Co / Co7Fe3-atC nanofiber composite material as well as preparation method and application thereof
By combining Co/Co7Fe3@C nanofiber composite with carbon fiber, the problems of agglomeration and uneven distribution of MOF derivatives are solved, and efficient electromagnetic wave absorption performance is achieved, especially in electromagnetic wave absorption, which shows a high reflection loss value. and wide bandwidth.
Patent Information
- Application Number
- CN202410999849.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The existing metal organic frame (MOF) derivatives have problems with nanoparticle agglomeration and uneven distribution in electromagnetic wave absorption, resulting in high fill volume and narrow band gaps, limiting their microwave absorption performance.
By preparing Co/Co7Fe3@C nanofiber composite materials, the MOF derivatives are compounded with carbon fibers by electrospinning and impregnation technology to generate Co elemental and Co7Fe3 alloy nanoparticles coated on the surface of the carbon fiber, forming a rich heterogeneous interface to enhance the media Electric loss capability.
The electromagnetic wave absorption performance with high reflection loss value, wide bandwidth and low fill amount is achieved, the preparation process is simplified, the material's conductivity and dielectric loss ability are improved, and it is suitable for electromagnetic wave absorption applications.
Smart Images

Figure HDA0004961257570000011 
Figure HDA0004961257570000012 
Figure HDA0004961257570000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electromagnetic wave absorption, and specifically relates to a Co / Co 7 Fe 3 @CNanofiber composite materials and their preparation methods and applications. Background Art
[0002] With the vigorous development of science and technology, especially the progress of 5G mobile technology, people's communication and exchanges have been promoted, and people's sense of happiness has been greatly improved. This has brought great convenience to people's lives, but it has also caused a series of electromagnetic wave pollution problems, affecting human health. Therefore, electromagnetic wave pollution has become a major environmental problem that needs to be solved urgently, and the design and development of electromagnetic wave absorbing materials is expected to become the key to effectively solving the problem of electromagnetic wave pollution.
[0003] Magnetic carbon derivatives prepared with metal organic framework (MOFs) materials as precursors show the advantages of high porosity, large specific surface area, and synergistic effects of multiple loss mechanisms. By optimizing the components and regulating the structure of the derivatives, it is expected to achieve the coordinated development of "thin, light, wide, and strong" absorbing materials, thereby optimizing the electromagnetic wave absorption performance. However, single MOF derivatives usually exist in the form of powders, which not only inevitably have the problems of nanoparticle agglomeration and uneven distribution, but also their high filling content and narrow band gap as absorbing materials also create obstacles to microwave absorption. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a Co / Co 7 Fe 3 @C nanofiber composite materials and their preparation methods and applications overcome the problems of particle agglomeration and uneven distribution of MOF derivatives. The prepared Co / Co 7 Fe 3 @CNFs composite materials have the advantages of higher reflection loss value, wider bandwidth and lower filling content.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention provides a Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0007] (1) Put Co(NO 3 ) 2 6H 2 O, polyacrylonitrile and polyvinyl pyrrolidone are dissolved in N,N-dimethylformamide to obtain solution A;
[0008] (2) electrospinning solution A to obtain polymer fibers containing metal ions;
[0009] (3) dissolving 2-methylimidazole in methanol to obtain solution B, and immersing the polymer fiber containing metal ions obtained in step (2) in solution B to obtain PAN / PVP@ZIF67 fiber;
[0010] (4) K 3 [Fe(CN) 6 ] is dissolved in a mixed solution of ethanol and water to obtain solution C, and then the PAN / PVP@ZIF67 fiber obtained in step (3) is immersed in solution C to obtain PAN@ZIF67 / CoFe-PBA fiber;
[0011] (5) Pre-oxidizing and carbonizing the PAN@ZIF67 / CoFe-PBA fibers obtained in step (4) to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0012] Preferably, in step (2), the positive voltage used for electrospinning is 12 to 18 kV, and the receiving distance between the tip of the syringe needle and the receiver is 12 to 20 cm.
[0013] Preferably, in step (3), the immersion is carried out at room temperature for 12 to 24 hours.
[0014] Preferably, in step (4), the immersion is carried out at room temperature, wherein K in solution C 3 [Fe(CN) 6 ] The concentration is (0.625~2.5) mg / mL.
[0015] Preferably, in step (5), the pre-oxidation temperature is 200 to 280° C. and the time is 1 to 3 hours.
[0016] Preferably, in step (5), the carbonization temperature is 600-800° C. and the time is 1-4 hours.
[0017] The present invention provides Co / Co obtained by the preparation method 7 Fe 3 @CNanofiber composite materials.
[0018] Preferably, the Co / Co 7 Fe 3 @C nanofiber composite material includes carbon nanofiber and Co element and Co coated on the surface of carbon nanofiber. 7 Fe 3 Alloy nanoparticles.
[0019] The present invention also provides the Co / Co 7 Fe 3 @CApplication of nanofiber composites in electromagnetic wave absorption.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention prepares PAN@ZIF67 / CoFe-PBA fibers by a simple method, and carbonizes them in an inert atmosphere to obtain Co / Co with rich heterogeneous interfaces. 7 Fe 3 @CNFs composites, Co single substance and Co 7 Fe 3 Alloy nanoparticles are coated on the surface of carbon fiber. 7 Fe 3 Rich heterogeneous interfaces are generated between the alloy, C matrix and paraffin (when testing the microwave absorption performance of the sample, the sample and paraffin need to be heated together and then pressed into a coaxial ring), which enhances the interface polarization ability. 7 Fe 3 The formation of the alloy greatly improves its dielectric loss capacity. The present invention overcomes the problems of particle agglomeration and uneven distribution of MOF derivatives by compounding the MOF derivatives with one-dimensional carbon fibers.
[0022] The Co / Co prepared by the present invention 7 Fe 3 @CNFs composite materials have the advantages of higher reflection loss value, wider bandwidth and lower filling amount. In addition, the dual MOF precursor can be successfully prepared at room temperature, the preparation method is simple, the equipment is easy to operate, and the fiber yield is high. It is a potential wave absorbing material. The electromagnetic wave absorption performance of the sample was tested by vector network analyzer. The results show that the optimal filling ratio of the material is 15wt%, which obtains a minimum reflection loss value of -45.6dB and a maximum effective absorption bandwidth of 6.2GHz. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1The SEM images of the materials prepared in the present invention; (a) is the SEM image of the PAN@ZIF67 / CoFe-PBA-25 fiber prepared in Example 2; (b) is the SEM image of the PAN@ZIF67 / CoFe-PBA-50 fiber prepared in Example 5; (c) is the SEM image of the PAN@ZIF67 / CoFe-PBA-100 fiber prepared in Example 8;
[0025] Figure 2 The Co / Co prepared in Example 8 of the present invention 7 Fe 3 (a) SEM image and (b) TEM image of @CNFs composites;
[0026] Figure 3 The Co / Co prepared in Example 8 of the present invention 7 Fe 3 XRD patterns of @CNFs composites;
[0027] Figure 4 The reflection loss value of the Co@CNFs composite material prepared in Comparative Example 1 of the present invention when the filling amount is 15wt%;
[0028] Figure 5 The reflection loss value of the Co / C@CNFs composite material prepared in Comparative Example 2 of the present invention when the filling amount is 15wt%;
[0029] Figure 6 The Co / Co prepared in Example 8 of the present invention 7 Fe 3 @Reflection loss value of CNFs composite material when the filling amount is 15wt%;
[0030] Figure 7 The Co / Co prepared in Example 8 of the present invention 7 Fe 3 (a) Cole-Cole plots and (b) C 0 picture. DETAILED DESCRIPTION
[0031] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0032] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0033] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0034] The Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0035] (1) Put Co(NO 3 ) 2 6H 2 O, polyacrylonitrile powder and polyvinyl pyrrolidone are dissolved in N,N-dimethylformamide to obtain a mixed solution A;
[0036] (2) transferring the solution A obtained in step (1) into a syringe, and loading it into an electrospinning instrument for electrospinning to obtain polymer fibers containing metal ions;
[0037] (3) dissolving 2-methylimidazole in methanol to obtain a mixed solution B, and immersing the polymer fiber obtained in step (2) into the solution B to obtain PAN / PVP@ZIF67 fiber;
[0038] (4) K 3 [Fe(CN) 6 ] is dissolved in a mixed solution of ethanol and water to obtain solution C, and then the PAN / PVP@ZIF67 fiber obtained in step (3) is immersed in solution C, and the product is washed and dried to obtain PAN@ZIF67 / CoFe-PBA fiber;
[0039] (5) After pre-oxidation, the PAN@ZIF67 / CoFe-PBA fiber obtained in step (4) is placed in a tubular furnace filled with an inert atmosphere and heated to 600-800°C for carbonization to obtain Co / Co 7 Fe 3 @C nanofiber composites (Co / Co 7 Fe 3 @CNFs).
[0040] In step (2) of the present invention, the positive voltage is 12 to 18 kV, and the receiving distance between the tip of the syringe needle and the receiver is 12 to 20 cm.
[0041] In step (3) of the present invention, the immersion is carried out at room temperature for a time of 12 to 24 hours.
[0042] In step (4) of the present invention, the immersion is carried out at room temperature; wherein K in solution C 3 [Fe(CN) 6 ] The concentration is (0.625~2.5) mg / mL.
[0043] In step (5) of the present invention, the pre-oxidation temperature is 200 to 280° C. and the time is 1 to 3 hours.
[0044] In step (5) of the present invention, the inert atmosphere is argon, the heating rate is 2 to 5° C. / min, and the carbonization time is 1 to 4 hours.
[0045] The Co / Co obtained by the preparation method of the present invention 7 Fe 3 @C nanofiber composite material, including carbon nanofiber and Co single substance and Co coated on the surface of carbon nanofiber 7 Fe 3 Alloy nanoparticles, Co and Co 7 Fe 3 The presence of the alloy not only enriches the heterogeneous interface, leading to enhanced interface polarization, but also 7 Fe 3 The alloy significantly improves the electrical conductivity of the composite material, thereby further enhancing the dielectric loss capacity of the material. 7 Fe 3 @CNanofiber composites can be used for electromagnetic wave absorption.
[0046] Embodiment 1:
[0047] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0048] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0049] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 12 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +10 kV and -1 kV, respectively;
[0050] (3) 0.1 g of the obtained Co@PAN / PVP polymer fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 12 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0051] (4) Add 25 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0052] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 200 °C for 1 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 600 °C at a heating rate of 2 °C / min, then kept at this temperature for 1 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0053] Embodiment 2:
[0054] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0055] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0056] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 20 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +18 kV and -1 kV, respectively;
[0057] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 18 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0058] (4) Add 25 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0059] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 250 °C for 2 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 700 °C at a heating rate of 3 °C / min, then kept at this temperature for 2 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0060] Embodiment 3:
[0061] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0062] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0063] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 16 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +14 kV and -1 kV, respectively;
[0064] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 24 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0065] (4) Add 25 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0066] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 280 °C for 3 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 800 °C at a heating rate of 5 °C / min, then kept at this temperature for 4 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0067] Embodiment 4:
[0068] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0069] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0070] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 12 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +10 kV and -1 kV, respectively;
[0071] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 12 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0072] (4) Add 50 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0073] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 200 °C for 1 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 600 °C at a heating rate of 2 °C / min, then kept at this temperature for 1 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0074] Embodiment 5:
[0075] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0076] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0077] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 20 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +18 kV and -1 kV, respectively;
[0078] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 18 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0079] (4) Add 50 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0080] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 250 °C for 2 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 700 °C at a heating rate of 3 °C / min, then kept at this temperature for 2 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0081] Embodiment 6:
[0082] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0083] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0084] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 16 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +14 kV and -1 kV, respectively;
[0085] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 24 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0086] (4) Add 50 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0087] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 280 °C for 3 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 800 °C at a heating rate of 5 °C / min, then kept at this temperature for 4 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0088] Embodiment 7:
[0089] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0090] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0091] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 12 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +10 kV and -1 kV, respectively;
[0092] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 12 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0093] (4) 100 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0094] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 200 °C for 1 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 600 °C at a heating rate of 2 °C / min, then kept at this temperature for 1 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0095] Embodiment 8:
[0096] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0097] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in 10 mL of DMF solution and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0098] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 20 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +18 kV and -1 kV, respectively;
[0099] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 18 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0100] (4) 100 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0101] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 250 °C for 2 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 700 °C at a heating rate of 3 °C / min, then kept at this temperature for 2 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0102] Embodiment 9:
[0103] A Co / Co 7 Fe 3 @C A method for preparing a nanofiber composite material comprises the following steps:
[0104] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0105] (2) Solution A was transferred into a 10 mL syringe and loaded into an electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The electrospinning setting parameters were as follows: the distance between the receiver and the needle tip was set to 16 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +14 kV and -1 kV, respectively;
[0106] (3) 0.1 g of the obtained Co@PAN / PVP fiber was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and placed at room temperature for 24 h. Finally, the obtained PAN / PVP@ZIF67 fiber was washed several times with ethanol;
[0107] (4) 100 mg of K 3 [Fe(CN) 6 ] was dissolved in a mixed solution of 40 mL of ethanol and water (ethanol: water = 1:1) to obtain solution C, and then the PAN / PVP@ZIF67 fiber was immersed in solution C at room temperature, and the product was washed and dried to obtain dual MOF@polymer fiber (PAN@ZIF67 / CoFe-PBA);
[0108] (5) The obtained PAN@ZIF67 / CoFe-PBA fibers were first kept at 280 °C for 3 h, then transferred to a tubular furnace filled with argon atmosphere and heated to 800 °C at a heating rate of 5 °C / min, then kept at this temperature for 4 h, and cooled to room temperature to obtain Co / Co 7 Fe 3 @CNanofiber composite materials.
[0109] Comparative Example 1:
[0110] A method for preparing a Co@CNFs composite material comprises the following steps:
[0111] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0112] (2) Solution A was transferred into a 10 mL syringe, and it was placed on the electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The setting parameters for electrospinning were as follows: the distance between the receiver and the needle tip was set to 20 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +18 KV and -1 KV, respectively;
[0113] (3) The obtained Co@PAN / PVP fibers were first kept at 250 °C for 2 h, then transferred to a tubular furnace filled with argon atmosphere, heated to 700 °C at a heating rate of 3 °C / min, and then kept at this temperature for 2 h. After cooling to room temperature, the Co@CNFs nanofiber composite material was obtained.
[0114] Comparative Example 2:
[0115] A method for preparing a Co / C@CNFs composite material comprises the following steps:
[0116] (1) Weigh 1g of Co(NO 3 ) 2 6H 2 O, 1 g of polyacrylonitrile powder and 0.25 g of polyvinyl pyrrolidone were dispersed in a solution of 10 mL of N,N-dimethylformamide and stirred for 12 h to ensure that the components in the solution were fully mixed. The resulting solution was recorded as A;
[0117] (2) Solution A was transferred into a 10 mL syringe, and it was placed on the electrospinning instrument and connected to a power source for spinning to obtain polymer fibers containing metal ions (Co@PAN / PVP). The setting parameters for electrospinning were as follows: the distance between the receiver and the needle tip was set to 20 cm, the feed rate was set to 0.6 mL / h, and the positive and negative voltages were set to +18 KV and -1 KV, respectively;
[0118] (3) 0.1 g of the obtained Co@PAN / PVP membrane was immersed in 15 mL of methanol solution containing 0.15 g of 2-methylimidazole (2-MI) and left at room temperature for 18 h. Finally, the obtained PAN / PVP@ZIF67 fiber membrane was washed several times with ethanol;
[0119] (4) The obtained PAN / PVP@ZIF67 fibers were first kept at 250 °C for 2 h, then transferred to a tubular furnace filled with argon atmosphere, heated to 700 °C at a heating rate of 3 °C / min, and then kept at this temperature for 2 h. After cooling to room temperature, the Co / C@CNFs nanofiber composite material was obtained.
[0120] Figure 1 The SEM images of (a) PAN@ZIF67 / CoFe-PBA-25, (b) PAN@ZIF67 / CoFe-PBA-50, and (c) PAN@ZIF67 / CoFe-PBA-100 are shown. It can be observed from the figure that the ZIF67@CoFe-PBA polyhedrons are successfully wrapped on the surface of PAN fibers. PAN@ZIF67 / CoFe-PBA nanofibers are prepared by introducing K 3[Fe(CN) 6 ] was synthesized by ion exchange reaction. The formation mechanism is as follows: PAN / PVP@ZIF67 slowly releases Co in a mixed solution of deionized water and ethanol. 2+ ,Co 2+ With K 3 [Fe(CN) 6 ] Rapid reaction generates CoFe-PBA nanoparticles and deposits on the surface of ZIF67 polyhedron. When the reaction is incomplete, a ZIF67 / CoFe-PBA mixed precursor is obtained.
[0121] Figure 2 The Co / Co prepared in the best embodiment (Example 8) is shown. 7 Fe 3 (a) SEM image and (b) TEM image of @C nanofiber composite material. After high temperature carbonization process, Co / Co 7 Fe 3 @CAlthough the surface of the nanofiber composite material showed shrinkage, it can be clearly observed that the ZIF67 / CoFe-PBA derivative is still evenly wrapped on the fiber surface.
[0122] Figure 3 The Co / Co prepared in the best embodiment (Example 8) 7 Fe 3 The XRD pattern of @C nanofibers shows that Co and Co 7 Fe 3 Alloy nanoparticles. Co and Co 7 Fe 3 The presence of the alloy not only enriches the heterogeneous interface, leading to enhanced interface polarization, but also 7 Fe 3 The alloy significantly improves the electrical conductivity of the composite material, thereby further enhancing the dielectric loss capability of the material.
[0123] Figure 4 The RL value of Co@CNFs prepared in Comparative Example 1 when the filling amount is 15wt% is shown. As can be seen from the figure, the RL values of Co@CNFs are all greater than -10dB, indicating that they do not have effective electromagnetic wave attenuation capability.
[0124] Figure 5 The RL value of Co / C@CNFs prepared in Comparative Example 2 when the filling amount is 15wt% is shown. Co / C@CNFs obtains the best RL value of -13.4dB and the maximum effective absorption bandwidth of 3.0GHz.
[0125] Figure 6 The Co / Co prepared in the best embodiment (Example 8) is shown.7 Fe 3 @C nanofiber RL value when the filling amount is 15wt%. When the matching thickness is 3.0mm, the best RL value of -45.6dB is obtained. When the matching thickness is reduced to 1.9mm, the Co / Co 7 Fe 3 @C The maximum effective absorption bandwidth of nanofibers reaches 6.2 GHz, which is significantly better than that of comparative example 2.
[0126] Figure 7 The Co / Co prepared in the best embodiment (Example 8) 7 Fe 3 (a) Cole-Cole plot of @C nanofibers and (b) C 0 Curve. From the Cole-Cole curve, we can see that Co / Co 7 Fe 3 @C The nanofiber has multiple semicircles, indicating that multiple polarization relaxation processes have occurred, and the straight line feature at the tail of the curve represents the good electrical conductivity of the composite material. Both are conducive to the improvement of dielectric loss capacity. 0 The curve can be used to analyze the main cause of magnetic loss. In the range of 2-12GHz, C 0 The significant change in the value is attributed to the effects of natural resonance and exchange resonance. In the 12-18 GHz range, C 0 The value has no significant change, which indicates that eddy current loss becomes dominant at this time.
[0127] The contents of the present invention can be further clearly understood through the above-given embodiments, but they are not intended to limit the present invention.
Claims
1. A method for preparing a Co / Co7Fe3@C nanofiber composite material, characterized in that: The following steps are involved: (1) dissolving Co(NO3)2·6H2O, polyacrylonitrile and polyvinylpyrrolidone in N,N-dimethylformamide to obtain solution A; (2) electrospinning solution A to obtain polymer fibers containing metal ions; (3) dissolving 2-methylimidazole in methanol to obtain solution B, and immersing the polymer fiber containing metal ions obtained in step (2) in solution B to obtain PAN / PVP@ZIF67 fiber; (4) dissolving K3[Fe(CN)6] in a mixed solution of ethanol and water to obtain solution C, and then immersing the PAN / PVP@ZIF67 fiber obtained in step (3) in solution C to obtain PAN@ZIF67 / CoFe-PBA fiber; (5) Pre-oxidizing and carbonizing the PAN@ZIF67 / CoFe-PBA fibers obtained in step (4) to obtain a Co / Co7Fe3@C nanofiber composite material.
2. The method for preparing the Co / Co7Fe3@C nanofiber composite material according to claim 1, characterized in that: In step (2), the positive voltage used for electrospinning is 12 to 18 kV, and the receiving distance between the tip of the syringe needle and the receiver is 12 to 20 cm.
3. The method for preparing the Co / Co7Fe3@C nanofiber composite material according to claim 1, characterized in that: In step (3), the immersion is carried out at room temperature for 12 to 24 hours.
4. The method for preparing the Co / Co7Fe3@C nanofiber composite material according to claim 1, characterized in that: In step (4), the immersion is carried out at room temperature, wherein the concentration of K3[Fe(CN)6] in solution C is (0.625-2.5) mg / mL.
5. The method for preparing the Co / Co7Fe3@C nanofiber composite material according to claim 1, characterized in that: In step (5), the pre-oxidation temperature is 200 to 280° C. and the time is 1 to 3 hours.
6. The method for preparing the Co / Co7Fe3@C nanofiber composite material according to claim 1, characterized in that: In step (5), the carbonization temperature is 600-800° C. and the time is 1-4 hours.
7. The Co / Co7Fe3@C nanofiber composite material obtained by the preparation method according to any one of claims 1 to 6.
8. The Co / Co7Fe3@C nanofiber composite material according to claim 7, characterized in that: The Co / Co7Fe3@C nanofiber composite material comprises carbon nanofibers and Co single substance and Co7Fe3 alloy nanoparticles coated on the surface of the carbon nanofibers.
9. Use of the Co / Co7Fe3@C nanofiber composite material according to claim 7 in electromagnetic wave absorption.