Modified PVDF diaphragm and preparation method thereof
The nanofiber membrane is prepared by alkali treatment and electrospinning technology of PVDF, which solves the problem that zinc ion battery separators are easily penetrated by zinc dendrites, improves the cycle stability and electrochemical performance of the battery, and achieves a higher ratio Capacity and service life.
Patent Information
- Application Number
- CN202411284353.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The separator of aqueous zinc ion batteries is easily penetrated by zinc dendrites during charging and discharging, resulting in a short circuit in the battery. The existing high-performance separator such as Nafion is costly and relies on imports, which limits its large-scale promotion.
By alkali treatment of PVDF, hydrophilic functional groups are increased, and nanofiber membranes are prepared by electrospinning technology to improve the water absorption and mechanical strength of the membrane, forming a porosity of 45-55%, a water absorption of 250-350%, and a fracture strength 8-9MPa alkali-treated modified PVDF nanofiber separator.
The mechanical and electrochemical properties of the diaphragm are significantly improved, the discharge specific capacity increases by 1.88 times, and the number of cycles exceeds 1,000 times, far exceeding the 400 times of traditional glass fiber diaphragm, extending the service life of the battery.
Smart Images

Figure CN118943650A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a diaphragm of an aqueous zinc ion battery and a preparation technology thereof. Background Art
[0002] The energy crisis is a major problem facing mankind. Secondary batteries with efficient electrical energy / chemical energy conversion are an effective green energy solution. Secondary batteries are also called rechargeable batteries, and their basic components include negative electrodes, positive electrodes, separators and electrolytes. Lithium-ion batteries are currently the dominant secondary batteries in the market, but the lack of lithium resources, high cost, poor safety, and potential safety hazards such as fire and explosion limit their large-scale promotion and application. Aqueous zinc-ion batteries have the advantages of abundant zinc reserves, low cost, safe operation, no environmental pollution and high ion conductivity, and are ideal green battery energy storage systems. The disadvantages of aqueous zinc-ion batteries are narrow window voltage, easy side reactions at the zinc negative electrode, and easy dissolution of the positive electrode active material, which leads to poor battery cycle stability.
[0003] The diaphragm is an important component of secondary batteries and has an important impact on the performance of the battery. The diaphragm can provide a physical barrier between the positive and negative electrodes of the battery to prevent the battery from short-circuiting. During the battery charge and discharge cycle, the diaphragm also has the function of allowing electrolyte ions to pass through. The composition, porosity, ionic conductivity and mechanical strength of the diaphragm will affect the transport behavior of ions inside the diaphragm and at the electrolyte-negative electrode interface, thereby affecting the cycle life of the negative electrode. The diaphragm of a zinc-ion battery is generally a glass fiber membrane several hundred microns thick with high hydrophilicity. However, the glass fiber diaphragm is very brittle, and the zinc dendrites generated during the charge and discharge process of the zinc-ion battery can easily penetrate the diaphragm and induce a battery short circuit. Therefore, there is an urgent need to develop high-performance diaphragms to further improve the electrochemical performance of the zinc negative electrode and the entire battery system.
[0004] Weijun et al. [Energy Storage Mater. 2022, 44: 57-65] used cotton cellulose as a diaphragm for aqueous zinc-ion batteries. The membrane has dense and uniform nanopores, good electrolyte wettability, excellent mechanical properties and high ionic conductivity. The disadvantage is that the cellulose diaphragm will expand in volume after being infiltrated with an aqueous electrolyte solution, which reduces the strength of the diaphragm and is easily penetrated by growing zinc dendrites, causing a short circuit in the battery. Meena et al. [Energy Technol. 2019: 1900442] used perfluorosulfonic acid resin Nafion as a diaphragm for zinc-vanadium batteries. The sulfonic acid groups in Nafion can attract zinc ions in the electrolyte in a directional manner, allowing zinc ions to pass through the diaphragm evenly, reducing the irregular deposition of zinc ions and the massive growth of zinc dendrites. The migration number of zinc ions bonded to the sulfonic acid group is 0.52, and the discharge specific capacity at 0.25A / g is 510mAh / g, close to its theoretical capacity of 589mAh / g, and the capacity retention rate after 1800 cycles is 88%. However, Nafion's cost is too high and it is heavily dependent on imports, which limits its large-scale promotion and application. Summary of the invention
[0005] To solve the above problems, the present invention proposes an alkali-treated modified PVDF membrane and a preparation method thereof, specifically, by subjecting PVDF to alkali treatment so that it contains a certain number of hydrophilic functional groups and exhibits suitable hydrophilic properties, and then utilizing electrospinning to process it into a nanofiber membrane, thereby further improving the water absorption and mechanical strength of the membrane.
[0006] The technical scheme adopted by the present invention is: alkali treatment is performed on PVDF to obtain hydrophilic modified PVDF, and then the alkali-treated modified PVDF nanofiber diaphragm is obtained by electrostatic spinning.
[0007] The first aspect of the present invention provides:
[0008] The invention discloses an alkali-treated modified PVDF nanofiber diaphragm, characterized by a porosity of 45-55%, a water absorption of 250-350%, a contact angle of 55-60 degrees, a breaking strength of 8-9 MPa, and an elongation of 7-8%.
[0009] The second technical solution of the present invention provides:
[0010] A method for preparing an alkali-treated modified PVDF nanofiber membrane, characterized in that:
[0011] (1) Add 5 g of PVDF to 50 mL of 0.3-0.7 mol / L alkali / ethanol solution, add 0.1-0.3 g of tetrabutylammonium bromide (TBAB), stir at 60° C. for 0.5-0.8 h, filter, wash the solid to neutrality, and dry to obtain a modified PVDF solid.
[0012] (2) Dissolve the modified PVDF solid obtained in step (1) in any one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone to obtain a spinning solution with a concentration of 17 wt%, and perform electrospinning to obtain an alkali-treated modified PVDF nanofiber membrane.
[0013] In the step (1), the base is NaOH or KOH, and the preferred concentration is 0.5 mol / L.
[0014] In the step (1), the preferred stirring time is 0.5 h and the amount of TBAB used is 0.15 g.
[0015] The alkali-treated modified PVDF nanofiber membrane prepared by the present invention has better mechanical properties than traditional glass fiber membranes. When applied to aqueous zinc ion battery membranes, the modified PVDF nanofiber membrane prepared by the present invention shows more excellent electrochemical performance, with a discharge capacity of 128 mAh / g at a current density of 1.0 A / g, which is 1.88 times that of glass fiber membrane batteries, and a cycle number of more than 1,000 times, which is much greater than the 400 times of glass fiber membrane batteries.
[0016] The beneficial effects of the present invention are:
[0017] (1) The present invention performs alkali treatment on PVDF to obtain alkali-treated modified PVDF, so that the PVDF has suitable hydrophilicity and can be used in aqueous batteries.
[0018] (2) The present invention utilizes electrospinning to prepare a modified PVDF nanofiber membrane, thereby further improving the mechanical properties, porosity and water absorption of the modified PVDF membrane.
[0019] (3) When the alkali-treated modified PVDF nanofiber membrane prepared by the present invention is used in aqueous zinc ion batteries, it has better specific capacity and cycle life than traditional glass fiber membranes. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The cyclic performance of the alkali-treated modified PVDF nanofiber membrane and glass fiber membrane obtained in Example 1 in a zinc ion battery at 1 A / g. DETAILED DESCRIPTION
[0021] To further illustrate the technical means adopted by the present invention, a specific description is given below in conjunction with the embodiments of the present invention and the accompanying drawings.
[0022] The specific embodiments of the present invention are as follows:
[0023] Example 1
[0024] (1) Alkali treatment of PVDF. Add 5 g of PVDF powder to 50 mL of 0.5 mol / L NaOH ethanol solution and stir at 60 °C for 0.5 h. The amount of TBAB added is 3 mg / mL. Filter and repeatedly rinse the collected PVDF powder with deionized water until it is neutral, and dry it at 105 °C for later use.
[0025] (2) Preparation of modified PVDF spinning solution: 1.6 g of modified PVDF powder was added to 10 mL of DMF and stirred with magnetic force at 60° C. for 8 h to completely dissolve the PVDF powder, thereby obtaining a modified PVDF spinning solution with a concentration of 17 wt %.
[0026] (3) Preparation of alkali-treated modified PVDF nanofibers. The modified PVDF solution was spun using electrospinning technology to obtain modified PVDF nanofibers. The spinning parameters were: spinning voltage 18KV, injection pump speed 1.0mL / h, receiving distance 15cm, and drum speed 60r / min.
[0027] Comparative Example 1
[0028] (1) Alkali treatment of PVDF. Add 5 g of PVDF powder to 50 mL of 1 mol / L NaOH ethanol solution and stir at 60°C for 0.5 h. The amount of TBAB added is 3 mg / mL. Filter and repeatedly rinse the collected PVDF powder with deionized water until it is neutral, and dry it at 105°C for later use.
[0029] (2) Preparation of modified PVDF spinning solution: 1.6 g of modified PVDF powder was added to 10 mL of DMF and stirred under magnetic force at 60° C. for 8 h to completely dissolve the PVDF powder, thereby obtaining a modified PVDF spinning solution with a concentration of 17 wt %.
[0030] (3) Preparation of modified PVDF nanofibers. The modified PVDF solution was spun using electrospinning technology to obtain modified PVDF nanofibers. The spinning parameters were: spinning voltage 18 KV, syringe pump speed 1.0 mL / h, receiving distance 15 cm, and drum speed 60 r / min.
[0031] Comparative Example 2
[0032] (1) Alkali treatment of PVDF. Add 5 g of PVDF powder to 50 mL of 2 mol / L NaOH ethanol solution and stir at 60 °C for 0.5 h. The amount of TBAB added is 3 mg / mL. Filter and repeatedly rinse the collected PVDF powder with deionized water until it is neutral, and dry it at 105 °C for later use.
[0033] (2) Preparation of modified PVDF spinning solution: 1.6 g of modified PVDF powder was added to 10 mL of DMF and stirred under magnetic force at 60° C. for 8 h to completely dissolve the PVDF powder, thereby obtaining a modified PVDF spinning solution with a concentration of 17 wt %.
[0034] (3) Preparation of modified PVDF nanofibers. The modified PVDF solution was spun using electrospinning technology to obtain modified PVDF nanofibers. The spinning parameters were: spinning voltage 18 KV, syringe pump speed 1.0 mL / h, receiving distance 15 cm, and drum speed 60 r / min.
[0035] Comparative Example 3
[0036] (1) Alkali treatment of PVDF. Add 5 g of PVDF powder to 50 mL of 4 mol / L NaOH ethanol solution and stir at 60 °C for 0.5 h. The amount of TBAB added is 3 mg / mL. Filter and repeatedly rinse the collected PVDF powder with deionized water until it is neutral, and dry it at 105 °C for later use.
[0037] (2) Preparation of modified PVDF spinning solution: 1.6 g of modified PVDF powder was added to 10 mL of DMF and stirred under magnetic force at 60° C. for 8 h to completely dissolve the PVDF powder, thereby obtaining a modified PVDF spinning solution with a concentration of 17 wt %.
[0038] (3) Preparation of modified PVDF nanofibers. The modified PVDF solution was spun using electrospinning technology to obtain modified PVDF nanofibers. The spinning parameters were: spinning voltage 18 KV, syringe pump speed 1.0 mL / h, receiving distance 15 cm, and drum speed 60 r / min.
[0039] The modified PVDF nanofiber membrane prepared in the above Example 1 and the comparative examples 1-3 and the glass fiber membrane were tested for porosity, water absorption, contact angle and mechanical properties, and Zn / / Zn and Zn / / MnO2 CR2032 button batteries were assembled respectively. The impedance and cycle performance of the batteries were tested using an electrochemical workstation. The test data are listed in Table 1. The positive and negative electrodes of the Zn / / Zn battery both used zinc discs with a diameter of 15 mm, and the electrolyte was 3 mol / L ZnSO4 aqueous solution. The negative electrode of the Zn / / MnO2 battery was a zinc disc with a diameter of 15 mm, and the positive electrode was MnO2 with a loading of about 2.0 mg / cm 2 , the electrolyte is: an aqueous solution of 2mol / L ZnSO4 and 0.2mol / L MnSO4.
[0040] Table 1 Properties of PVDF nanofiber membranes and glass fiber membranes modified by different alkali treatments and their performance in zinc ion batteries
[0041]
[0042] Table 1 lists the properties of Example 1, Comparative Examples 1-3 and glass fiber diaphragms and their performance data when used as zinc ion battery diaphragms. The contact angle of Example 1 is 55°, which is hydrophilic, and the breaking strength is 8.4MPa, which is better than Comparative Examples 1-3 and glass fiber diaphragms. When used in a Zn / / Zn symmetrical battery, the charge transfer impedance of the battery of Example 1 is 45.51Ω, the conductivity is 0.80mS / cm, and the battery life is 92h, which is significantly greater than the glass fiber diaphragm battery, while the battery life of Comparative Examples 1-3 is less than the glass fiber diaphragm battery. When used in a Zn / / MnO2 battery, the battery of Example 1 has a charge and discharge frequency of more than 1000 times, a charge transfer impedance of 175.4Ω, a conductivity of 2.39mS / cm, and a maximum discharge specific capacity of 128mAh / g, which is significantly better than the glass fiber diaphragm battery.
[0043] The above examples are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above examples. All variations that can be directly derived or associated with the technical content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A modified PVDF nanofiber membrane, characterized in that Porosity 45-55%, water absorption 250-350%, contact angle 55-60°, breaking strength 8-9MPa, elongation 7-8%.
2. The method for preparing the modified PVDF nanofiber membrane according to claim 1, characterized in that: The following steps are involved: (1) Add 5 g of PVDF to 50 mL of 0.3-0.7 mol / L alkali / ethanol solution, add 0.1-0.3 g of tetrabutylammonium bromide (TBAB), stir at 60° C. for 0.5-0.8 h, filter, wash the solid to neutrality, and dry to obtain a modified PVDF solid. (2) Dissolve the modified PVDF solid obtained in step (1) in any one of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone to obtain a spinning solution with a concentration of 17 wt%, and perform electrospinning to obtain a modified PVDF nanofiber membrane.
3. The method for preparing the modified PVDF nanofiber membrane according to claim 2, characterized in that: In the step (1), the base is NaOH or KOH, and the preferred concentration is 0.5 mol / L.
4. The method for preparing the modified PVDF nanofiber membrane according to claim 2, characterized in that: In the step (1), the preferred stirring time is 0.5 h and the amount of TBAB used is 0.15 g.
5. The PVDF nanofiber membrane according to claim 1, characterized in that: The discharge specific capacity of the zinc ion battery is 128 mAh / g at 1.0 A / g, and the number of cycles exceeds 1000 times.
Citation Information
Patent Citations
Non-woven fabric based PVDF (polyvinylidene fluoride) film preparation method
CN106192369A
Preparation method of polyvinylidene fluoride hydrophilic film with acid, alkali and ethanol resistance