Method for manufacturing thermoelectric thin film based on laser liquid phase sintering mixed nanoparticles
Through laser liquid phase sintering technology, the problems of the suitability and sintering degree regulation of multi-component materials of thermoelectric films are solved, and efficient and low-cost thermoelectric film manufacturing is achieved, which significantly improves the thermoelectric performance and exceeds the limitations of traditional physical vapor deposition methods. .
Patent Information
- Application Number
- CN202411012073.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing thermoelectric film manufacturing methods, multi-component materials are not suitable, the degree of sintering is limited, the process takes a long time and high cost, making the performance of thermoelectric films difficult to meet the requirements of bulk thermoelectric materials.
Using a hybrid nanoparticle manufacturing method based on laser liquid phase sintering, Ni-SrTiO3 mixed nanoparticle ink is deposited through inkjet printing, and laser sintering technology is used to regulate grain growth and melting to achieve efficient manufacturing of multi-component thermoelectric films.
It realizes high-efficiency and low-cost multi-component thermoelectric film manufacturing, improves the thermoelectric performance of thermoelectric films, exceeds the limitations of traditional physical vapor deposition methods, and achieves excellent thermoelectric characteristics.
Smart Images

Figure CN118946235A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermoelectric thin film materials, and in particular relates to a method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles. Background Art
[0002] With the trend of green development and energy conservation and emission reduction, thermoelectric materials that can directly convert heat into electrical energy have attracted the interest of a large number of researchers. After more than 20 years of development, the optimal zT value of bulk thermoelectric materials can be close to 2, which is attributed to material selection and process optimization. At present, the mixed process of ball milling (BM) and spark plasma sintering (SPS) is the mainstream method for manufacturing bulk thermoelectric materials. Based on this bottom-up powder metallurgy-like process, the material composition, microstructure, sintering / melting degree, etc. can be easily and quickly controlled to optimize key performance indicators such as thermal conductivity, electrical conductivity, and Seebeck coefficient in a higher dimension. When BM and SPS are used to manufacture multi-component mixed particles, the liquid phase sintering state (sintering temperature is between the low melting point and high melting point of different components, and liquid and solid phases coexist) is often conducive to the improvement of its thermoelectric performance.
[0003] In recent years, flexible, lightweight and low-cost thermoelectric thin film materials have gradually become a new track for thermoelectric material manufacturing. However, the geometric limitations of two-dimensional thin films in terms of thickness make BM and SPS processes unsuitable. Currently, physical vapor deposition is a common method for manufacturing thermoelectric thin films, but this method faces the disadvantages of being unsuitable for multi-component materials, limited control of sintering degree, long process time and high cost, resulting in the thermoelectric performance of thermoelectric thin films always being difficult to reach the corresponding bulk thermoelectric materials. Therefore, developing a multi-component thermoelectric film strategy that can widely control the sintering degree is the key to improving the performance of thermoelectric films. Summary of the invention
[0004] In order to solve the problems of existing physical vapor deposition manufacturing methods of thermoelectric films, such as the inapplicability of multi-component materials, limited control of sintering degree, long process time, high cost, and difficulty in meeting the requirements of thermoelectric properties of thermoelectric films, the present invention provides a method for manufacturing thermoelectric films based on laser liquid phase sintering of mixed nanoparticles to solve the above technical problems.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0006] The present invention discloses a thermoelectric film made of mixed nanoparticles by laser liquid phase sintering, which specifically comprises:
[0007] A base layer and three Ni-SrTiO3 mixed nanoparticle inks with different mass fractions sequentially deposited on the base layer by inkjet printing;
[0008] The three Ni-SrTiO3 mixed nanoparticle inks are all mixed by Ni nanoparticles and SrTiO3 nanoparticles in different mass ratios; the mass ratios of the Ni nanoparticles and SrTiO3 nanoparticles are 3:7, 2:8 and 1:9 respectively; the mass fractions of the three Ni-SrTiO3 mixed nanoparticle inks are all 12-15%.
[0009] The present invention provides a method for manufacturing a thermoelectric thin film based on laser liquid phase sintering of mixed nanoparticles, which specifically comprises the following steps:
[0010] (1) Preparing Ni-SrTiO3 mixed nanoparticle ink;
[0011] (2) Ni-SrTiO3 mixed nanoparticle film inkjet printing deposition;
[0012] (3) Laser sintering of Ni-SrTiO3 mixed nanoparticle film: The substrate temperature of the Ni-SrTiO3 mixed nanoparticle film after inkjet printing deposition is controlled at 50-52°C. After adjusting the laser spot diameter, setting the laser scanning path, and adjusting the laser sintering parameters in sequence, a single laser sintering of the deposition line is started to promote grain growth or partial melting.
[0013] The specific process of step (1) is as follows: Ni nanoparticles and SrTiO3 nanoparticles are fully mixed in different mass ratios to prepare three parts of Ni-SrTiO3 mixed nanoparticles, and the three parts are dispersed in organic solvents respectively, and then ultrasonically dispersed and filtered to prepare three parts of Ni-SrTiO3 mixed nanoparticle inks with a mass fraction of 12-15%.
[0014] Preferably, the mass ratios of the Ni nanoparticles and the SrTiO3 nanoparticles are 3:7, 2:8 and 1:9 respectively.
[0015] Preferably, the particle size of the Ni nanoparticles is 30-40 nm; the particle size of the SrTiO3 nanoparticles is 100-150 nm.
[0016] Preferably, the power during ultrasonic dispersion is 120-200 W and the temperature is 10-15°C.
[0017] The specific process of step (2) is as follows: selecting an Al2O3 ceramic substrate, ultrasonically cleaning it, and drying it for use; preparing a droplet sequence corresponding to three Ni-SrTiO3 mixed nanoparticle inks; controlling the temperature of the Al2O3 ceramic substrate to 130-140°C, setting printing parameters and patterns, and sequentially printing three droplet sequences corresponding to the Ni-SrTiO3 mixed nanoparticle inks.
[0018] Preferably, when preparing three droplet sequences corresponding to Ni-SrTiO3 mixed nanoparticle inks, the inkjet printing waveform is a positive pressure of 60-70V, a negative pressure of 75-85V, a reference voltage of 0-5V, a positive pressure rise time of 5-8ms, a positive pressure duration of 30-40ms, a positive pressure fall time of 10-20ms, a negative pressure duration of 40-50ms, and a negative pressure rise time of 5-8ms.
[0019] Preferably, the printing parameters are: horizontal printing dot spacing 0.025-0.03 mm, vertical printing dot spacing 0.03-0.035 mm, and printing speed 15-17 mm / s.
[0020] Preferably, the laser spot diameter is 0.3-0.31 mm; the laser is a Nd-YAG laser with a wavelength of 1064 nm; the laser scanning path is a zigzag mode (ZigZag); the laser sintering parameters are: power 20-40 W, scanning speed 100-120 mm / s, scanning line spacing 0.01-0.015 mm.
[0021] The beneficial effects of the present invention are:
[0022] (1) The present invention provides a method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles, which realizes the high-efficiency and high-economic-benefit manufacturing of multi-component mixed material thermoelectric thin films. Traditional physical vapor deposition methods are difficult to manufacture multi-component thermoelectric thin films, which limits the further improvement of the thermoelectric properties of thermoelectric thin films. The present invention benefits from the bottom-up high-freedom film manufacturing process of nanoparticle mixing and inkjet printing, and realizes the manufacture of multi-component thermoelectric thin films with controllable ratios, laying the foundation for the optimization of thermoelectric performance.
[0023] (2) The present invention provides a method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles, which realizes liquid phase sintering of thermoelectric thin films. Different from the traditional physical vapor deposition method, benefiting from the optical properties of inkjet printing mixed nanoparticles and laser energy input regulation, instantaneous high-temperature laser sintering of thermoelectric thin films can be achieved, thereby manufacturing thermoelectric thin films in a laser liquid phase sintering state (thermoelectric material structure with excellent performance). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The sintering state / melting degree of the film under different nanoparticle ratios and laser powers.
[0025] Figure 2 This is the comprehensive thermoelectric performance curve of laser liquid phase sintered films compared with traditional solid phase sintered films. DETAILED DESCRIPTION
[0026] The present invention discloses a thermoelectric film made of mixed nanoparticles based on laser liquid phase sintering, which specifically includes: a base layer;
[0027] and, sequentially inkjet printing three Ni-SrTiO3 mixed nanoparticle inks with different mass fractions deposited on the base layer;
[0028] Among them, the three Ni-SrTiO3 mixed nanoparticle inks are all mixed by Ni nanoparticles and SrTiO3 nanoparticles in different mass ratios.
[0029] Preferably, the mass ratios of Ni nanoparticles to SrTiO3 nanoparticles are 3:7, 2:8 and 1:9 respectively, but not limited thereto.
[0030] Preferably, the mass fractions of the three Ni-SrTiO3 mixed nanoparticle inks are all 12-15%, but not limited thereto.
[0031] Preferably, the base layer is an Al2O3 ceramic substrate, but is not limited thereto.
[0032] The present invention discloses a method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles, which mainly includes three steps: preparation of mixed nanoparticle ink, inkjet printing deposition of mixed nanoparticle thin films, and laser sintering of mixed nanoparticle thin films. The present invention can be used to manufacture various types of mixed nano thermoelectric thin films.
[0033] The present invention provides a method for manufacturing a thermoelectric thin film based on laser liquid phase sintering of mixed nanoparticles, and the specific manufacturing process thereof includes:
[0034] 1. Preparation of Ni-SrTiO3 mixed nanoparticle ink: The obtained Ni-SrTiO3 mixed nanoparticle ink has better dispersibility and stability than the prior art, which can reduce the influence of nanoparticle agglomeration and sedimentation on the uniformity of the deposition layer during the inkjet printing deposition process, thereby ensuring the continuity of the inkjet printing deposition process and the consistency of the inkjet droplets.
[0035] 2. Inkjet printing deposition of Ni-SrTiO3 mixed nanoparticle film: Since Ni-SrTiO3 mixed nanoparticle ink is more prone to aggregation and sedimentation, in order to obtain a better deposition route, the present invention optimizes and adjusts the inkjet printing deposition steps and parameters, and prepares Ni-SrTiO3 mixed nanoparticle films with different component proportions by inkjet printing deposition, thereby obtaining a Ni-SrTiO3 mixed nanoparticle film with high surface flatness and uniformity, thereby avoiding local ablation and film failure problems caused by uneven deposition.
[0036] 3. Laser sintering of Ni-SrTiO3 mixed nanoparticle film: Laser sintering is used to promote grain coarsening and even partial melting, and the thermoelectric properties of the film are measured to obtain the optimal thermoelectric properties.
[0037] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0038] Example 1
[0039] A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles, the specific manufacturing steps are as follows:
[0040] (1) Preparation steps of Ni-SrTiO3 mixed nanoparticle ink;
[0041] 1) Add 7±0.07g SrTiO3 nanoparticles (particle size 125nm) to 3±0.03g Ni nanoparticles (particle size 35nm), and fully mix the two nanoparticles by shaking or stirring to prepare the first portion of Ni-SrTiO3 mixed nanoparticles; add 8±0.08g SrTiO3 nanoparticles (particle size 125nm) to 2±0.02g Ni nanoparticles (particle size 35nm), and fully mix the two nanoparticles by shaking or stirring to prepare the second portion of Ni-SrTiO3 mixed nanoparticles; add 9±0.09g SrTiO3 nanoparticles (particle size 125nm) to 1±0.01g Ni nanoparticles (particle size 35nm), and fully mix the two nanoparticles by shaking or stirring to prepare the third portion of Ni-SrTiO3 mixed nanoparticles, thereby obtaining three different portions of Ni-SrTiO3 mixed nanoparticles.
[0042] 2) The three different Ni-SrTiO3 mixed nanoparticles are dispersed in organic solvents composed of ethylene glycol and isopropanol to prepare three Ni-SrTiO3 mixed nanoparticle inks with mass fractions of 12%, 13% and 15%, respectively, wherein the mass ratio of ethylene glycol to isopropanol is 0.85.
[0043] 3) The three Ni-SrTiO3 mixed nanoparticle inks with mass fractions of 12%, 13% and 15% were ultrasonically dispersed in an ultrasonic crusher with a power of 165 W for 2.5 hours, and the ink dispersion temperature was controlled at 15° C. in a water bath.
[0044] 4) The ink was filtered using a PTFE filter membrane with a pore size of 0.45 μm to obtain three Ni-SrTiO3 mixed nanoparticle inks with different mass fractions that can be used for inkjet printing.
[0045] (2) Ni-SrTiO3 mixed nanoparticle film inkjet printing deposition step;
[0046] 1) Before inkjet printing deposition, the Al2O3 ceramic substrate was thoroughly cleaned with an ultrasonic cleaner, and then treated with isopropanol, ethanol and ultrapure water for 3 minutes in sequence, and dried in a hot oven for later use.
[0047] 2) Setting a suitable inkjet printing waveform to prepare three droplet sequences corresponding to the Ni-SrTiO3 mixed nanoparticle ink; wherein, the suitable inkjet printing waveform may specifically be a positive pressure of 60-70V, a negative pressure of 75-85V, a reference voltage of 0-5V, a positive pressure rise time of 5-8ms, a positive pressure duration of 30-40ms, a positive pressure fall time of 10-20ms, a negative pressure duration of 40-50ms, and a negative pressure rise time of 5-8ms.
[0048] 3) The temperature of the Al2O3 ceramic substrate is controlled to 135°C using a temperature-controllable heating stage.
[0049] 4) The printing parameters and patterns can be set through the host computer software; the printing parameters can be specifically: horizontal printing dot spacing 0.025mm, vertical printing dot spacing 0.03mm, printing rate 16mm / s; the printing pattern can be specifically: 2×10mm rectangular line; according to the first Ni-SrTiO3 mixed nanoparticle ink with a mass fraction of 12%, the Ni-SrTiO3 mixed nanoparticle ink with a mass fraction of 13% and the Ni-SrTiO3 mixed nanoparticle ink with a mass fraction of 15%.
[0050] (3) Laser sintering step of Ni-SrTiO3 mixed nanoparticle film;
[0051] 1) Place the Al2O3 ceramic substrate with printed deposition circuits on a temperature-controllable heating table and set the heating temperature to 51°C.
[0052] 2) The spot diameter of the continuous wave Nd-YAG (wavelength 1064 nm) laser is adjusted to 0.3 mm.
[0053] 3) Set the laser scanning path to zigzag mode (ZigZag).
[0054] 4) Adjust the laser sintering parameters: power 35 W, scanning speed 115 mm / s, scanning line spacing 0.015 mm, and perform single laser sintering on the deposition line to promote grain growth or partial melting.
[0055] (4) The microscopic morphology of each Ni-SrTiO3 circuit after sintering (SEM) was characterized to determine the range of laser liquid phase sintering. Thermoelectric performance tests (including thermal conductivity, electrical conductivity, Seebeck coefficient, etc.) were carried out on the samples within the range of laser liquid phase sintering to determine the optimal thermoelectric performance film and obtain the optimal thermoelectric characteristic working conditions.
[0056] The core idea of the present invention is to realize the laser sintering / melting state control of thermoelectric thin films by regulating the film components (especially the relative proportion of multi-component mixed nanoparticles) and laser sintering parameters, thereby realizing the manufacture of high-performance thermoelectric thin films.
[0057] The present invention first realizes the deposition of thermoelectric thin films with controllable components by inkjet printing inks with different nanoparticle ratios. On the one hand, different metal / semiconductor materials exhibit significantly different thermoelectric properties (including thermal conductivity, electrical conductivity, Seebeck coefficient, etc.), and the optimization of the composition of nanoparticles is an effective control handle for the thermoelectric properties of thin films; on the other hand, the control of film composition can optimize the optical properties of the film, especially the absorbance, which is crucial for the subsequent laser sintering temperature, grain coarsening, and sintering state control. Secondly, by adjusting the laser sintering parameters, the degree of sintering / melting of the film can be controlled ( Figure 1 ), and then regulate the thermoelectric properties of the film, and optimize the film performance under orthogonal realization ( Figure 2 ).
[0058] like Figure 1 As shown in the figure, when the mass fraction of Ni nanoparticles in Ni-SrTiO3 mixed nanoparticles is 10wt%, as the laser power increases from 20W to 35W, the microscopic density gradually increases, the grains gradually coarsen, and the degree of sintering increases. When the laser power reaches 40W, a liquid phase sintering mode (solid phase grains are incorporated into the liquid phase matrix) is observed, which indicates that the small particle size phase (Ni) begins to melt, confirming that the liquid phase sintering mode can be achieved by laser sintering. When the mass fraction of Ni nanoparticles in Ni-SrTiO3 mixed nanoparticles is 20wt% and 30wt%, the proportion of small particle size phase (Ni) increases, and the liquid phase sintering state is reached at 35W, which indicates that as the proportion of Ni increases, the absorbance of the mixed nanoparticles increases, and at the same laser power, a higher sintering temperature can be formed, which promotes the formation of liquid phase sintering at a lower power.
[0059] In summary, thin film laser liquid phase sintering can be achieved under high Ni ratio and high laser power.
[0060] like Figure 2 As shown, when the mass fraction of Ni nanoparticles in the Ni-SrTiO3 mixed nanoparticles is 20wt%, and the laser power is P=30W (no molten phase is formed, it is a solid phase sintering state), the zT value of the Ni-SrTiO3 film gradually increases with the increase of temperature, from 0.045 at 300K to 0.54 at 800K, and the growth rate gradually decreases with the increase of ambient temperature. When the mass fraction of Ni nanoparticles in the Ni-SrTiO3 mixed nanoparticles is 20wt%, and the laser power is P=40W (molten phase is formed, it is a liquid phase sintering state), the zT value of the Ni-SrTiO3 film gradually increases with the increase of temperature, from 0.12 at 300K to 0.95 at 800K, and the growth rate gradually increases with the increase of ambient temperature.
[0061] In summary, compared with the traditional solid-phase sintered film, the comprehensive thermoelectric performance of the laser liquid-phase sintered film of the present invention is improved.
[0062] The present invention discloses a method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the method. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The products of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the products described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
Claims
1. A thermoelectric film made of mixed nanoparticles based on laser liquid phase sintering, It is characterized in that include: Base layer and three Ni-SrTiO layers with different mass fractions deposited on the base layer by inkjet printing 3 Hybrid nanoparticle ink; Three parts Ni-SrTiO 3 The mixed nanoparticle ink is composed of Ni nanoparticles and SrTiO 3 The nanoparticles are mixed in different mass ratios; the Ni nanoparticles and SrTiO 3 The mass ratios of the nanoparticles were 3:7, 2:8 and 1:9 respectively; three Ni-SrTiO 3 The mass fraction of the mixed nanoparticle ink is 12-15%.
2. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles, It is characterized in that The following steps are involved: (1) Preparation of Ni-SrTiO 3 Hybrid nanoparticle ink; (2)Ni-SrTiO 3 Inkjet printing deposition of hybrid nanoparticle films; (3)Ni-SrTiO 3 Laser sintering of mixed nanoparticle films: Ni-SrTiO 3 The substrate temperature after the mixed nanoparticle film inkjet printing deposition is controlled at 50-52°C. After adjusting the laser spot diameter, setting the laser scanning path, and adjusting the laser sintering parameters in sequence, a single laser sintering of the deposition line is started to promote grain growth or partial melting.
3. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 2, It is characterized in that The specific process of step (1) is: Ni nanoparticles and SrTiO 3 The nanoparticles were mixed evenly in different mass ratios to form three Ni-SrTiO 3 The nanoparticles are mixed and dispersed in organic solvents respectively, and then ultrasonically dispersed and filtered to prepare three Ni-SrTiO 3 Hybrid nanoparticle ink.
4. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 3, It is characterized in that The Ni nanoparticles and SrTiO 3 The mass ratios of the nanoparticles are 3:7, 2:8 and 1:9, respectively.
5. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 3, It is characterized in that The particle size of the Ni nanoparticles is 30-40 nm; the SrTiO 3 The particle size of nanoparticles is 100-150nm.
6. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 3, It is characterized in that The power of the ultrasonic dispersion is 120-200W and the temperature is 10-15°C.
7. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 2, It is characterized in that The specific process of step (2) is: select Al 2 O 3 The ceramic substrate was ultrasonically cleaned and dried for later use; three Ni-SrTiO 3 Droplet sequence corresponding to mixed nanoparticle ink; control Al 2 O 3 After the temperature of the ceramic substrate reaches 130-140℃, set the printing parameters and pattern, and print three Ni-SrTiO 3 Droplet sequence corresponding to mixed nanoparticle ink.
8. A method for manufacturing thermoelectric thin films based on laser liquid phase sintering of mixed nanoparticles according to claim 7, It is characterized in that Preparation of three Ni-SrTiO 3 When the droplet sequence corresponding to the mixed nanoparticle ink is used, the inkjet printing waveform is 60-70V positive pressure, 75-85V negative pressure, 0-5V reference voltage, 5-8ms positive pressure rise time, 30-40ms positive pressure duration, 10-20ms positive pressure fall time, 40-50ms negative pressure duration, and 5-8ms negative pressure rise time.
9. The method for manufacturing thermoelectric thin film based on laser liquid phase sintering of mixed nanoparticles according to claim 7, It is characterized in that The printing parameters are: horizontal printing dot spacing 0.025-0.03mm, vertical printing dot spacing 0.03-0.035mm, and printing speed 15-17mm / s.
10. The method for manufacturing thermoelectric thin film based on laser liquid phase sintering of mixed nanoparticles according to claim 2, It is characterized in that The laser spot diameter is 0.3-0.31 mm; the laser is a Nd-YAG laser with a wavelength of 1064 nm; the laser scanning path is a zigzag mode; the laser sintering parameters are: power 20-40 W, scanning speed 100-120 mm / s, and scanning line spacing 0.01-0.015 mm.