PS in the electrolyte are 0.3%, 0.2% and 0.1%, respectively. The rest is the same as that in embodiment 11.

[0110] The preparation of the electrolyte in this embodiment is consistent with that in Example 11.

[0111] 2. Preparation of batteries

[0112] The preparation of the battery in this example is consistent with that in Example 11.

[0113] Comparative Example 1

[0114] 1. Electrolyte and preparation of electrolyte

[0115] The electrolyte in this comparative example is different from that in Example 1 in that the first functional additive is not added. The rest is the same as that in Example 1.

[0116] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0117] 2. Preparation of batteries

[0118] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0119] Comparative Example 2

[0120] 1. Electrolyte and preparation of electrolyte

[0121] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive is added (ie, no FEC is added). The rest is the same as in Example 1.

[0122] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0123] 2. Preparation of batteries

[0124] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0125] Comparative Example 3

[0126] 1. Electrolyte and preparation of electrolyte

[0127] The electrolyte in this comparative example is different from that in Example 1 in that the first additive is adjusted to 8-hydroxyquinoline. The rest is the same as in Example 1.

[0128] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0129] 2. Preparation of batteries

[0130] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0131] Comparative Example 4

[0132] 1. Electrolyte and preparation of electrolyte

[0133] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive (ie, no FEC) and no second additive (ie, no sulfur-containing additive PS) are added. The rest is the same as in Example 1.

[0134] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0135] 2. Preparation of batteries

[0136] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0137] Test Case

[0138] 1. Experimental Construction Method

[0139] The batteries (lithium-ion batteries) prepared in all the above embodiments and comparative examples were subjected to electrochemical tests using a Xinwei charge and discharge test cabinet.

[0140] (1) Cycle performance test of lithium-ion batteries:

[0141] At 25 or 45°C, charge the lithium-ion battery at a constant current of 1.0C (nominal capacity) to a voltage of 4.4V, then charge at a constant voltage of 4.4V to a current ≤0.05C. After standing for 10 minutes, discharge at a constant current of 1C to 2.8V. The above is one charge and discharge cycle.

[0142] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0143] (2) High temperature storage performance test of lithium-ion batteries:

[0144] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0145] The volume expansion ratio (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0)V0×100%.

[0146] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0147] The batteries obtained from the above examples and comparative examples were tested as follows:

[0148] (a) High temperature storage performance test of lithium-ion batteries:

[0149] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0150] The volume expansion rate (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0) / V0×100%.

[0151] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0152] (b) High temperature storage experiment:

[0153] Carry out 5 charge and discharge cycle tests at room temperature at a charge and discharge rate of 1C, and then charge to full charge at a rate of 1C. Record the 1C capacity Q0 and battery volume V0 respectively. Store the fully charged battery at 60°C for 90 days, record the battery volume V1 and 1C discharge capacity Q1, then charge and discharge the battery at room temperature at a rate of 1C for 5 weeks, record the 1C discharge capacity Q2, and calculate the experimental data such as the battery's high temperature storage capacity retention rate, capacity recovery rate and volume change rate. The recorded results are shown in Table 1 below. The calculation formulas used are as follows: Capacity retention rate (%) = Q1 / Q0×100%; Capacity recovery rate (%) = Q2 / Q0×100%; Volume change rate (%) = (V1-V0) / V0×100%.

[0154] (c) Normal temperature cycle test:

[0155] Place the battery at 25°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 weeks as A2, and calculate the capacity retention rate of the battery after 2000 weeks of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%.

[0156] (d) High temperature cycle test:

[0157] Place the battery at 45°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 cycles as A2, and calculate the capacity retention rate of the battery after 2000 cycles of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%, and record the result.

[0158] 2. Experimental results

[0159] The test results of the battery performance of the above embodiments and comparative examples are shown in Table 1 below.

[0160] Table 1 Related performance test results of batteries in embodiments and comparative examples

[0161]

[0162]

[0163] As can be seen from Table 1, the electrolyte provided by the present invention has high high-voltage stability, and can not only form a stable CEI film at the positive electrode interface, but also form a stable SEI film at the negative electrode interface, effectively inhibiting the side reactions at the positive and negative electrode interfaces, and can improve the room temperature, high temperature cycle and high temperature storage characteristics of the high-voltage battery system. For details, refer to Examples 1 to 14.

[0164] In comparative example 1, the first functional additive is not added, that is, the functional additive containing both a disulfide bond and a thiophene structure is not added, and the normal temperature and high temperature cycle performance deteriorates, which eventually leads to the deterioration of the high temperature storage performance and the increase of the production period.

[0165] In Comparative Example 2, no carbonate additive is added (ie, no FEC is added), and the room temperature and high temperature cycle performance deteriorates, which ultimately leads to poor high temperature storage performance and increased production period.

[0166] In Comparative Example 3, the first functional additive is 8-hydroxyquinoline, and the room temperature and high temperature cycle performance deteriorates, which ultimately leads to poor high temperature storage performance and increased production period.

[0167] In Comparative Example 4, no carbonate additive (ie, no FEC) and no second additive (ie, no sulfur-containing additive PS) were added, and the formed interface film was unstable, ultimately resulting in poor cycle and storage performance.

[0168] Further comparing Example 1 with Examples 2 to 5, the mass fractions of the first functional additive in the electrolyte in Examples 4 and 5 are 0.6% and 1.7%, respectively. If the mass fraction is too small, the interface film formed is unstable and the side reaction cannot be effectively reduced. If the mass fraction is too large, the interface film formed is too thick, which affects the cycle and storage performance of the battery. And further comparing Examples 1 to 3, it can be found that when the mass fraction of the first functional additive in the electrolyte is 1.1%, the high temperature storage performance, normal temperature cycle performance and high temperature cycle performance of the battery are better.

[0169] By comparing Example 1 with Examples 6 to 8, it can be found that adjusting the type of sulfur-containing additive will also affect the performance of the battery. And after comparison, it can be found that when the sulfur-containing additive is the first additive, the battery has better cycle and storage performance. This shows that under such a combination, the high-voltage stability of the electrolyte can be further improved, the positive and negative interface stability can be optimized, and the high-temperature storage performance, room temperature cycle performance and high-temperature cycle performance of the battery can be further optimized.

[0170] At the same time, it can be further observed that in Example 1 and Examples 9 to 11, when the type of the first functional additive is changed, the battery can also maintain good or even better performance.

[0171] In addition, it can be further observed that Example 9 and Example 12, Example 11 and Example

[0172] 13. From Examples 11 and 14, it can be seen that further adjusting the combination of the first additive and the sulfur-containing additive can further optimize the high-voltage stability of the electrolyte, and further optimize the high-temperature storage performance, room-temperature cycle performance, and high-temperature cycle performance of the battery. From these examples, the combination of the first additives such as DTD and PST and the sulfur-containing additive is more conducive to further improving the performance of the battery.

[0173] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: Including lithium salt, organic solvent, carbonate additive, first functional additive; The structural formula of the first functional additive is as follows: Wherein R1, R2, R3, R4, R5, and R6 are each independently selected from hydrogen, C1-C10 straight chain or branched alkyl or alkoxy, C1-C10 straight chain or branched alkyl or alkoxy substituted with halogen, C3-C10 straight chain or branched alkenyl, C3-C10 straight chain or branched alkynyl, C6-C26 unsubstituted aryl, C6-C26 aryl substituted with alkyl, and / or hydroxyl, and / or halogen, C7-C27 unsubstituted aryl, and C7-C27 benzyl substituted with alkyl, and / or hydroxyl, and / or halogen.

2. The electrolyte according to claim 1, characterized in that: The mass proportion of the first functional additive in the electrolyte is 0.8-1.5%.

3. The electrolyte according to claim 1, characterized in that: Also included is a second functional additive, wherein the second functional additive is a sulfur-containing additive, and the sulfur-containing additive includes at least one of vinyl sulfate, 1,3-propane sultone, and propenyl-1,3-sultone; The sulfur-containing additive accounts for 0.3-0.9% by mass in the electrolyte.

4. The electrolyte according to claim 3, characterized in that: The sulfur-containing additive includes the vinyl sulfate and the 1,3-propane sultone; Or, the sulfur-containing additive includes the vinyl sulfate and the propenyl-1,3-sultone; Alternatively, the sulfur-containing additive includes the vinyl sulfate, the 1,3-propane sultone, and the propenyl-1,3-sultone.

5. The electrolyte according to claim 1, characterized in that: The first functional additive comprises at least one of the following structural formulas:

6. The electrolyte according to claim 1, characterized in that: The carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; The carbonate additive accounts for 0.2-0.6% by weight in the electrolyte.

7. The electrolyte according to claim 1, characterized in that: Also included is a lithium salt additive, wherein the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); The lithium salt additive accounts for 0.5-1.0% by mass in the electrolyte.

8. The electrolyte according to claim 1, characterized in that: The lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

9. The electrolyte according to claim 1, characterized in that: The organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

10. A battery, characterized in that: Comprising the electrolyte as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Electrolyte additive and lithium ion battery containing electrolyte additive

    CN102324564A

  • Electrolyte and battery containing same

    CN118017005A

  • Lithium battery

    JP1990158059A

  • Compound, additive agent, electrolytic solution and lithium ion secondary battery

    JP2017069146A

  • Solid-state secondary battery and manufacturing method thereof

    US20220149429A1

Cited By

  • Electrolyte and application thereof

    CN119764557A

  • An electrolyte and its application

    CN119764557B