Preparation method of TCC-VCSEL containing transverse coupled cavity
By performing As+ ion implantation and photolithography precise control in the first p-DBR layer of VCSEL, combined with high-temperature wet oxidation technology, the problems of traditional VCSEL speed limitation and difficulty in oxide window control are solved, and high-frequency performance and yield are achieved. Improved, suitable for high-speed communications TCC-VCSEL preparation.
Patent Information
- Application Number
- CN202411003159.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The speed of traditional VCSEL is limited by the relaxation oscillation frequency and parasitic capacitance, the modulation bandwidth is difficult to exceed 10Gbps, and the size and uniformity of the oxide window are complex to control, which cannot meet the performance requirements of high-speed communication.
By performing As+ ion implantation in the first p-DBR layer, the oxidation rate is significantly increased, the oxidation process is almost self-terminated, the oxide window size and uniformity are accurately controlled, and the transverse coupling cavity structure is formed in combination with photolithography and high-temperature wet oxidation technology. Improve the photon-photon resonance effect and enhance bandwidth.
It significantly improves the high-frequency performance and controllability of VCSEL, reduces the uniformity error of the oxide window, and thus improves the product yield and high-speed communication application capabilities.
Smart Images

Figure CN118943885A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of semiconductor laser technology, and in particular relates to a method for preparing a TCC-VCSEL containing a transversely coupled cavity. Background Art
[0002] Vertical cavity surface emitting laser (VCSEL) has the advantages of good monochromaticity, small divergence angle, single longitudinal mode lasing, low threshold current, high modulation bandwidth, easy coupling with optical fiber, easy high-density integration, wafer-level detection and low cost. It is widely used in laser printing, optical storage, density optical storage and readout, free space optical interconnection and high-speed data transmission in single-mode optical fiber.
[0003] However, the maximum speed of directly modulated VCSELs is limited by the inherent limit of the relaxation oscillation frequency and its parasitic capacitance. Since the resonant frequency increases with the square root of the drive current, high current density is required to increase the modulation bandwidth, which leads to long-term reliability issues. Therefore, the speed of traditional VCSELs is difficult to exceed 10Gbps.
[0004] The photon-photon resonance (PPR) effect in the small signal modulation response has been used in single-mode edge-emitting semiconductor lasers, such as DBR edge-emitting semiconductor lasers, to significantly increase the 3dB modulation bandwidth beyond the relaxation oscillation frequency. VCSELs using transversely coupled cavities (TCCs) can also increase the bandwidth by 3 times compared to conventional VCSELs by utilizing PPR feedback. For example, the bowtie TCC-VCSEL consists of two square oxide windows connected at one corner to form a "bowtie" shape. One side of the square is the normal VCSEL emission window, and the other side is the transversely coupled cavity, which is connected to the left and right by a narrow channel and insulated from each other by ion implantation. The oxide interface of the feedback cavity acts as a lateral perfect mirror to couple the lateral light back to the VCSEL emission window. To form the transversely coupled cavity structure, a bowtie-shaped mesa process is formed by dry etching, followed by a wet oxidation process. The basic principle of bandwidth enhancement is the same as that of DBR lasers with extended cavities, that is, to provide photon-photon resonance in the small signal modulation response. Due to slow light propagation, a feedback cavity several microns long is sufficient to accommodate photon-photon resonances with a spacing of tens of GHz (see APPLIED PHYSICS LETTERS 103, 0911092013). Because the modulation bandwidth is achieved through the PPR effect, the bandwidth improvement is extremely sensitive to the lateral feedback cavity size. The model shows that changing the width of the bow tie from 0.5μm to 2μm will reduce the lateral coupling strength from 98% to 50% (see SPIE Photonics West 2013, 2013, 8639-31). Therefore, in practical applications, the control requirements for the size and uniformity of the oxide limiter window of TCC-VCSEL are extremely strict.
[0005] The oxide-limited window control of VCSEL is very complex. Strict control of AlAs mole fraction, water (bath) temperature, sample temperature, gas flow rate, etc. is very important for repeatable and uniform oxide-limited VCSEL manufacturing (see J.Phys.D: Appl.Phys.56(2023), 154002). Since the composition of the epitaxial material has certain non-uniformity during the growth process, the wet thermal oxidation rate may be non-uniform. In addition, dry etching will also cause non-uniformity in the shape of the etched mesa. So far, using the most advanced selective wet oxidation equipment and process, the uniformity of the oxide layer window of a 4-inch wafer is + / -0.6um, and the uniformity of the oxide layer window of a 6-inch wafer is + / -0.8um. The narrowest part of the bowtie-type lateral coupling cavity is only 0.5-3um, so the current oxidation process cannot meet the performance and yield requirements of TCC-VCSEL containing lateral coupling cavity.
[0006] In addition, a proton implantation method can be used to form a conductive confinement window for a VCSEL. By damaging the semiconductor material with protons, an insulating layer is formed around the window, thereby limiting the current injection area of the VCSEL device (see ELECTRONICSLETTERS 13th May 1993 Vol. 29 No. 10, pp. 918-919). Since the proton implantation area is determined by the photolithography process, the proton implantation mask in the photolithography process can be easily controlled within an accuracy and uniformity of + / - 0.1um, but this method can only provide conductive confinement. Laterally coupled cavities also require differences in the refractive index of the materials. Usually, the oxide interface of the feedback cavity acts as a lateral perfect mirror to couple lateral light into the VCSEL, providing photon-photon resonance in the small signal modulation reaction, thereby achieving the effect of enhancing the bandwidth. Since proton implantation can only provide current confinement but not optical emission, this method cannot be applied to the preparation of VCSELs containing lateral coupled cavities. Summary of the invention
[0007] The purpose of this application is to propose a method for preparing a high-speed directly modulated TCC-VCSEL containing a lateral coupled cavity. This method can significantly increase the oxidation rate of the oxidation restriction layer grown on the first p-DBR by injecting arsenic ions into it. This difference in oxidation rate can make the oxidation process of the VCSEL restriction window a process that is close to self-termination. +The regional control of ion implantation is mainly determined by the precise photolithography process. This preparation method not only improves the precise control of the oxide window size, but also reduces the uniformity of the oxide restriction window from + / -0.6um to + / -0.15um, thereby improving the optoelectronic performance of the device, such as improving the high-frequency performance of VCSEL and its controllability. At the same time, the yield of the product is significantly improved. Since the critical size of the TCC-VCSEL lateral integrated feedback cavity is only 0.5-3um, and its bandwidth increase performance is determined by the optical coupling strength in the lateral cavity, this method is particularly suitable for the production of TCC-VCSEL for high-speed communication.
[0008] To this end, the present invention provides a method for preparing a TCC-VCSEL containing a lateral coupling cavity, comprising the following steps:
[0009] growing an n buffer layer and an n-DBR layer on an n substrate;
[0010] Growing an active layer including a light-emitting quantum well and a barrier layer embedded in an AlGaAs separation heterostructure layer with a thickness of 1-λ on the n-DBR layer;
[0011] growing a first p-DBR layer on the active layer;
[0012] The first p-DBR layer is oxidized to limit the As outside the window area + Ion implantation;
[0013] In being + Continue to grow an oxidation restriction layer on the ion-implanted first p-DBR layer; continue to grow a second p-DBR layer on the oxidation restriction layer;
[0014] Continue to grow a highly doped p-type contact layer on the second p-DBR layer;
[0015] Performing mesa etching on the p-type contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer, the active layer, the n-DBR layer and the buffer layer;
[0016] performing a high temperature wet oxidation operation on the oxidation restriction layer,
[0017] Here, λ thickness refers to the thickness of the VCSEL emission wavelength.
[0018] Optionally, the n-substrate is an n-type GaAs substrate.
[0019] Optionally, the quantum well and barrier layer of the active layer are made of InGaAs, AlGaAs, GaAs or InGaAsN quantum well materials and corresponding barrier layer materials that are lattice-matched with the GaAs substrate.
[0020] Optionally, the n-DBR, the first p-DBR and the second p-DBR are made of a high-contrast AlGaAs / GaAs DBR pair lattice-matched with a GaAs substrate, such as Al0.92GaAs / Al0.16GaAs DBR material.
[0021] Optionally, the surface layer of the first p-DBR layer is GaAs or AlGaAs layer with high Ga content, and the thickness is N pairs, 1 <N<4。
[0022] Optionally, the first p-DBR layer is oxidized to limit the As outside the window area. + Ion implantation specifically includes:
[0023] Firstly, a photolithography mask is formed on the first p-DBR layer according to an oxidation restriction window pattern;
[0024] Then proceed to As + Ion implantation, As + The ion implantation energy is 100 KeV and the dose is 1x10 15 -2x10 16 cm -3 ;
[0025] After completing As + After ion implantation, the mask material is removed and high temperature annealing is performed.
[0026] The annealing temperature and time are 700°C and 2 hours respectively, and the mask material can be photoresist or other mask materials.
[0027] Optionally, performing mesa etching on the p-contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer and the active layer, the n-DBR layer and the n-buffer layer specifically includes:
[0028] Firstly, a partial photolithography mask is performed on the p-contact layer, and then the p-contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer and the active layer, the n-DBR layer and the n buffer layer are etched;
[0029] After etching is completed, the mask material is removed. The mask material may be photoresist or other mask materials.
[0030] Optionally, performing a high temperature wet oxidation operation on the oxidation restriction layer specifically includes:
[0031] Introduce N2 / H2O mixed gas or other oxidizing mixed gas to carry out controlled oxidation of the oxide layer.
[0032] Among them, the temperature is controlled at 400-425C°.
[0033] Optionally, after the step of performing high temperature wet oxidation on the oxidation restriction layer, the step further includes:
[0034] A p-metal contact electrode for RF signals is arranged on the p-contact layer corresponding to the VCSEL light emitting window, and a p-metal contact electrode for DC signals is arranged corresponding to the lateral coupling cavity.
[0035] Optionally, after a p-metal contact electrode for RF signal is provided on the p-contact layer corresponding to the VCSEL light emitting window, and a p-metal contact electrode for DC signal is provided corresponding to the lateral coupling cavity, the method further comprises:
[0036] After the n-type substrate is thinned, n multi-layer metal layers are deposited and high-temperature alloying is performed.
[0037] Optionally, after thinning the n-type substrate, depositing n multi-layer metal layers and performing high-temperature alloying, the method further comprises:
[0038] In the p-DBR, multi-level energy proton injection is used to electrically isolate the light-emitting window and the lateral feedback cavity of the TCC-VCSEL to ensure that the p-type DBRs on the top of the VCSEL are insulated from each other.
[0039] The proton injection voltage ranges from 60 kV to 350 kV, and the fixed injection dose is 1×10 15 cm 2 .
[0040] The preparation method of the TCC-VCSEL containing a lateral coupling cavity of the present invention, wherein when the top-emitting TCC-VCSEL optoelectronic device is manufactured by the method, firstly, the oxidation restriction window area of the first p-DBR layer is subjected to As + Ion implantation and high temperature annealing are performed, and then the oxide confinement layer and the second p-DBR layer are grown. More generally, this oxide confinement layer must be grown on As + This preparation method can be applied to the manufacture of any oxidation-limited window-type VCSEL chip grown on a GaAs substrate, and is particularly suitable for the manufacture of high-bandwidth TCC-VCSELs that have very strict requirements on the size and uniformity of the lateral coupling cavity.
[0041] The present invention also provides another method for preparing a TCC-VCSEL containing a lateral coupling cavity, comprising the following steps:
[0042] (1) Grow a 500nm silicon-doped GaAs buffer layer on an n-type GaAs substrate and grow 40 pairs of silicon-doped n-type Al 0.92 GaAs / Al 0.16 GaAs DBR;
[0043] (2) Continue to grow Al embedded in 1-λ thickness 0.3 Ga 0.7 As separates three pairs of In heterostructure layers 0.2 GaAs / GaAs quantum well active layer;
[0044] (3) Continue to grow the first carbon-doped p-type Al 0.92 GaAs / Al 0.16 GaAs DBR pair;
[0045] (4) A bowtie-shaped oxidation restriction window is defined by a photolithography process, and the window area is covered with photoresist and As + Perform ion implantation, remove the photoresist after the ion implantation is completed, and perform high temperature annealing;
[0046] (5) Then grow 300A Al 0.92 GaAs and complete the growth of the second carbon-doped p-type Al 0.92 GaAs / Al 0.16 GaAsDBR pair, and highly doped p-contact layer.
[0047] (6) After forming a bow-tie VCSEL mesa by photolithography and dry etching processes, the photoresist or other mask materials are removed, and then the oxide layer is selectively oxidized under wet heat conditions to form a normal square VCSEL light-emitting window and a laterally coupled feedback cavity. The two squares are connected at right angles to form a "bow tie" shape;
[0048] (7) Use BCB or polyimide to protect the sidewalls of the mesa and achieve surface flatness, and then deposit two separate p-metal contact regions, RF and DC, on the p-contact layer;
[0049] (8) After thinning the n-type substrate, depositing n multi-layer metal layers and performing high-temperature alloying.
[0050] (9) Finally, multi-level energy ion implantation is used to electrically isolate the light-emitting cavity and the lateral coupling cavity of the oxide confinement layer, and ensure that the p-type DBRs on the top of the VCSEL are insulated from each other.
[0051] When the TCC-VCSEL chip is manufactured by the present application, an active layer of AlGaAs / GaAs DBR and InGaAs, AlGaAs, GaAs or InGaAsN quantum well materials and corresponding barrier layer materials that are lattice-matched to the n-type GaAs substrate are grown.
[0052] When the TCC-VCSEL chip is manufactured by the present invention, 2-3 pairs of Al are first grown on the active layer. 0.92 GaAs / Al 0.16GaAs first DBR, the surface layer is a DBR layer with high Ga content, and then a photoresist is used to protect the oxidation restriction window area from arsenic ion implantation. + The ion implantation energy is 100 KeV and the dose is 1x10 15 -2x10 16 cm -3 ,After removing the photoresist, the wafer was annealed at 700°C for 2 hours.
[0053] When the TCC-VCSEL chip is manufactured by using the present application, in As + 300A of AlAs or AlGaAs oxide limiting layer material and the remaining second p-DBR are grown on the surface of the ion-implanted p-DBR. The total p-type Al 0.92 GaAs / Al 0.16 The number of GaAsDBR pairs is 26.
[0054] When the TCC-VCSEL chip is manufactured by the present application, the wafer after epitaxy is subjected to photolithography and dry etching to form a bowtie-shaped mesa. Then, under wet and hot conditions, a N2 / H2O mixed gas is introduced to control oxidation of the oxide layer, and the temperature is controlled at 400-425°C. + The oxidation rate of the oxide restriction layer grown on the ion implanted area is about 0.5um / min, while in the absence of As + The oxidation rate of the oxide confinement layer grown on the ion implantation area is about 0.12um / min. After oxidation, the width of the light emission window and the lateral coupling cavity of the TCC-VCSEL is between 3-6um, and they are connected to each other at right angles to form a bow tie shape. The narrowest point where the two blocks are connected is only 0.5-3um.
[0055] When the TCC-VCSEL chip is manufactured by the present application, the light emission window of the oxide confinement layer and the lateral coupling cavity need to be electrically isolated, and the isolation depth needs to penetrate the p-DBR. Proton implantation with a graded 60-350 KeV and a dose of 10 15 cm- 3 The isolation depth is about 4um. The isolation resistance reaches 10MΩ and the leakage current is less than 10uA.
[0056] The characteristic of the present application is that after growing 1-3 pairs of first p-DBR layers, regional As + Ion implantation, the shape of the oxidation window area can be precisely controlled by the photolithography process according to the design requirements. Then continue to complete the conventional oxidation restriction layer, the second p-DBR layer and the p-contact layer epitaxial growth. + The oxidation rate of the oxide confinement layer in the ion implantation area under 400-425°C wet heat conditions is non-As+ 2-4 times of the ion implantation area. By utilizing this oxidation rate difference, the oxidation interface is in a relatively stopped state after reaching the oxidation window, thereby achieving the purpose of accurately controlling the size and uniformity of the oxidation window. Since this oxidation limit window is defined by photolithography and ion implantation, its accuracy can be significantly improved. This method avoids the uncontrollability of the oxidation process caused by the non-uniformity of the epitaxial material of the oxide layer and the non-uniformity of the table etching. Especially for structures with complex cavities such as TCC-VCSEL, these uncontrollable properties will seriously affect the high-frequency performance of the laser chip and cannot meet the design requirements. The method of the present application can significantly reduce the difficulty of TCC-VCSEL preparation, which is conducive to improving the mass production capacity of the product, improving the yield, and expanding the application of VCSEL laser chips in high-speed communication scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] To further illustrate the content of the present application, the present application is further described below in conjunction with the accompanying drawings and specific examples, which will make the technical solution and other beneficial effects of the present application apparent.
[0058] Figure 1A Schematic diagram of a bowtie TCC-VCSEL structure with a transverse coupling cavity in one embodiment of the present application;
[0059] Figure 1B A partial cross-sectional view of a bowtie-type TCC-VCSEL containing a transverse coupling cavity in an embodiment of the present application;
[0060] Figure 2 For an embodiment of this application, As + Process flow chart of TCC-VCSEL with ion implantation of the first p-DBR controlled growth of the oxide confinement layer window;
[0061] Figure 3A As in the epitaxial process of TCC-VCSEL material in one embodiment of the present application + Schematic diagram of the structure before ion implantation into the first p-DBR layer;
[0062] Figure 3B As in the epitaxial process of TCC-VCSEL material in one embodiment of the present application + Schematic diagram of the structure after ion implantation into the first p-DBR layer; Figure 4 In one embodiment of the present application, there is As + and no As + The oxide confinement layer Al grown on the ion-implanted DBR 0.95 Ga 0.05 Comparison of the oxidation rate of As under wet heat conditions;
[0063] Figure 4 In one embodiment of the present application, there is As+ and no As + Ion implantation of Al oxide layer grown on the first p-DBR 0.95 Ga 0.05 Comparison of the oxidation rate of As under wet heat conditions;
[0064] Figure 5 In one embodiment of the present application, As + Ion implantation of Al grown on the first p-DBR 0.95 Ga 0.05 Cross-sectional view of a VCSEL with an As oxide confinement layer window;
[0065] Figure 6 In one embodiment of the present application, As + Schematic diagram of the TCC-VCSEL chip structure with a lateral coupling cavity and an oxidation confinement layer window controlled by ion implantation. DETAILED DESCRIPTION
[0066] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0067] like Figure 1A and Figure 1B As shown, they are a schematic diagram of a bowtie TCC-VCSEL structure containing a lateral coupling cavity and a partial cross-sectional view thereof, wherein the epitaxial layer structure is composed of an n-type GaAs substrate 100, an n-buffer layer 110, an n-DBR layer 120, an active layer 130 including a semiconductor quantum well and a barrier layer, an oxidation restriction layer 140, a p-DBR layer 150 and a p-contact layer 160.
[0068] Reference Figure 1BOn the oxidation restriction layer 140, the unoxidized left block 141 is the normal VCSEL emission window, and the unoxidized right block and the connection area 142 are the lateral feedback cavity, which are connected left and right by a narrow channel of several microns to pass the lateral traveling wave. The oxide interface of the feedback cavity acts as a lateral mirror to couple the lateral light back to the VCSEL light-emitting window. Ion implantation is used to form an insulating band 500 to electrically isolate the light-emitting window and the lateral coupling cavity. The n metal layer 400 is deposited on the bottom of the substrate and the p contact metal layer is the RF metal contact 320 on the emission cavity and the DC metal contact 310 on the coupling cavity. The basic principle of bandwidth enhancement is that the feedback cavity can provide photon-photon resonance in the small signal modulation response. Due to slow light feedback, the feedback cavity of several microns can accommodate a photon-photon spacing of tens of GHz, so the increase in bandwidth is achieved through the PPR effect.
[0069] See also Figure 2 , Figure 3A , Figure 3B , Figure 2 For the use of As + TCC-VCSEL process flow chart of the oxide confinement layer window with ion implantation to control the growth of the first p-DBR. Figure 3A and Figure 3B The regions As used in the TCC-VCSEL epitaxy process are + Schematic diagram of the structure before and after ion implantation into the first p-DBR layer. The present application proposes a method for preparing a TCC-VCSEL with a lateral coupling cavity, and the implementation process includes the following steps:
[0070] (1) In a specific embodiment, Figure 2 (S1) and Figure 3A , Figure 3B As shown, first, a silicon-doped GaAs buffer layer 110 is grown on an n-type GaAs substrate 100 and a silicon-doped n-type Al 0.92 GaAs / Al 0.16 GaAs DBR layer 120 .
[0071] In a specific implementation, the thickness of the silicon-doped GaAs buffer layer 110 is 400-800 nm. 0.92 GaAs / Al 0.16 The number of pairs of the GaAs DBR layer 120 is 38-41 pairs.
[0072] (2) In the specific implementation, refer to Figure 2 (S2) and Figure 3, the present application selects Al embedded in 1-λ thickness 0.3 Ga 0.7 As separates three pairs of In heterostructure layers 0.2Active layer 130 of GaAs / GaAs quantum well and barrier layers,
[0073] Here, λ thickness refers to the thickness of the VCSEL emission wavelength.
[0074] In a specific implementation, the quantum well material of the VCSEL may also be InGaAs, AlGaAs, GaAs, or InGaAsN and corresponding barrier layers that are lattice-matched to GaAs.
[0075] (3) Continue to refer to Figure 2 (S3) and Figure 3A , Figure 3B In the embodiment of the present application, a carbon-doped first p-DBR layer 151 is first grown on the VCSEL active layer 130;
[0076] In a specific implementation, the first p-DBR layer 151 is composed of P-doped Al 0.92 GaAs / Al 0.16 The first p-DBR layer 151 is composed of GaAs or similar high contrast materials. The DBR pairs of the first p-DBR layer 151 need to be greater than 1 pair and less than 4 pairs. Furthermore, the surface layer of the first p-DBR layer 151 is a high-Ga and low-Al material layer.
[0077] (4) In the present application examples, refer to Figure 2 (S4-S5) and Figure 3A , Figure 3B A bowtie-shaped oxidation restriction window photoresist mask 200 is defined on the first p-DBR layer 151 according to the design by using a photolithography process. The design of this window pattern needs to comprehensively consider the emission window of the VCSEL, the lateral feedback cavity length, and the width of the narrowest part in the middle of the connecting square bowtie.
[0078] In the specific implementation, refer to Figure 3A , the window is covered by photoresist 200, and the area outside the window is As + The first p-DBR layer 151 is subjected to As + Ion implantation. + The ion implantation energy is 100 KeV and the dose is 1x10 15 -2x10 16 cm -3 . Reference Figure 3B , in As + After the ion implantation process, the arsenic-rich first p-DBR layer 155 and the bow-tie-shaped first p-DBR layer 151 in the non-implanted region are formed. The advantage of using ion implantation to prepare the arsenic-rich GaAs layer is that the excess arsenic concentration and the related gallium vacancy density can be flexibly controlled by adjusting the implantation dose. This gallium vacancy density determines the increase in the oxidation rate of the oxidation restriction layer.
[0079] In the presence of As + and no As + Ion implantation of Al oxide layer grown on the first p-DBR 0.95 Ga 0.05 Comparison of the oxidation rate of As under wet and hot conditions (see Figure 4 ) is displayed in the + The oxidation rate of the oxide confinement layer grown in the ion implanted area is four times that of the non-implanted area. This increase in the oxidation rate of the AlGaAs layer with a high aluminum content is mainly attributed to the As + The gallium vacancies caused by ion implantation can enhance the ability to remove arsenic-containing byproducts of the oxidation reaction process. This leads to accelerated oxidation of the AlGaAs layer and improved oxide-GaAs interface quality. + The increase in oxidation rate is determined by the defect density under the implantation dose. The saturation dose is set at 10x16cm -2 the following.
[0080] It should be noted that after completing As + After ion implantation, the photoresist is removed with a solvent, and then the epitaxial wafer needs to be annealed at 700°C for 2 hours to form a good epitaxial surface.
[0081] (5) In the present application examples, refer to Figure 2 (S6-S7) and Figure 5 As + Ion implantation of Al grown on the first p-DBR 0.95 Ga 0.05 As VCSEL cross-sectional view of the oxidation confinement layer window, then grow 300A oxidation confinement layer 140 and the remaining carbon-doped second p-DBR layer 152, and the highly doped p-contact layer 160.
[0082] In a specific implementation, the oxidation restriction layer 140 may be made of Al 0.95 Ga 0.05 As, AlAs or similar materials with high aluminum content. The constituent material of the second p-DBR layer 152 is usually the same as the constituent material of the first p-DBR layer 151.
[0083] Furthermore, a highly doped p-contact layer 160 is finally grown epitaxially to reduce the contact resistance between the semiconductor and the metal after the p-metal layer is deposited on this surface;
[0084] (6)Reference Figure 2 (S8-S9), Figure 3A , Figure 3B and Figure 5, using photolithography and dry etching process to form a bowtie VCSEL table, the bowtie table shape is non-As + A magnification of the ion implantation region 151, from the sidewall of the mesa to the As + The distances between the edges of the ion implanted bowtie contours should be as close as possible.
[0085] In a specific implementation, a fluorine-containing corrosive gas is used to transfer the bowtie-shaped photolithography pattern to a SiO2 or SiNx passivation film by inductively coupled plasma etching, and finally the bowtie-shaped mesa structure of the TCC-VCSEL is formed by inductively coupled plasma etching under the passivation mask. The chemical reaction gas can be chlorine-containing gas, nitrogen, argon and helium, as well as a combination of these gases. The etching depth must at least exceed the active layer. Furthermore, the etching depth of the mesa can reach the GaAs substrate to reduce the parasitic effect of the device at high frequencies. The mesa structure formed after etching is as follows: Figure 6 By As + The schematic diagram of the TCC-VCSEL chip structure with a lateral coupling cavity and an oxidation restriction layer window controlled by ion implantation is shown.
[0086] In a specific implementation, after removing the photoresist and passivation mask, the wafer is then heated at 400-425°C by introducing a N2 / H2O mixed gas to the oxidation restriction layer (Al 0.95 Ga 0.05 As)155 is selectively oxidized.
[0087] It should be further pointed out that As + The difference between the oxidation rate of the restriction layer grown on the implanted area and the oxidation rate of the non-implanted area, when the oxidation process enters the design window 151 (non-implanted area), the oxidation rate will be significantly reduced, so that the oxidation process is suppressed. This substantially reduces the problems that may occur during the oxidation process and improves the uniformity of the VCSEL oxidation restriction window. Therefore, by adding the bottom layer AlGaAs:As + The first p-DBR layer can increase the yield of VCSEL and reduce the manufacturing cost.
[0088] Equally important, another advantage of the present application is that the injection area is defined by the photolithography process, and the accuracy of the photolithography is very easy to reach + / -0.05um. In the traditional oxidation process, the initial point of the oxidation process is the side wall of the mesa etching. Since the oxidation restriction layer is at the bottom of the p-DBR layer, the etching depth generally needs to exceed 3um to expose the side wall of the oxidation restriction layer. Therefore, the accuracy of the initial point of the oxidation process in the traditional process is difficult to control to less than + / -0.25um.
[0089] Reference Figure 1A , Figure 1B and Figure 6, the final oxidation window is composed of a normal square VCSEL light emitting window 141 and a laterally coupled feedback cavity 142, where the two squares are connected at right angles to form a "bow tie" shape;
[0090] (7)Reference Figure 2 (S10-S11) and Figure 6 The sidewalls of the mesa are protected with BCB or polyimide and the surface is flattened 600. The BCB or polyimide on the mesa surface is removed by photolithography and reactive ion etching to expose the highly doped p-contact layer 160 on the surface. The etching gas can be fluorine-containing corrosive gas, oxygen and argon, or a combination of these gases, which is not limited here.
[0091] Furthermore, the wafer surface is patterned again and a p-type metal layer is deposited. The wafer after deposition is subjected to metal stripping in a heated solvent to form a p-metal layer separated from the top of the table and RF (320) and DC (310) pads. The p-metal layer is generally composed of Ti / Pt / Au multilayer metal, which is not limited here.
[0092] (8)Reference Figure 2 Process flow chart (S12-S14) and Figure 6 Schematic diagram of the structure, in a possible implementation, after thinning the n-type GaAs substrate, a multi-layer n-metal layer 400 is deposited, and the n-metal layer is generally composed of Au / Ge / Ni / Au multi-layer metal, which is not limited here.
[0093] Furthermore, the wafer after the n-type metal deposition is alloyed at a high temperature of 400-450C° to form an ohmic contact between the substrate and the metal.
[0094] (9)Reference Figure 2 (S15) and Figure 6 , multi-level energy proton implantation is used to electrically isolate the light emitting cavity and the lateral feedback cavity of the VCSEL 500, and ensure that the p-DBR layer 152 on the top of the VCSEL is insulated from left to right.
[0095] In the specific implementation, the following six different proton implantation voltages were used: 60 kV, 120 kV, 180 kV, 240 kV, 300 kV, and 350 kV, and a fixed dose of 1 × 10 1 5cm 2 The light-emitting cavity and the lateral feedback cavity are electrically isolated. The isolation depth needs to penetrate the 4um thick p-DBR. The isolation resistance reaches 10MΩ and the leakage current is less than 10uA. This ensures that the DC current is injected into the feedback cavity, thereby controlling the optical coupling phase and amplitude fed back to the VCSEL (see Figure 1A, Figure 1B Schematic diagram).
[0096] In the specific implementation, the final cleavage is performed by grinding wheel cutting or laser cutting ( Figure 2 , S16), completing the production of the entire TCC-VCSEL chip.
[0097] Figure 6 It is to adopt As + Schematic diagram of the structure of a TCC-VCSEL chip containing a transverse coupling cavity and a window of an oxidation restriction layer controlled by ion implantation. Referring to the above specific manufacturing steps (1)-(9), a complete optoelectronic chip containing a TCC-VCSEL containing a transverse coupling cavity as described in this application is realized.
[0098] TCC-VCSEL with lateral coupling cavity is an important technical approach to improve the high-frequency performance of VCSEL. Accurate control of the emission window, lateral feedback cavity and the connection area between the device is a necessary condition to ensure chip performance, and its critical size is only 0.5-2um. In particular, since the lateral coupling strength is very sensitive to the control of critical size, the characteristic of the method of the present application is that this method significantly reduces the difficulty of controlling the oxidation process of the oxidation restriction window of the TCC-VCSEL with lateral coupling cavity, thereby improving the high-frequency performance of VCSEL, and at the same time significantly reducing the cost of TCC-VCSEL chip devices by improving the yield.
[0099] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0100] The above is a detailed introduction to a method for preparing a VCSEL containing a laterally coupled cavity provided in an embodiment of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solution and its core idea of the present application. A person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features thereof can be replaced by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solution deviate from the scope of the technical solution of the embodiments of the present application.
Claims
1. A method for preparing a TCC-VCSEL containing a lateral coupling cavity, characterized in that: Includes the following steps 2 growing an n buffer layer and an n-DBR layer on an n substrate; Growing an active layer including a light-emitting quantum well and a barrier layer embedded in a 1-Å thick AlGaAs separation heterostructure layer on the n-DBR layer; growing a first p-DBR layer on the active layer; The first p-DBR layer is oxidized to limit the As outside the window area + Ion implantation; In being + Continue to grow an oxidation restriction layer on the ion-implanted first p-DBR layer; continue to grow a second p-DBR layer on the oxidation restriction layer; Continue to grow a highly doped p-type contact layer on the second p-DBR layer; Performing mesa etching on the p-type contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer, the active layer, the n-DBR layer and the buffer layer; performing a high temperature wet oxidation operation on the oxidation restriction layer, Here, λ thickness refers to the thickness of the VCSEL emission wavelength.
2. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The n-substrate is an n-type GaAs substrate.
3. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The quantum well and barrier layer of the active layer adopt InGaAs, AIGaAs, GaAs or InGaAsN quantum well materials and corresponding barrier layer materials that are lattice-matched with the GaAs substrate.
4. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The n-DBR, the first p-DBR and the second p-DBR are made of a high-contrast AlGaAs / GaAs DBR pair that is lattice-matched with a GaAs substrate.
5. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The surface layer of the first p-DBR layer is GaAs or AlGaAs layer with high Ga content, and its thickness is N pairs, 1 <N<4。 6. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The first p-DBR layer is oxidized to limit the As outside the window area + Ion implantation specifically includes: Firstly, a photolithography mask is formed on the first p-DBR layer according to an oxidation restriction window pattern; Then proceed to As + Ion implantation, As + The ion implantation energy is 100 KeV and the dose is 1x10 15 -2x10 16 cm -3 ; After completing As + After ion implantation, the mask material is removed and high temperature annealing is performed. The annealing temperature and time are 700°C and 2 hours respectively.
7. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The mesa etching of the p-contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer and the active layer, the n-DBR layer and the n-buffer layer specifically includes: Firstly, a partial photolithography mask is performed on the p-contact layer, and then the p-contact layer, the second p-DBR layer, the oxidation restriction layer, the first p-DBR layer and the active layer, the n-DBR layer and the n buffer layer are etched; After etching is completed, the mask material is removed.
8. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 1, characterized in that: The high temperature wet oxidation operation of the oxidation restriction layer specifically includes: Introduce N2 / H2Q mixed gas or other oxidizing mixed gas to carry out controlled oxidation of the oxide layer. Among them, the temperature is controlled at 400-425C°.
9. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 8, characterized in that: After the oxidation restriction layer is subjected to a high temperature wet oxidation operation step, the method further comprises: A p-metal contact electrode for RF signals is arranged on the p-contact layer corresponding to the VCSEL light emitting window, and a p-metal contact electrode for DC signals is arranged corresponding to the lateral coupling cavity.
10. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 9, characterized in that: After a p-metal contact electrode for RF signal is arranged on the p-contact layer corresponding to the VCSEL light emitting window, and a p-metal contact electrode for DC signal is arranged corresponding to the lateral coupling cavity, the method further comprises: After the n-type substrate is thinned, n multi-layer metal layers are deposited and high-temperature alloying is performed.
11. The method for preparing a TCC-VCSEL containing a lateral coupling cavity according to claim 10, characterized in that: After thinning the n-type substrate, depositing n multi-layer metal layers and performing high-temperature alloying, the method further comprises: In the p-DBR, multi-level energy proton injection is used to electrically isolate the light-emitting window and the lateral feedback cavity of the TCC-VCSEL to ensure that the p-type DBRs on the top of the VCSEL are insulated from each other. The proton injection voltage ranges from 60 kV to 350 kV, and the fixed injection dose is 1×10 15 cm 2 .
Citation Information
Patent Citations
Current guidance VCSEL and preparation method thereof
CN108539577A
Vertical cavity surface emitting laser with transverse structure and manufacturing method thereof
CN117791305A
Optical devices with transverse-coupled-cavity
US10658815B1
Photonic crystal single transverse mode defect structure for vertical cavity surface emitting laser
US20040091010A1
Surface emitting laser
US20220085573A1
Cited By
Vertical cavity surface emitting laser and preparation method thereof
CN121097503A
Vertical cavity surface emitting laser and method for manufacturing the same
CN121097503B
Vertical cavity surface emitting laser and preparation method thereof
CN121216222A