Interfacial interaction spin-photon conversion body heterostructure and preparation method thereof

By using the interface interaction between chiral perovskite and lead halide in heterostructure, the spin relaxation time is extended, the spin-photon conversion efficiency is improved, and the low circular polarization polarization degree in the prior art is solved Problem, efficient spin-photon conversion and high circular polarization polarization are achieved.

CN118946165APending Publication Date: 2024-11-12WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970395.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing heterostructures based on chiral spin filters and optical absorbers or emitters have a circular polarization polarization value of less than 20% at room temperature, which is reduced due to rapid spin relaxation in the absorbers or emitters. Spin-photon conversion efficiency makes it difficult to achieve high-efficiency spin-photon conversion and high circular polarization polarization.

Method used

By constructing a heterostructure composed of chiral spin filters and inorganic light absorbers, spin relaxation in the absorbers is suppressed using interface interactions, including chiral perovskites as spin filters and lead halide as optical Absorber extends the spin relaxation time through asymmetric hydrogen bond interactions and improves spin-photon conversion efficiency.

Benefits of technology

The spin relaxation time in the absorber is significantly extended, the spin-photon conversion efficiency is improved, and a circular polarization polarization of 36.5% is achieved in the circular polarization light detector, surpassing the effects of the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946165A_ABST
    Figure CN118946165A_ABST
Patent Text Reader

Abstract

The invention discloses an interfacial interaction spin-photon conversion bulk heterostructure and a preparation method thereof. The bulk heterostructure comprises a chiral spin filter and an optical absorber, wherein the optical absorber is vertically inserted into the chiral spin filter; the optical absorber is lead halide; and the chiral spin filter is chiral perovskite containing halogen and lead. According to the bulk heterostructure disclosed by the invention, the transmission of chirality from a chiral spin filter to an optical absorber can be realized through the interaction of asymmetric hydrogen bonds at an interface, the spin-photon conversion efficiency in the absorber is remarkably improved, and 36.5% circular polarization degree is realized in a circularly polarized light detector based on the bulk heterostructure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chiral perovskite materials, and in particular to an interface-interactive spin-photon converter heterostructure and a preparation method thereof. Background Art

[0002] Photons have an intrinsic chiral property, i.e. circularly polarized light, in which the electric field vector of the light exhibits a clockwise or counterclockwise rotation in the propagation direction. This chiral property of photons plays a key role in many fields, such as photonics, optoelectronics, optical spintronics, and quantum physics. In recent years, chirality-induced self-selection (CISS) has been exploited to manipulate chiral light through spin-photon conversion, in which charge transport in homochiral molecules exhibits a significant chirality-dependent spin filtering effect. By integrating chiral spin filters with achiral optical absorbers or emitters into heterostructures, charge-photon and spin-charge conversions can be decoupled, thereby combining excellent optoelectronic and spintronic properties to achieve chiral light manipulation. Many efforts have been devoted to assembling chiral organic molecules into supramolecules or anchoring chiral organic molecules on inorganic frameworks to maximize the spin selectivity of chiral spin filters. However, the circular polarization degree of polarization (DOP) values ​​of devices based on chiral spin filters and optical absorber or emitter heterostructures are still less than 20% at room temperature, which may be due to the fast spin relaxation (a few picoseconds at room temperature) in the absorber or emitter, which reduces the spin-to-photon conversion efficiency. Therefore, suppressing spin relaxation in the absorber or emitter to achieve efficient spin-to-photon conversion and high DOP has become a major challenge in current research. Summary of the invention

[0003] The purpose of the present invention is to construct a heterostructure consisting of a chiral spin filter and an inorganic light absorber to achieve efficient spin-photon conversion, suppress spin relaxation in the absorber through strong interface interaction, and improve the spin-photon conversion efficiency.

[0004] In order to achieve the above-mentioned object, the present invention provides an interface-interacting spin-photon converter heterostructure, comprising a chiral spin filter and an optical absorber; wherein the optical absorber is vertically inserted into the chiral spin filter; The optical absorber is lead halide; The chiral spin filter is a chiral perovskite containing halogen and lead.

[0005] Further, the optical absorber accounts for 0%-50% of the bulk heterostructure, excluding the endpoint value of 0%; The ratio increases as the heat treatment time of the chiral perovskite containing halogen and lead increases.

[0006] The present invention also provides a circularly polarized light detector, comprising the above-mentioned bulk heterostructure.

[0007] The present invention also provides a method for preparing the above-mentioned bulk heterostructure, comprising: The lead salt, the chiral organic halide ammonium salt and the solvent are mixed and dissolved to obtain a precursor solution; After adding an anti-solvent to the precursor solution, the liquid is removed by heat treatment to obtain a chiral perovskite; The chiral perovskite is further heat treated to obtain an interface-interacting spin-photon converter heterostructure.

[0008] Further, the heat treatment of removing the solution is continued at 80-120°C for 3-8 minutes; The heat treatment is continued at 80-120°C for 10-100 min.

[0009] Preferably, the continued heat treatment is continued at 80-120° C. for 20-30 min.

[0010] Furthermore, the concentration of the lead salt and the chiral organic halide ammonium salt is 0.5-1.5 mol / L.

[0011] Furthermore, the chiral organic halide ammonium salt is obtained by reacting a chiral organic amine with a hydrohalic acid aqueous solution; Wherein, the chiral organic amine includes at least one of (R)-1-(1-naphthyl)ethylamine, (S)-1-(1-naphthyl)ethylamine, (R)-α-methylbenzylamine, (S)-α-methylbenzylamine, (R)-β-methylphenethylamine, (S)-β-methylphenethylamine, (R)-1-phenylpropylamine, (S)-1-phenylpropylamine, (R)-1-(2-naphthyl)ethylamine, (R)-1-(2-bromophenyl)-ethylamine, (S)-1-(2-bromophenyl)-ethylamine, (R)-1-(3-bromophenyl)-ethylamine, (S)-1-(3-bromophenyl)-ethylamine, (R)-1-(4-bromophenyl)-ethylamine, and (S)-1-(4-bromophenyl)-ethylamine.

[0012] Specifically, the preparation method of the chiral organic halide ammonium salt comprises: dissolving the chiral organic amine in an organic solvent, evacuating the solution and introducing nitrogen to maintain the vacuum environment, then adding a hydrohalic acid aqueous solution and phosphorous acid, stirring the reaction at a low temperature, and purifying the solid product obtained by removing the impurity liquid to obtain the chiral organic halide ammonium salt. Preferably, the solute in the hydrohalic acid aqueous solution comprises at least one of hydrogen iodide and hydrogen bromide.

[0013] Further, the lead salt includes at least one of lead halide and lead acetate. Preferably, the lead halide includes at least one of lead chloride, lead bromide and lead iodide.

[0014] Furthermore, the solvent includes at least one of dimethyl sulfoxide and N,N-dimethylformamide.

[0015] The type of anti-solvent does not need to be strictly limited. For example, it can be at least one of chlorobenzene, chloroform, ether, and the like.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The bulk heterostructure of the present invention can realize the transfer of chirality from the chiral spin filter to the optical absorber through asymmetric hydrogen bonding interactions at the interface, significantly prolong the spin relaxation time in the absorber and increase the spin-photon conversion efficiency, and achieve a circular polarization polarization degree of 36.5% in a circularly polarized light detector based on the bulk heterostructure. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 The schematic diagram of the structure of the circularly polarized light detector prepared in Example 5 is shown; Figure 2 The surface morphology of the R-NEAIPbI2 material prepared in the comparative example is shown; Figure 3 The surface morphology of the bulk heterostructure prepared in Example 1 is shown; Figure 4 The surface morphology of the bulk heterostructure prepared in Example 2 is shown; Figure 5 The surface morphology of the bulk heterostructure prepared in Example 3 is shown; Figure 6 The surface morphology of the bulk heterostructure prepared in Example 4 is shown; Figure 7 shows a cross-sectional morphology of the bulk heterostructure prepared in Example 2; Figure 8 CD spectra of bulk heterostructures prepared in Examples 1-4 and Comparative Examples are shown; Fig. 9 The photocurrent response diagram of the circularly polarized light detector prepared in Example 5 under left-handed circularly polarized light and right-handed circularly polarized light of 505 nm is shown. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0020] The following will be combined with the specific embodiments of the present invention and the drawings of the specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1 A method for preparing an interface-interacting spin-photon converter heterostructure comprises the following steps: S1. Synthesis of chiral organic halide ammonium salts 12 mL of (R)-1-(1-naphthyl)ethylamine (R-NEA) was dissolved in 50 mL of anhydrous ethanol, and the vacuum environment was maintained by evacuating and continuously introducing nitrogen; 20 mL of 45% aqueous hydrogen iodide solution and 2 mL of phosphorous acid were slowly added, and the reaction was continuously stirred at 0°C for 2 hours, and then the resulting solution was placed at 80°C for vacuum drying to obtain a light yellow solid; the yellow solid was dissolved in 25 mL of anhydrous ethanol, and then 150 mL of anhydrous ether was added for precipitation, and the product was collected by filtration, and the process was repeated three times to obtain a pure white powder product, namely, the iodine salt of (R)-1-(1-naphthyl)ethylamine R-NEAI.

[0022] S2. Preparation of bulk heterostructures, S201, soaking the nahcolite glass in detergent, pure water, acetone and isopropanol respectively and ultrasonically cleaning them for 15 minutes, and then treating the cleaned nahcolite glass with ultraviolet ozone (UVO) for 30 minutes to obtain pretreated glass; S202, dissolving PbI2 and R-NEAI in N,N-dimethylformamide, and heating on a 70°C hot plate for 1 h to obtain a precursor solution with a concentration of PbI2 and R-NEAI of 0.9 mol / L; S203, adding 50 μL of the precursor solution to the pretreated glass surface and then spin coating, first at 1000 rpm for 10 seconds, then at 5000 rpm for 60 seconds, and adding 200 μL of chlorobenzene as an anti-solvent at 30 seconds, and then transferring to a 100°C hot plate for annealing for 5 minutes to obtain R-NEAIPbI2 material; S204. Continue annealing on the hot plate for 10 minutes to obtain a NEAPbI3@PbI2 bulk heterojunction.

[0023] Tests have shown that the proportion of PbI2 in the NEAPbI3@PbI2 bulk heterojunction obtained in this embodiment is 2.0%.

[0024] Example 2-Example 4 It is basically the same as Example 1, except that the annealing time in step S204 of preparing the bulk heterostructure is 25 minutes, 55 minutes, and 85 minutes respectively. Accordingly, the proportion of PbI2 in the NEAPbI3@PbI2 bulk heterojunction obtained in Examples 2 to 4 is 6.0%, 19.9%, and 45.7% respectively.

[0025] Comparative Example The method is basically the same as Example 1, except that the preparation of the bulk heterostructure does not include step S204.

[0026] Example 5 A method for preparing a circularly polarized light detector comprises the following steps: T1. Substrate pretreatment Indium tin oxide glass (ITO) was immersed in detergent, pure water, acetone and isopropanol and ultrasonically cleaned for 15 minutes, and then the cleaned indium tin oxide glass was treated with ultraviolet ozone (UVO) for 30 minutes to obtain a pretreated substrate.

[0027] T2. Preparation of electron transport layer The SnO2 colloidal dispersion was diluted to 2 wt % and then spin-coated on the surface of the pretreated substrate at 3000 rpm for 30 s, followed by annealing at 150 °C for 30 min.

[0028] T3. Preparation of bulk heterostructures The preparation steps are the same as those in Example 1, but the annealing is continued for 25 minutes, that is, the total annealing time is 30 minutes. The specific preparation process will not be described in detail here.

[0029] T4. Preparation of hole transport layer Above the bulk heterostructure, below 8×10 -5 Pa, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) was deposited to form a hole transport layer.

[0030] T5. Preparation of metal electrodes An Ag layer was deposited on the upper side of the interface modification layer by vacuum evaporation.

[0031] Through the above steps, we can get Figure 1The circularly polarized light detector shown has an active area of ​​2×2 mm 2 .

[0032] Test Case The surface morphology of the bulk heterostructures prepared in the embodiment and the comparative example was observed using a scanning electron microscope. The results are as follows: Figure 2-Figure 6 As shown. Figure 2 It can be seen that the pure chiral perovskite material R-NEAIPbI2 has an inhomogeneous granular structure; Figure 3-Figure 6 It shows that as the annealing time increases, PbI2 is gradually formed on the surface of R-NEAIPbI2 and is vertically inserted. In Example 4 where the annealing time is longer, PbI2 shows obvious agglomeration. Figure 7 The interface morphology of the bulk heterostructure prepared in Example 2 is also shown, and it can be clearly seen that PbI2 is vertically inserted at the interface.

[0033] The CD spectra of the bulk heterostructures of the embodiment and the comparative example are shown as follows: Figure 8 As shown. Figure 8 In the figure, the double peaks with opposite signals near 400nm correspond to the circular dichroism response of R-NEAPbI3, while the CD shoulder at 500nm corresponds to the circular dichroism effect of the PbI2 phase, which is caused by the interface chirality transfer from R-NEAPbI3 to PbI2, indicating that PbI2 has a spin splitting band structure due to the chirality-induced inversion asymmetry. The positive CD response near 500nm increases with the increase of PbI2 concentration, and the CD peak near 400nm first increases and then decreases with the PbI2 concentration. In Example 2, when the PbI2 concentration is 6.0%, not only the intrinsic chirality of R-NEAPbI3 is well retained, but also efficient interface chirality transfer can be achieved, inducing the PbI2 phase to produce strong intrinsic chirality.

[0034] The circularly polarized light detector prepared in Example 5 was irradiated with left-handed circularly polarized light and right-handed circularly polarized light of 505 nm respectively. The circularly polarized light was absorbed by the PbI2 optical absorber, thereby detecting the difference in the photocurrent response of the device in different circular polarization states. The spin-to-photon conversion efficiency was expressed as the circular polarization polarization degree. To measure, I L and I R is the photocurrent response generated by the device under left-handed circularly polarized light and right-handed circularly polarized light. The results are as follows Fig. 9 It can be seen that the maximum DOP of the device working under -0.4V bias is as high as 36.5%, which is the highest value reported so far in heterostructures using chiral filters.

[0035] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An interface-interacting spin-photon converter heterostructure, It is characterized in that Includes chiral spin filters and optical absorbers; wherein the optical absorber is vertically inserted into the chiral spin filter; The optical absorber is lead halide; The chiral spin filter is a chiral perovskite containing halogen and lead.

2. The interfacially interacting spin-photon converter heterostructure according to claim 1, It is characterized in that The optical absorber accounts for 0%-50% of the bulk heterostructure, excluding the endpoint value of 0%; The ratio increases as the heat treatment time of the chiral perovskite containing halogen and lead increases.

3. A circularly polarized light detector, It is characterized in that Comprising the bulk heterostructure as described in claim 1 or 2.

4. A method for preparing a bulk heterostructure as claimed in claim 1 or 2, It is characterized in that include, The lead salt, the chiral organic halide ammonium salt and the solvent are mixed and dissolved to obtain a precursor solution; After adding an anti-solvent to the precursor solution, the liquid is removed by heat treatment to obtain a chiral perovskite; The chiral perovskite is further heat treated to obtain an interface-interacting spin-photon converter heterostructure.

5. The method for preparing a bulk heterostructure according to claim 4, It is characterized in that The heat treatment to remove the solution lasts for 3-8 min at 80-120°C; The heat treatment is continued at 80-120°C for 10-100 min.

6. The method for preparing a bulk heterostructure according to claim 4, It is characterized in that The chiral organic halide ammonium salt is obtained by reacting a chiral organic amine with a hydrohalic acid aqueous solution; Wherein, the chiral organic amine includes at least one of (R)-1-(1-naphthyl)ethylamine, (S)-1-(1-naphthyl)ethylamine, (R)-α-methylbenzylamine, (S)-α-methylbenzylamine, (R)-β-methylphenethylamine, (S)-β-methylphenethylamine, (R)-1-phenylpropylamine, (S)-1-phenylpropylamine, (R)-1-(2-naphthyl)ethylamine, (R)-1-(2-bromophenyl)-ethylamine, (S)-1-(2-bromophenyl)-ethylamine, (R)-1-(3-bromophenyl)-ethylamine, (S)-1-(3-bromophenyl)-ethylamine, (R)-1-(4-bromophenyl)-ethylamine, and (S)-1-(4-bromophenyl)-ethylamine.

7. The method for preparing a bulk heterostructure according to claim 4, It is characterized in that The lead salt includes at least one of lead halide and lead acetate.