Organic heterojunction transistor photoelectric detector and preparation method thereof

By employing non-fullerene acceptor molecules as the photosensitive layer and layer heterostructure in the photodetector, the problems of high dark current and low photosensitivity are solved, realizing a high-performance photodetector suitable for flexible and portable devices.

CN118946164APending Publication Date: 2024-11-12HANHUIXINCHEN INFRARED TECHNOLOGY (HANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310518839.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing photodetectors suffer from problems such as high dark current, low photosensitivity, and insufficient channel carrier mobility. In particular, the complexity of inorganic semiconductor material growth and processing limits their application in flexible and portable devices.

Method used

An organic heterojunction transistor photodetector with a bottom-up structure includes a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer, and a charge injection layer. The non-fullerene acceptor molecule is used as the photosensitive layer to form a layered heterostructure to suppress dark current. The materials of each layer are prepared by solution method and vacuum evaporation method.

Benefits of technology

It achieves extremely low dark current and high photoresponse source leakage current, significantly improving the photodetector's photodetector sensitivity and detectivity. It is suitable for ultraviolet, visible, and near-infrared photoelectric detection and has mechanical flexibility, making it suitable for wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946164A_ABST
    Figure CN118946164A_ABST
Patent Text Reader

Abstract

The invention discloses an organic heterojunction transistor photoelectric detector and a preparation method thereof. The organic heterojunction transistor photoelectric detector sequentially comprises a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer and a charge injection layer from bottom to top, and a source electrode and a drain electrode are further arranged in a partial region on the charge injection layer. According to the invention, the non-fullerene acceptor molecules are selected as the photosensitive layer, so that the extremely low dark current is realized, meanwhile, a layer heterostructure is formed between the non-fullerene acceptor molecules and the conductive channel layer, the off-state dark current is effectively inhibited, and the extremely low dark current and high light response source-drain current of the device are further realized; therefore, the comprehensive performances such as the light detection sensitivity and the detection rate of the light detector are obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor photoelectric devices, and in particular to an organic heterojunction transistor photoelectric detector and a preparation method thereof. Background Art

[0002] Photodetectors are an important type of photoelectric conversion device. Such devices are widely used in image sensing, environmental monitoring, health monitoring, optical communications, military aerospace, and industrial and agricultural product testing. At present, most commercial photodetectors are based on inorganic semiconductors such as Si, Ga, a-Se, and InGaAs. Although traditional inorganic materials have advantages such as high stability, the growth of detector crystal materials has strict requirements on the lattice matching of substrate materials, and their growth environment is difficult to control and consumes high energy, resulting in high costs. In addition, due to the wide absorption band of inorganic semiconductors, it is difficult for inorganic photodetectors to achieve spectrally selective detection without filters for selection. In addition, the use of traditional inorganic semiconductors to prepare focused image arrays has certain limitations, and the connection between the detector and the readout circuit needs to be achieved through complex processes. For example, short-wave infrared detection materials (such as InGaAs, etc.) are grown on traditional CMOS silicon-based readout circuit substrates. This method is not only complex in process and poor in reliability, but also the mechanical rigidity of inorganic semiconductors limits its application in flexible and portable devices.

[0003] Since 1977, when AJ Heeger, AG Macdiarmid and H. Shirakawa synthesized the conductive polymer polyacetylene and proved its conductivity, organic semiconductors with advantages such as solubility, large-area preparation, low-temperature (room temperature) process, mechanical flexibility, biocompatibility, high sensitivity, light weight and low cost have gradually become the rising star in the field of light detection. Organic semiconductors are usually relatively soft, have high compression coefficients, and are easily soluble in organic solvents, which makes them widely used in fields such as solar cells and photodetectors. How to effectively optimize the device process and prepare high-performance optoelectronic devices is an important direction in the field of organic electronics. In the preparation process of organic optoelectronic devices, small molecule organic semiconductors are usually prepared by vacuum deposition, while polymer semiconductors can be formed into films by solution processing methods such as spin coating, printing, spraying, and scraping. For organic photodetectors, based on the advantages of adjustable detection wavelength of organic molecules, low device manufacturing cost and outstanding equipment compatibility, organic photodetectors for ultraviolet (UV), visible light (Vis) and near-infrared (NIR) can achieve short-wave detection by optimizing the optical band gap of organic semiconductors and the device structure of organic semiconductors, thereby avoiding the filter modules commonly used in inorganic photodetectors, simplifying the manufacturing process of spectrally selective photodetectors, and thus reducing manufacturing costs. At the same time, due to the mechanical flexibility of organic semiconductors, it is conducive to the realization of wearable applications of photodetectors in the future, thereby broadening the application potential in health detection sensors.

[0004] Organic phototransistors (OPTs) are three-terminal devices that offer high sensitivity, adjustable gain, EQE exceeding 100%, and the possibility of monolithic integration with external circuits, making them potentially attractive for light detection applications at various wavelengths. In OPTs, an active channel that is sensitive to an applied light source is formed between two laterally placed electrodes (source and drain). A third gate electrode is located near the active channel, and the channel current can be regulated by adjusting the gate voltage or the intensity of the applied light. Because OPTs have advantages such as high EQE and low-noise photoconductive mode, OPTs light detection has attracted increasing attention in recent years. By optimizing the materials and structures of OPTs devices, further reducing the dark current of OPTs devices, improving the OPTs photosensitivity, improving the photon-to-charge conversion process, and enhancing the channel carrier mobility have become the direction of people's efforts in recent years.

[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an organic heterojunction transistor photodetector and a method for preparing the same, aiming to solve the problem of how to reduce the dark current of OPTs devices, improve the OPTs photosensitivity, improve the photon-to-charge conversion process and enhance the channel carrier mobility.

[0007] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0008] An organic heterojunction transistor photodetector includes, from bottom to top, a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer, and a charge injection layer, wherein a partial area on the charge injection layer is also provided with a source electrode and a drain electrode.

[0009] In the organic heterojunction transistor photodetector, the substrate is made of a rigid material or a flexible material, the rigid material is selected from one of quartz, glass, and silicon wafer, and the flexible material is plastic.

[0010] The organic heterojunction transistor photodetector, wherein the material of the dielectric layer is selected from SiO2, AlO x , hafnium oxide, ZrO x , polyvinyl alcohol, and CYTOP.

[0011] In the organic heterojunction transistor photodetector, the material of the non-fullerene photosensitive layer is selected from one or more of ITIC, IT-4F, Y6, and IEICO-4F.

[0012] In the organic heterojunction transistor photodetector, the material of the conductive channel layer is selected from one or more of C8-BTBT and its derivatives, pentacene and its derivatives, and conjugated polymer semiconductors.

[0013] The organic heterojunction transistor photodetector, wherein the material of the charge injection layer is selected from MoO3, V2O5, NiO x , WO x , CuO x One or more of the .

[0014] The organic heterojunction transistor photodetector, wherein the source electrode, the drain electrode and the gate electrode are respectively selected from one or more of Au, Ag, Cu, Ni, In, Mo, Cr, Al, ITO, PSS:PEDOT, graphene, and carbon nanotubes.

[0015] The organic heterojunction transistor photodetector, wherein the sum of the thickness of the gate and the dielectric layer is 300 nm, the thickness of the photosensitive layer is 30-100 nm, the thickness of the conductive channel layer is 20-200 nm, and the thickness of the source electrode and the drain electrode are both 30-100 nm.

[0016] A method for preparing an organic heterojunction transistor photodetector as described in the above embodiment of the present invention, comprising the steps of:

[0017] providing a substrate;

[0018] Sequentially preparing a gate electrode and a dielectric layer on the surface of the substrate;

[0019] On the dielectric layer, a non-fullerene photosensitive layer is prepared by a solution method, and the non-fullerene photosensitive layer is subjected to a thermal annealing treatment;

[0020] preparing a conductive channel layer on the non-fullerene photosensitive layer by vacuum evaporation;

[0021] A charge injection layer, a source electrode and a drain electrode are sequentially vacuum-deposited on the conductive channel layer through a mask.

[0022] The preparation method, wherein the temperature of the thermal annealing treatment is 0-90°C, and the time of the thermal annealing treatment is 25-35 minutes; in the step of preparing the conductive channel layer by vacuum evaporation, the substrate heating temperature is 0-60°C.

[0023] Beneficial effects: The present invention discloses an organic heterojunction transistor photodetector and a preparation method thereof. By selecting non-fullerene acceptor molecules as the photosensitive layer, extremely low dark current is achieved. At the same time, a layer heterostructure is formed between the non-fullerene acceptor molecules and the conductive channel layer, which effectively suppresses the off-state dark current, further achieving extremely low dark current and high light response source-drain current of the device, thereby significantly improving the comprehensive performance of the photodetector, such as light detection sensitivity and detection rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic structural diagram of an organic heterojunction transistor photodetector of the present invention.

[0025] Figure 2 Graph showing the transmission characteristics of the device obtained in Example 1 under dark and light conditions.

[0026] Figure 3 This is a graph showing the relationship between the responsiveness and light intensity of the device obtained in Example 1.

[0027] Figure 4 This is a test chart of the detection rate of the device obtained in Example 1.

[0028] Figure 5 This is a transmission characteristic diagram of the device obtained in Example 2 under dark and light conditions.

[0029] Figure 6 This is a transmission characteristic diagram of the device obtained in Example 3 under dark and light conditions.

[0030] Figure 7 This is a transmission characteristic diagram of the device obtained in Example 13 under dark and light conditions.

[0031] Figure 8 This is a transmission characteristic diagram of the device obtained in Example 14 under dark and light conditions.

[0032] Fig. 9 This is a transmission characteristic diagram of the device obtained in Example 20 under dark and light conditions.

[0033] Fig.10 This is a test graph of the device's responsiveness, light intensity and relative detectivity of the device obtained in Example 20.

[0034] Fig.11 This is a transmission characteristic diagram of the device obtained in Comparative Example 1 under dark and light conditions.

[0035] Fig.12 This is a transmission characteristic diagram of the device obtained in Comparative Example 4 under dark and light conditions. DETAILED DESCRIPTION

[0036] The present invention provides an organic heterojunction transistor photodetector and a method for preparing the same. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0037] Organic phototransistors (OPTs) are three-terminal devices that offer high sensitivity, adjustable gain, EQE exceeding 100%, and the possibility of monolithic integration with external circuits, making them potentially attractive for light detection applications at various wavelengths. In OPTs, an active channel that is sensitive to an applied light source is formed between two laterally placed electrodes (source and drain). A third gate electrode is located near the active channel, and the channel current can be regulated by adjusting the gate voltage or the intensity of the applied light. Because OPTs have advantages such as high EQE and low-noise photoconductive mode, OPTs light detection has attracted increasing attention in recent years. By optimizing the materials and structures of OPTs devices, further reducing the dark current of OPTs devices, improving the OPTs photosensitivity, improving the photon-to-charge conversion process, and enhancing the channel carrier mobility have become the direction of people's efforts in recent years.

[0038] Based on this, the present invention provides an organic heterojunction transistor photodetector and a method for preparing the same, see Figure 1 , from bottom to top, it includes a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer, and a charge injection layer. A partial area on the charge injection layer is also provided with a source electrode and a drain electrode.

[0039] Specifically, the present invention achieves extremely low dark current by selecting non-fullerene acceptor molecules as the photosensitive layer. At the same time, a layer heterostructure is formed between the non-fullerene acceptor molecules and the conductive channel layer, which effectively suppresses the off-state dark current, further achieving extremely low dark current and high light response source-drain current of the device, thereby significantly improving the comprehensive performance of the photodetector, such as light detection sensitivity and detection rate.

[0040] In some embodiments, the substrate is made of a rigid material or a flexible material, the rigid material is selected from quartz, glass, and silicon wafer, and the flexible material is plastic.

[0041] In some embodiments, the material of the dielectric layer is selected from SiO2, AlO x , hafnium oxide, ZrO x , polyvinyl alcohol, CYTOP or more; preferably, the material of the dielectric layer is SiO2 or high k dielectric material AlO x 、ZrO x , polyvinyl alcohol, etc.

[0042] In some embodiments, the material of the non-fullerene photosensitive layer is selected from one or more of ITIC, IT-4F, Y6, and IEICO-4F; preferably, the material of the non-fullerene photosensitive layer is ITIC or IT-4F.

[0043] In some embodiments, the material of the conductive channel layer is selected from one or more of C8-BTBT and its derivatives, pentacene and its derivatives, and conjugated polymer semiconductors; the conductive channel layer is a p-type organic semiconductor or an n-type organic semiconductor; preferably, the channel semiconductor layer is a p-type organic semiconductor; more preferably, the p-type organic semiconductor is a C8-BTBT material.

[0044] In some embodiments, the material of the charge injection layer is selected from MoO3, V2O5, NiO x , WO x , CuO x One or more of the .

[0045] In some embodiments, the source electrode, the drain electrode and the gate electrode are respectively selected from one or more of Au, Ag, Cu, Ni, In, Mo, Cr, Al, ITO, PSS:PEDOT, graphene, and carbon nanotubes; those skilled in the art can select the material of the source electrode and the drain electrode according to the matching of the HOMO or LUMO of the organic semiconductor and the metal work function. Preferably, the material of the source electrode and the drain electrode is Au.

[0046] Further preferably, the source electrode and the drain electrode are located on both sides of the conductive channel layer, and a channel is formed between the source electrode and the drain electrode. Preferably, the formed channel has a length of 500-1000 μm and a width of 5-100 μm. More specifically, the length and width of the formed channel are 1000 μm and 100 μm, 800 μm and 80 μm, 600 μm and 60 μm, 400 μm and 40 μm, 200 μm and 20 μm, 100 μm and 10 μm, 80 μm and 8 μm, 50 μm and 5 μm, respectively.

[0047] In some embodiments, the sum of the thickness of the gate and the dielectric layer is 300 nm, the thickness of the photosensitive layer is 30-100 nm, the thickness of the conductive channel layer is 20-200 nm, and the thickness of the source electrode and the drain electrode are both 30-100 nm.

[0048] Optionally, the organic heterojunction transistor photodetector of the present invention may be one of an ultraviolet photodetector, an infrared photodetector, a visible light photodetector and a full-band photodetector.

[0049] The present invention also provides a method for preparing the organic heterojunction transistor photodetector as described in the above embodiment of the present invention, which comprises the steps of:

[0050] S10, providing a substrate;

[0051] S20, sequentially preparing a gate electrode and a dielectric layer on the surface of the substrate;

[0052] S30, preparing a non-fullerene photosensitive layer on the dielectric layer by a solution method and performing a thermal annealing treatment on the non-fullerene photosensitive layer, and preparing a conductive channel layer on the non-fullerene photosensitive layer by a vacuum evaporation method;

[0053] S40, vacuum evaporating a charge injection layer, a source electrode and a drain electrode in sequence on the conductive channel layer through a mask.

[0054] Specifically, the solution method is one of spin coating, scraping coating or spray coating, the solution concentration is 5-15 mg / ml, and the solvent is selected from one or more of chlorobenzene, chloroform, dichloromethane, and o-dichlorobenzene.

[0055] The sizes of the conductive channel layer, the source electrode and the drain electrode can be patterned by a mask, and the channel, source electrode and drain electrode of corresponding sizes can be selected according to actual needs.

[0056] In some embodiments, the temperature of the thermal annealing treatment is 0-90°C, and the time of the thermal annealing treatment is 25-35 minutes; in the step of preparing the conductive channel layer by vacuum evaporation, the substrate heating temperature is 0-60°C.

[0057] More specifically, the method for preparing an extremely low dark current organic transistor photodetector based on small acceptor molecules and a thick channel transport layer comprises the following steps:

[0058] 1) The substrate (on which the gate electrode and dielectric layer have been prepared) is ultrasonically cleaned in acetone, alcohol solvent and deionized water for 5-30 minutes, blown dry with a nitrogen gun, and then treated with UV / ozone or plasma for 5-10 minutes;

[0059] 2) Prepare a 5-15 mg / ml receptor molecule solution (chlorobenzene solution of ITIC or chlorobenzene solution of IT-4F) and stir at 50-80°C for 4-12 hours;

[0060] 3) 40-70 μl of the receptor molecule solution is processed by solution processing (spin coating, scraper coating or spray coating), for example, spin coating is used at a speed of 2000-6000 rpm / s for 30-60 seconds to obtain a 40-80 nm photosensitive layer;

[0061] 4) annealing the substrate with the photosensitive layer deposited thereon at 0-90° C. for 25-40 min;

[0062] 5) A C8-BTBT conductive channel layer is deposited on the photosensitive layer by vacuum evaporation. During the deposition process, the substrate annealing temperature is 0-40°C and the evaporation rate of C8-BTBT is The back vacuum is 3×10 -6 Torr, and finally a 50-120nm C8-BTBT organic conductive channel layer was obtained;

[0063] 6) A 30-100 nm Au layer is vacuum evaporated on both sides of the conductive channel layer through a mask plate as a source electrode and a drain electrode, wherein a channel region is formed between the source electrode and the drain electrode, thereby completing the preparation of an extremely low dark current organic transistor photodetector based on a thick channel transport layer.

[0064] More preferably, the alcohol solvent in step 1) is a commonly used alcohol solvent, such as isopropanol or ethanol.

[0065] More preferably, the ultrasonic cleaning treatment in step 1) is performed for 30 minutes, and the UV / ozone or Plasma surface treatment hydrophilic treatment is performed for 10 minutes.

[0066] More preferably, in step 5), the annealing temperature during the C8-BTBT evaporation process is room temperature, specifically 0 to 25°C.

[0067] More preferably, in step 5), the thickness of the C8-BTBT conductive channel layer is 80 nm.

[0068] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only used to illustrate the present invention but not to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] Example 1

[0070] providing a substrate;

[0071] Sequentially preparing a gate electrode and a dielectric layer on the surface of the substrate;

[0072] Growth of photosensitive layer: The organic semiconductor uses a non-fullerene acceptor 3,9-bis(2-methylene-(3-(1,1-dicyanomethylidene)-indanone)-5,5,11,11-tetra(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indenadiene[1,2-b:5,6-b']-dithiophene (ITIC) and chlorobenzene as a solvent to prepare a 10 mg / ml solution. Take 60 microliters of ITIC chlorobenzene solution and spin coat it on a SiO2 / Si substrate by a spin coating method (3000 rpm×40s), and then anneal at 60°C for 30 minutes to obtain a photosensitive layer film (about 50-70 nm).

[0073] Preparation of the conductive channel layer: 2,7-dioctyl[1]benzothiophene[3,2-b][1]benzothiophene (C8-BTBT) is grown by vacuum evaporation. The substrate speed is 3-10 r / min, and the growth rate of C8-BTBT during the evaporation process is Finally, a conductive channel layer with a thickness of 80 nm is obtained.

[0074] Gold was evaporated as source and drain electrodes.

[0075] like Figure 2 As shown in Figure 2, the dark current of the device is as low as 100 fA, while the light intensity is 2.8 mW / cm 2Under the irradiation of 730nm external light source, when Vg = -22V, the source-drain current (Id) is as high as about 20μA, and the extremely low dark current is only about 20fA. Its light response (R) is as follows Figure 3 As shown, up to 7.2×10 3 A / W, specific detection rate (D * )like Figure 4 Shown>10 17 Jones.

[0076] Example 2

[0077] Growth of photosensitive layer: The organic semiconductor still uses ITIC and chlorobenzene as solvent, but the difference is that the solution is prepared into a 5 mg / ml solution. The film forming process is the same as that of Example 1, and finally a photosensitive layer film (about 30 to 50 nm) is obtained.

[0078] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0079] Gold was evaporated as source and drain electrodes.

[0080] like Figure 5 As shown, the dark current of the obtained device is as low as 100fA. At the same time, when a 730nm infrared light source is applied, its photocurrent shows an increase of 7 orders of magnitude.

[0081] Example 3

[0082] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the concentration of the solution is adjusted to 15 mg / ml, and finally a photosensitive layer film with a thickness of about 70-80 nm is obtained.

[0083] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0084] Gold was evaporated as source and drain electrodes.

[0085] like Figure 6 As shown, the resulting light detection transistor dark current has an extremely low dark current, and the photocurrent also shows an increase of 7 orders of magnitude.

[0086] Example 4

[0087] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the spin coating process is adjusted to (2000 rpm×40 s), and finally a photosensitive layer film with a thickness of about 60-80 nm is obtained.

[0088] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0089] Gold was evaporated as source and drain electrodes.

[0090] The reduction in rotation speed does not significantly affect the thickness of the photosensitive layer, so the device has similar performance to that of Example 1.

[0091] Example 5

[0092] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the spin coating process is adjusted to (4000 rpm×40 s), and finally a photosensitive layer film with a thickness of about 40-50 nm is obtained.

[0093] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0094] Gold was evaporated as source and drain electrodes.

[0095] The increase in rotation speed did not significantly reduce the thickness of the photosensitive layer, and the device performance was similar to that of Example 1.

[0096] Example 6

[0097] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the annealing process is changed to standing at room temperature for 30 minutes to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0098] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0099] Gold was evaporated as source and drain electrodes.

[0100] The photosensitive layer did not show obvious changes, and thus also exhibited extremely low dark current and a photocurrent of up to 6 orders of magnitude.

[0101] Example 7

[0102] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the annealing process is changed to annealing at 90° C. for 30 min to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0103] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0104] Gold was evaporated as source and drain electrodes.

[0105] The photosensitive layer did not show obvious changes, and thus also showed extremely low dark current, and the device performance was similar to that of Example 1.

[0106] Example 8

[0107] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the annealing time is adjusted to 15 minutes to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0108] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0109] Gold was evaporated as source and drain electrodes.

[0110] The resulting photosensitive layer does not undergo significant detail changes, so the device performance is maintained.

[0111] Example 9

[0112] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the solvent is replaced with chloroform to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0113] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0114] Gold was evaporated as source and drain electrodes.

[0115] During the film-forming process of the ITIC solution, the rapid volatilization of chloroform causes the thickness of the photosensitive layer to increase slightly, but the device still exhibits extremely low dark current and excellent photocurrent response.

[0116] Example 10

[0117] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the solvent is replaced with a mixed solution of chlorobenzene and chloroform in a mixing ratio of 1:1 to obtain a photosensitive layer film with a thickness of 55 to 75 nm.

[0118] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0119] Gold was evaporated as source and drain electrodes.

[0120] The thickness of the photosensitive layer of the obtained device did not change significantly, so it also had a dark current of 100fA and a photoresponse source-drain current of about 7 orders of magnitude relative to the dark current.

[0121] Embodiment 11

[0122] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the solvent is replaced with dichloromethane to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0123] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0124] Gold was evaporated as source and drain electrodes.

[0125] The resulting device has an extremely low dark current of about 1pA, and the photoresponse current can also be increased by 5 to 6 orders of magnitude.

[0126] Example 12

[0127] Growing a photosensitive layer: The method for preparing the photosensitive layer is similar to that in Example 1, except that the solvent is replaced with o-dichlorobenzene to obtain a photosensitive layer film with a thickness of 50 to 70 nm.

[0128] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0129] Gold was evaporated as source and drain electrodes.

[0130] The thickness of the device's photosensitive layer did not change significantly, and the extremely low dark current characteristics were maintained.

[0131] Embodiment 13

[0132] Growing a photosensitive layer: The method for preparing the photosensitive layer is the same as that in Example 1.

[0133] Preparation of the conductive channel layer: The method for preparing the conductive channel layer is similar to that in Example 1, except that the conductive channel layer is evaporated with C8-BTBT to a thickness of 50 nm.

[0134] Gold was evaporated as source and drain electrodes.

[0135] like Figure 7 As shown, the resulting device has an extremely low dark current of about 100fA, and its photoresponse source-drain current is improved by >6 orders of magnitude compared to the dark current.

[0136] Embodiment 14

[0137] Growing a photosensitive layer: The method for preparing the photosensitive layer is the same as that in Example 1.

[0138] Preparation of the conductive channel layer: The method for preparing the conductive channel layer is similar to that in Example 1, except that the conductive channel layer is evaporated with C8-BTBT to a thickness of 120 nm.

[0139] Gold was evaporated as source and drain electrodes.

[0140] like Figure 8 As shown, the device still has an extremely low dark current (about 100fA), and its relative dark current is also improved by 7 orders of magnitude under the excitation of an external light source.

[0141] Embodiment 15

[0142] Growing a photosensitive layer: The method for preparing the photosensitive layer is the same as that in Example 1.

[0143] Preparation of the conductive channel layer: The method for preparing the conductive channel layer is similar to that in Example 1, except that the growth rate of C8-BTBT during the evaporation growth process is Finally, a conductive channel layer with a thickness of 80 nm is obtained.

[0144] Gold was evaporated as source and drain electrodes.

[0145] The dark current of the obtained device is about 100fA, and the source-drain current is increased by 7 orders of magnitude compared with the dark state when Vg=0V.

[0146] Example 16

[0147] Growing a photosensitive layer: The method for preparing the photosensitive layer is the same as that in Example 1.

[0148] Preparation of the conductive channel layer: The method for preparing the conductive channel layer is similar to that in Example 1, except that the growth rate of C8-BTBT during the evaporation growth process is Finally, a conductive channel layer with a thickness of 80 nm is obtained.

[0149] Gold was evaporated as source and drain electrodes.

[0150] At a relatively fast growth rate, C8-BTBT can still achieve relatively regular growth, thus exhibiting an extremely low dark current of about 100fA. At the same time, under the irradiation of an external light source of 730nm, when Vg=0, the source-drain current can reach >10μA, which is 7 orders of magnitude higher than the dark state.

[0151] Embodiment 17

[0152] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in the embodiment;

[0153] The difference is that the SiO2 / Si substrate is replaced with high-k ZrO x Replace the SiO2 dielectric layer. Specifically: 2-methoxyethanol is used as a solvent to prepare a 0.2 mol / ml zirconium oxynitrate solution, and after sufficient stirring, a trace amount of acetylacetone and ammonia water are added. After sufficient stirring, in a glove box with an air humidity of less than 30%, the solution is evenly coated on the Si wafer, and a thin film is obtained by spin coating (3000 rpm × 30s), and annealed at 120 ° C for 1 minute, and then transferred to a 300 ° C hot stage for annealing for 5 minutes, and repeated 4 times to obtain a ZrO film with a thickness of about 25 nm. x Dielectric film.

[0154] The resulting device also exhibits an extremely low dark current of about 1pA, and when a near-infrared light source is applied, it shows a photocurrent increase of about 6 orders of magnitude.

[0155] Embodiment 18

[0156] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in Example 1;

[0157] The difference is that high k AlO is used. x Replace the SiO2 dielectric layer. The specific preparation method is the same as that of ZrO in Example 15. x The preparation method is similar to that of the present invention, except that zirconyl nitrate is replaced by aluminum nitrate to obtain a ZrO film with a thickness of about 30 nm. x Dielectric film.

[0158] Similar to Example 15, the change of the dielectric layer did not significantly change the performance of the device, which still exhibited an extremely low dark current of about 100 fA.

[0159] Embodiment 19

[0160] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in Example 1;

[0161] The difference is that the SiO2 / Si substrate is replaced, and the SiO2 dielectric layer is replaced by high-k polyvinyl alcohol. Specifically: 60 mg of PVA powder is dissolved in 3 ml of deionized water, and then 12 mg of 50wt% glutaraldehyde aqueous solution is added. After stirring for one hour, a preliminary cross-linked PVA solution is obtained. 60 microliters of the solution is taken and evenly coated on a heavily doped silicon wafer. A thin film is prepared by spin coating (3000 rpm×30s), and annealed at 100°C for 1 hour to obtain a dielectric layer film with a thickness of about 300 nm.

[0162] The extremely low dark current is similar to that of Example 16, and the light-responsive source-drain current can reach 10 μA.

[0163] Embodiment 20

[0164] Growing a photosensitive layer: The non-fullerene system acceptor in Example 1 is replaced by 3,9-bis(2-methylene-((3-(1,1-dicyanomethylidene)-6,7-difluoro)-indanone))-5,5,11,11-tetra(4-hexylphenyl)-dithiophene[2,3-d:2',3'-d']-s-indenetriene[1,2-b:5,6-b']dithiophene (IT-4F) as the photosensitive layer. The preparation method is similar to that of ITIC, and a photosensitive layer film with a thickness of about 50-60 nm is finally obtained.

[0165] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0166] Gold was evaporated as source and drain electrodes.

[0167] like Fig. 9 As shown, the obtained device has an extremely low dark current. When Vg = -20V, its extremely low dark current can reach <100fA. At the same time, when a 730nm external light source is applied, the light response source leakage current can reach >10μA, as shown in Fig.10 As shown, its photoresponsivity can reach 10 4 , and the highest detection rate can reach 10 18 In addition, Fig. 9 As shown, the device structure can still exhibit a source-drain photocurrent response of >7 orders of magnitude even under the action of an external light source of 900nm.

[0168] Embodiment 21

[0169] Growth of photosensitive layer: The photosensitive layer of the device was constructed in the same manner as in Example 1.

[0170] Preparation of the conductive channel layer: A film-forming method similar to that of Example 1 was used, except that pentacene was used instead of C8-BTBT molecules to obtain a film with a thickness of about 80 nm.

[0171] Gold was evaporated as source and drain electrodes.

[0172] The obtained device still shows dependence on the thickness of the conductive channel layer. Under the influence of the 80nm conductive channel layer, the device still exhibits an extremely low dark current of 100fA and an excellent photoresponse source-drain current of 6 orders of magnitude.

[0173] Embodiment 22

[0174] Growing a photosensitive layer: Different from Example 1, a spraying method is used to construct a photosensitive layer with a thickness of 50-70 nm.

[0175] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0176] Gold was evaporated as source and drain electrodes.

[0177] The photosensitive layer did not undergo significant changes, so after depositing the conductive channel layer, the dark current of the device was about 1pA. At the same time, relative to the dark current, the device had a light-responsive source-drain current of about 6 orders of magnitude.

[0178] Embodiment 21

[0179] Growing a photosensitive layer: The photosensitive layer is constructed in the same manner as in Example 1.

[0180] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0181] The source and drain electrodes are made of copper metal.

[0182] The change of the source and drain electrodes did not cause significant changes in the performance of the device. The extremely low dark current of about 100fA and the photoresponsive source-drain current of 7 to 8 orders of magnitude are still the highlights of the device structure.

[0183] Embodiment 23

[0184] Growing a photosensitive layer: The photosensitive layer is constructed in the same manner as in Example 1.

[0185] Preparation of the conductive channel layer: The conductive channel layer is prepared in the same manner as in Example 1.

[0186] Silver metal is used for source and drain electrodes.

[0187] The experimental results are similar to those of Example 21.

[0188] Embodiment 24

[0189] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in Example 1;

[0190] The difference is that transparent ITO is used instead of heavily doped silicon electrodes, high-k AlO x The specific preparation method is the same as the preparation method of AlOx in Example 16.

[0191] The results of this device are similar to those of Example 16.

[0192] Embodiment 25

[0193] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in Example 1;

[0194] The difference is that transparent ITO is used to replace the heavily doped silicon electrode, and high-k ZrOx is used to replace the SiO2 dielectric layer. The specific preparation method is the same as the preparation method of ZrOx in Example 15.

[0195] The performance of this device structure shows similar performance to that of Example 15.

[0196] Embodiment 26

[0197] The preparation of the photosensitive layer, the conductive channel layer and the electrode is consistent with that in Example 1;

[0198] The difference is that transparent ITO is used to replace the heavily doped silicon electrode, and high-k PVA is used to replace the SiO2 dielectric layer. The specific preparation method is the same as the preparation method of PVA in Example 17.

[0199] The performance of this device structure shows similar performance to that of Example 17.

[0200] Comparative Example 1

[0201] Growing a photosensitive layer: The photosensitive layer is constructed in the same manner as in Example 1.

[0202] Preparation of the conductive channel layer: Similar to Example 1, except that annealing at 50° C. is added during the evaporation process.

[0203] Gold was evaporated as source and drain electrodes.

[0204] like Fig.11 As shown, if annealing is performed simultaneously when constructing the conductive channel layer, the resulting device has an extremely low dark current of about 100fA, but the light-responsive source-drain current is only about 20nA, and the device performance drops rapidly.

[0205] Comparative Example 2

[0206] Growing a photosensitive layer: Similar to Example 1, except that the spin coating method is adjusted to (1000 rpm*40 s).

[0207] Preparation of the conductive channel layer: the same as in Example 1.

[0208] Gold was evaporated as source and drain electrodes.

[0209] The lower rotation speed makes the photosensitive layer extremely uneven, which in turn leads to poor performance of the device, and the light response source leakage current is only about 10nA.

[0210] Comparative Example 3

[0211] Growing a photosensitive layer: Similar to Example 1, except that the spin coating method is adjusted to (6000 rpm*40 s).

[0212] Preparation of the conductive channel layer: the same as in Example 1.

[0213] Gold was evaporated as source and drain electrodes.

[0214] The higher rotation speed makes the photosensitive layer thinner. Although the dark current of the device can still reach 100fA, the source-drain current of the light response is only increased by about 5 orders of magnitude compared to the dark state.

[0215] Comparative Example 4

[0216] Growth of photosensitive layer: same as in Example 1.

[0217] Preparation of the conductive channel layer: Similar to Example 1, except that the thickness of the evaporated C8-BTBT is 30 nm.

[0218] Gold was evaporated as source and drain electrodes.

[0219] like Fig.12 As shown, the thinner conductive channel layer makes the photoresponse source-drain current <1μA, resulting in poor performance.

[0220] Comparative Example 5

[0221] Growth of photosensitive layer: same as in Example 1.

[0222] Preparation of the conductive channel layer: similar to Example 1, except that the substrate rotation speed is 0.

[0223] Gold was evaporated as source and drain electrodes.

[0224] No rotation process is applied during the growth of C8-BTBT, which makes the conductive channel layer grow unevenly, resulting in a higher dark current of about 1nA and a lower photoresponse source-drain current of only 400μA.

[0225] Comparative Example 6

[0226] Growth of photosensitive layer: same as in Example 1.

[0227] Preparation of the conductive channel layer: Similar to Example 1, except that the growth rate of C8-BTBT is Finally, a conductive channel layer of 80 nm is obtained.

[0228] Gold was evaporated as source and drain electrodes.

[0229] The excessively fast growth rate of C8-BTBT results in uneven growth of the conductive channel layer, resulting in a large leakage current, which causes the light-response source-drain current to be as low as 60nA.

[0230] In summary, the present invention discloses an organic heterojunction transistor photodetector and a preparation method thereof, which includes, from bottom to top, a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer, and a charge injection layer, wherein a partial area on the charge injection layer is also provided with a source electrode and a drain electrode. The present invention realizes extremely low dark current by selecting non-fullerene acceptor molecules as the photosensitive layer, and at the same time, a layer heterostructure is formed between the non-fullerene acceptor molecules and the conductive channel layer, thereby realizing effective suppression of off-state dark current, further realizing extremely low dark current and high light response source leakage current of the device, so that the comprehensive performance of the photodetector, such as light detection sensitivity and detection rate, is significantly improved.

[0231] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An organic heterojunction transistor photodetector, characterized in that: From bottom to top, it includes a substrate, a gate electrode, a dielectric layer, a non-fullerene photosensitive layer, a conductive channel layer, and a charge injection layer. A partial area on the charge injection layer is also provided with a source electrode and a drain electrode.

2. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The substrate is made of a rigid material or a flexible material, the rigid material is selected from quartz, glass, and silicon wafer, and the flexible material is plastic.

3. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The material of the dielectric layer is selected from SiO2, AlO x , hafnium oxide, ZrO x , polyvinyl alcohol, and CYTOP.

4. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The material of the non-fullerene photosensitive layer is selected from one or more of ITIC, IT-4F, Y6, and IEICO-4F.

5. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The material of the conductive channel layer is selected from one or more of C8-BTBT and its derivatives, pentacene and its derivatives, and conjugated polymer semiconductors.

6. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The material of the charge injection layer is selected from MoO3, V2O5, NiO x , WO x , CuO x One or more of the .

7. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The source electrode, the drain electrode and the gate electrode are respectively selected from one or more of Au, Ag, Cu, Ni, In, Mo, Cr, Al, ITO, PSS:PEDOT, graphene, and carbon nanotubes.

8. The organic heterojunction transistor photodetector according to claim 1, characterized in that: The total thickness of the gate and the dielectric layer is 300 nm, the thickness of the photosensitive layer is 30-100 nm, the thickness of the conductive channel layer is 20-200 nm, and the thickness of the source electrode and the drain electrode are both 30-100 nm.

9. A method for preparing an organic heterojunction transistor photodetector according to any one of claims 1 to 8, characterized in that: Includes steps: providing a substrate; Sequentially preparing a gate electrode and a dielectric layer on the surface of the substrate; On the dielectric layer, a non-fullerene photosensitive layer is prepared by a solution method, and the non-fullerene photosensitive layer is subjected to a thermal annealing treatment; A conductive channel layer is prepared on the non-fullerene photosensitive layer after thermal annealing by vacuum evaporation; A charge injection layer, a source electrode and a drain electrode are sequentially vacuum-deposited on the conductive channel layer through a mask.

10. The preparation method according to claim 9, characterized in that: The temperature of the thermal annealing treatment is 0-90° C., and the time of the thermal annealing treatment is 25-35 minutes; in the step of preparing the conductive channel layer by vacuum evaporation, the substrate heating temperature is 0-60° C.