Composite solid polymer electrolyte material and preparation method and application thereof
By using composite solid polymer electrolyte materials in zinc ion batteries, the problems of low ion conductivity and narrow electrochemical stability window of solid zinc ion batteries are solved, and high ion conductivity and wide voltage stability window are achieved, suitable for flexible Wearing equipment and energy storage systems.
Patent Information
- Application Number
- CN202411269410.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
AI Technical Summary
The existing solid zinc ion batteries have low room temperature ion conductivity and narrow electrochemical stability windows, making it difficult to meet the needs of flexible wearable devices and energy storage systems.
Using the preparation method of composite solid polymer electrolyte materials, polyethylene oxide PEO and Zn(CF3SO3)2 were added to the solvent and carbonized polymer points were added to prepare high ionic conductivity and wide voltage by solution casting. Stabilize window electrolyte material.
It realizes high room temperature ionic conductivity and wide electrochemical stability window, provides excellent mechanical flexibility and long cycle stability, and is suitable for flexible wearable devices and energy storage systems.
Smart Images

Figure CN118943523A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery electrolyte materials, and in particular to a composite solid polymer electrolyte material and a preparation method and application thereof. Background Art
[0002] With the concept of sustainable development, development and environment are closely linked. Zinc-ion batteries have made breakthrough progress in electrode material preparation, electrolyte research and development, and mechanism exploration in recent years due to their advantages such as low cost, safety, and simple operation. However, a series of side reactions caused by aqueous electrolytes, such as the growth of zinc dendrites, the dissolution of negative electrode materials, and liquid leakage, remain to be solved.
[0003] Among them, the development of polymer-based solid electrolytes can alleviate the problems of corrosion, hydrogen evolution and other side reactions caused by the presence of water in aqueous zinc-ion batteries. However, there are still some key issues in the design and development of solid electrolytes, such as low ionic conductivity at room temperature and narrow electrochemical stability window. Carbonized polymer dots have a special organic-inorganic composite core-shell structure. This unique structure makes it have excellent compatibility with polymers, which can effectively reduce the crystallinity of polymer electrolytes and improve the ionic conductivity of electrolytes. Summary of the invention
[0004] The purpose of the present invention is to provide a composite solid polymer electrolyte material and a preparation method and application thereof. The preparation method is simple to operate, and the obtained electrolyte material is smooth and flat as a whole, has high room temperature ionic conductivity and good cycle stability. After the material is installed into an all-solid-state zinc ion battery, it can be applied to flexible wearable devices and energy storage systems.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The present invention first provides a method for preparing a composite solid polymer electrolyte material, comprising:
[0007] Step 1: Preparation of carbonized polymer dots;
[0008] Step 2: Add polyethylene oxide PEO and Zn(CF 3 SO 3 ) 2 A pure PEO electrolyte is prepared, and then the carbonized polymer dots in step 1 are added to obtain a mixed solution, which is stirred, and a composite solid polymer electrolyte material is obtained by solution casting and drying.
[0009] Preferably, the method for preparing carbonized polymer dots in step 1 comprises:
[0010] 1) Dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction to obtain a brown solution;
[0011] 2) The brown solution of step 1) is dialyzed and freeze-dried to obtain carbonized polymer dots.
[0012] Preferably, the reaction temperature in step 1) is 180° C. and the reaction time is 5 h.
[0013] Preferably, the solvent in step 2 is acetonitrile.
[0014] Preferably, the polyethylene oxide PEO and Zn(CF 3 SO 3 ) 2 The mass ratio is 0.5:0.206.
[0015] Preferably, the amount of carbonized polymer dots added is Zn(CF 3 SO 3 ) 2 1-4% of mass.
[0016] Preferably, the amount of carbonized polymer dots added is Zn(CF 3 SO 3 ) 2 3% of mass.
[0017] Preferably, the stirring temperature in step 2 is room temperature, and the stirring time is 8-10 hours.
[0018] The present invention also provides a composite solid polymer electrolyte material obtained by the above preparation method.
[0019] The present invention also provides application of the composite solid polymer electrolyte material in a solid zinc ion battery.
[0020] Beneficial Effects of the Invention
[0021] The present invention provides a composite solid polymer electrolyte material and its preparation method and application. The material mainly utilizes the characteristics that the functional groups on the surface of carbonized polymer dots are easy to regulate and can form covalent bonds with polymers to change the length of polymer chain segments on the surface of carbonized polymer dots to regulate the crystallization behavior of polymers. The composite solid polymer electrolyte material provided by the present invention has excellent mechanical flexibility, high ionic conductivity, wide voltage stability window, and good cycle stability, and can be applied to flexible wearable devices and energy storage systems.
[0022] The composite solid polymer electrolyte material provided by the invention has simple preparation process, mild synthesis conditions and low preparation cost.
[0023] The composite solid polymer electrolyte provided by the present invention can be used in a solid zinc ion battery assembled using the composite solid polymer electrolyte, and can be applied to flexible wearable devices and energy storage devices. The zinc symmetric battery assembled using the composite solid polymer electrolyte membrane has a high conductivity at 2 mA cm -2 It can stably cycle for more than 1400 h at a current density of , and the electrochemical stability window can reach 2.902V. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a SEM image of the composite solid polymer electrolyte material prepared in Example 1;
[0025] Figure 2 The physical picture and flexibility display of the composite solid polymer electrolyte membrane prepared in Example 1;
[0026] Figure 3 This is a crystallinity test diagram of the composite solid polymer electrolyte membrane prepared in Example 1;
[0027] Figure 4 Electrochemical stability window test of the composite solid polymer electrolyte material prepared in Example 1;
[0028] Figure 5 This is a cycle stability diagram of the composite solid polymer electrolyte material prepared in Example 1;
[0029] Figure 6 The ionic conductivity of the composite solid polymer electrolytes prepared in Example 2 and Comparative Example 1 with different carbonized polymer dot addition amounts was tested. DETAILED DESCRIPTION
[0030] The present invention first provides a method for preparing a composite solid polymer electrolyte material, comprising:
[0031] Step 1: Prepare carbonized polymer dots; the specific preparation is preferably: dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction, preferably at 180°C for 5 hours to obtain a brown solution, and then dialyze the brown solution, preferably using a dialysis bag with a molecular weight cutoff of 200D for 48 hours with water, change the water 3 times, and obtain carbonized polymer dots after freeze drying. The mass of citric acid g: the volume of ethylenediamine μL is 1.921:670;
[0032] Step 2: Add polyethylene oxide PEO and Zn(CF 3 SO 3 ) 2Prepare pure PEO electrolyte, the solvent is preferably acetonitrile, then add the carbonized polymer dots in step 1, and stir the obtained mixed solution, the stirring temperature is preferably room temperature, the stirring time is preferably 8-10 hours, and the composite solid polymer electrolyte material is obtained by solution casting and drying. The polyethylene oxide PEO and Zn(CF 3 SO 3 ) 2 The mass ratio of is preferably 0.5:0.206, and the amount of the carbonized polymer dots added is preferably Zn(CF 3 SO 3 ) 2 1-4% by mass, more preferably 3%.
[0033] The present invention also provides a composite solid polymer electrolyte material obtained by the above preparation method, and the electrolyte material is smooth and flat as a whole.
[0034] The present invention also provides application of the composite solid polymer electrolyte material in a solid zinc ion battery.
[0035] In the application of the composite solid polymer electrolyte material provided by the present invention, preferably, the composite solid polymer electrolyte material is assembled, a stainless steel sheet is used as a working electrode, a zinc sheet is used as a counter electrode and a reference electrode to form a half-cell, and the electrochemical stability window can reach 2.902V.
[0036] The present invention is further described in detail below with reference to specific examples, in which the raw materials involved are all commercially available.
[0037] Comparative Example 1
[0038] Preparation of PEO-based solid polymer electrolyte:
[0039] 0.5g PEO, 0.206g Zn(CF 3 SO 3 ) 2 Dissolve it in a sample bottle containing 10 mL of acetonitrile solution, stir it magnetically for 10 hours, and then use the solution casting method to dry it at room temperature for about 6 hours to obtain a pure PEO-based solid polymer electrolyte membrane, which is finally cut into 16 mm small discs for use.
[0040] Example 1
[0041] Preparation of carbonized polymer dots: 1.921 g of citric acid and 670 uL of ethylenediamine were dissolved in 60 mL of deionized water and stirred evenly. The mixture was then transferred to a 100 mL polytetrafluoroethylene reactor and reacted at 180 °C for 5 h to obtain a brown solution. The solution was dialyzed with water using a dialysis bag with a molecular weight cutoff of 200 for 48 h, and the water was changed 3 times. The obtained solution was freeze-dried to obtain a dark brown carbonized polymer dot powder.
[0042] Preparation of composite solid electrolyte: 0.5 g PEO, 0.206 g Zn(CF 3 SO 3 ) 2 A uniform electrolyte solution was obtained under magnetic stirring. Then, carbonized polymer dots were added at a mass ratio of 3% to zinc salt. The mixture was stirred continuously at room temperature for 10 hours, and then dried at room temperature for about 6 hours to obtain a PEO-based electrolyte membrane by solution casting, which was finally cut into 16 mm small discs.
[0043] The SEM image of the composite solid polymer electrolyte membrane of Example 1 is as follows: Figure 1 As shown, Figure 1 A represents the PEO-based solid polymer electrolyte membrane of Comparative Example 1, Figure 1 B represents the composite solid electrolyte membrane prepared in Example 1, Figure 1 It can be seen that the electrolyte microscopic surface presents a uniformly distributed water ripple shape, which is smooth and flat as a whole, which is beneficial to reducing the interfacial impedance of the electrolyte-electrode interface.
[0044] Figure 2 The actual picture (2A) and flexibility display (2B) of the composite solid polymer electrolyte membrane prepared in Example 1; it can be seen from the figure that the electrolyte material of the present invention has excellent mechanical flexibility and can be applied to flexible wearable devices and energy storage systems.
[0045] The crystallinity of the composite solid polymer electrolyte material of Example 1 was obtained by XRD test. Figure 3 As shown. Figure 3 It can be seen that the PEO matrix has two obvious characteristic diffraction peaks at 2θ of 19.09° and 23.37°, indicating that pure PEO has a higher degree of crystallinity. The intensity of the two crystallization peaks of the composite solid polymer electrolyte material after adding carbonized polymer dots is reduced, indicating that the crystallinity of the polymer electrolyte is reduced, which is conducive to the movement of chain segments and improves the ion transport kinetics.
[0046] The LSV diagram of the composite solid polymer electrolyte material of Example 1 is as follows: Figure 4 The prepared composite polymer electrolyte membrane was assembled into a half-cell, and the electrochemical stability window of the electrolyte was tested by linear sweep voltammetry. The electrochemical oxidation decomposition of the electrolyte could be judged based on the obvious oxidation current. The scan rate was 1 mV s -1 .like Figure 4 As shown, the oxygen evolution potential of the composite polymer electrolyte reaches 2.902 V, and the current trend is very stable, indicating that the electrolyte is very stable in this voltage range and does not decompose.
[0047] The cyclic stability of the composite solid polymer electrolyte material of Example 1 is as follows Figure 5 As shown, Zn|CPD-CPE|Zn battery at 2mAcm -2 It cycled stably for 1430 h at the current density, showing good cycle stability and cycle life.
[0048] Example 2
[0049] Preparation of composite solid electrolytes with different carbonized polymer dot contents:
[0050] Carbonized polymer dots were prepared according to the method of Example 1;
[0051] 0.5 g PEO, 0.206 g Zn(CF 3 SO 3 ) 2 , a uniform electrolyte solution was obtained under magnetic stirring. Then carbonized polymer dots were added at a mass ratio of 1%, 2%, and 4% to zinc salt, and the mixture was stirred continuously at room temperature for 10 hours. Then, electrolyte membranes with different carbonized polymer dot contents were obtained by solution casting and dried at room temperature for about 6 hours, and finally cut into 16 mm small discs for use.
[0052] The ionic conductivity of the composite solid polymer electrolytes obtained in Examples 1-2 and Comparative Example 1 was tested to explore the effect of carbonized polymer dots on the ion transport kinetics in the solid polymer electrolytes. Figure 6 As shown in Figure 2, when the carbonized polymer dots content is 3%, the composite solid polymer electrolyte exhibits the highest ionic conductivity. The ionic conductivity of PEO-3% CPD at 50 °C is 4.055×10 -4 S cm -1 .
[0053] The above embodiments illustrate that the composite solid polymer electrolyte material provided by the present invention has a wide voltage window and stable long cycle performance. After the material is installed into an all-solid-state zinc ion battery, it can be applied to flexible wearable devices and energy storage systems.
Claims
1. A method for preparing a composite solid polymer electrolyte material, characterized in that: include: Step 1: Preparation of carbonized polymer dots; Step 2: Add polyethylene oxide PEO and Zn(CF3SO3)2 into the solvent to prepare pure PEO electrolyte, then add the carbonized polymer dots prepared in step 1, stir the obtained mixed solution, cast the mixed solution, and dry the mixed solution to obtain a composite solid polymer electrolyte material.
2. The method for preparing a composite solid polymer electrolyte material according to claim 1, characterized in that: The method for preparing carbonized polymer dots in step 1 comprises: 1) Dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction to obtain a brown solution; 2) The brown solution of step 1) is dialyzed and freeze-dried to obtain carbonized polymer dots.
3. The method for preparing a composite solid polymer electrolyte material according to claim 2, characterized in that: The reaction temperature in step 1) is 180° C. and the reaction time is 5 h.
4. The method for preparing a composite solid polymer electrolyte material according to claim 1, characterized in that: The solvent in step 2 is acetonitrile.
5. The method for preparing a composite solid polymer electrolyte material according to claim 1, characterized in that: The mass ratio of polyethylene oxide PEO and Zn(CF3SO3)2 is 0.5:0.
206.
6. The method for preparing a composite solid polymer electrolyte material according to claim 1, characterized in that: The added amount of the carbonized polymer dots is 1-4% of the mass of Zn(CF3SO3)2.
7. The method for preparing a composite solid polymer electrolyte material according to claim 6, characterized in that: The added amount of the carbonized polymer dots is 3% of the mass of Zn(CF3SO3)2.
8. The method for preparing a composite solid polymer electrolyte material according to claim 1, characterized in that: The stirring temperature of step 2 is room temperature, and the stirring time is 8-10 hours.
9. The composite solid polymer electrolyte material obtained by the preparation method according to claim 1.
10. Use of the composite solid polymer electrolyte material according to claim 9 in a solid-state zinc ion battery.