Method for improving thermoelectric property of thin film based on printing and stacking of special-shaped nanoparticles

Through the special-shaped nanoparticle printing stacking technology, the problem of difficulty and high cost of improving the thermoelectric characteristics of thin films is solved, and efficient and simple improvement of the thermoelectric characteristics of thin films is achieved. The Sybeck coefficient is increased by 25%-45%, and the film structure is optimized.

CN118927844AInactive Publication Date: 2024-11-12BEIHANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411012210.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing methods for improving thermoelectric properties of thin films have problems such as difficult, complicated processes and limited performance improvement, especially due to material selection and characteristic optimization, which lead to high costs and limited performance improvement.

Method used

The special-shaped nanoparticle printing stacking technology is adopted to configure functional inks of nanoparticles in different shapes, and the special-shaped nanoparticle printing stacking film is formed on the substrate using inkjet printing technology, and annealing is performed to optimize the film structure to improve the thermoelectric characteristics.

Benefits of technology

The film deposition without cracks, firmly adhered and highly ordered is achieved, which significantly improves the Sybeck coefficient of the film thermocouple, increases by 25%-45%, and simplifies the operation process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927844A_ABST
    Figure CN118927844A_ABST
Patent Text Reader

Abstract

A method for improving thermoelectric properties of a thin film based on special-shaped nanoparticle printing and stacking relates to the field of thin film manufacturing, and comprises the following steps: preparing nanoparticle functional ink with different shapes; designing BMP images in different printing stacking forms; controlling the temperature of the substrate; the ink is placed in different printing channels of an ink-jet printing system, and piezoelectric ceramic waveforms are adjusted to generate stable ink droplets; printing parameters are set, and according to a preset BMP image, different printing channels are sequentially used for deposition on the substrate to form a special-shaped nanoparticle printing stacked film; and placing the special-shaped nanoparticle printing stacked thin film in a high-temperature tubular annealing furnace for annealing treatment to obtain the stacked thin film thermocouple. The stacking structure and the mixing proportion of the special-shaped nanoparticles are controlled through the ink-jet printing technology, the film quality is improved, film deposition without cracks and firm adhesion is achieved, the film structure is optimized, the thermoelectric property of the film thermocouple is greatly enhanced, and the Seebeck coefficient is increased by 25%-45%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thin film manufacturing, and in particular relates to a method for improving the thermoelectric properties of a thin film based on printing and stacking of special-shaped nanoparticles. Background Art

[0002] Inkjet printing technology is an efficient, flexible, non-contact on-demand manufacturing technology. It has the advantages of simplifying the process, accelerating manufacturing and reducing costs in the preparation of thin-film thermocouples. Inkjet printing technology uses ultrasound to evenly disperse nanoparticles in an organic solvent to prepare functional inks, and generates a sequence of ink droplets through a nozzle to deposit on the target surface to form a continuous line. After heating and evaporating the solvent, a thin-film thermocouple that can accurately measure temperature in real time is obtained through annealing. The thermoelectric properties of thin-film thermocouples are mainly subject to material properties, film quality and structural design. Improving the thermoelectric properties of thin-film thermocouples is crucial to increasing temperature measurement sensitivity, accelerating response speed and improving anti-interference ability. Therefore, in recent years, many studies have adopted a variety of methods to improve the thermoelectric properties of thin-film thermocouples.

[0003] In the existing technology, the main means to improve the thermoelectric properties of thin films are concentrated on material selection and property optimization, but this method has problems such as complex process, limited space for performance improvement and high cost. Specifically, the process of preparing high-quality thin-film thermoelectric materials in the existing technology is very complicated, requiring advanced synthesis technology and multi-step optimization, including doping, annealing treatment and interface engineering, etc. Each step requires precise control and repeated experiments. In addition, due to the inherent physical trade-off relationship between the Seebeck coefficient, electrical conductivity and thermal conductivity, the performance improvement of a single material is restricted. Often when enhancing a certain performance, it may inevitably sacrifice other performance. The main reasons for the high cost are the use of rare and high-purity materials, expensive advanced equipment and high energy consumption, high-precision measurement and technical personnel expenses.

[0004] Therefore, how to enhance the thermoelectric properties of thin films by improving film quality and optimizing film structure is a key technical path that urgently needs to be developed. Summary of the invention

[0005] The purpose of the present invention is to provide a method for improving the thermoelectric properties of thin films based on printing and stacking of special-shaped nanoparticles, so as to solve the problems of high difficulty, complex process and limited space for performance improvement in existing methods for improving the thermoelectric properties of thin films.

[0006] The present invention discloses a method for improving the thermoelectric properties of a thin film based on printing and stacking of special-shaped nanoparticles, aiming to improve the thermoelectric properties of the thin film by improving the quality of the thin film and optimizing the structure of the thin film.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0008] The present invention provides a method for improving the thermoelectric properties of thin films based on printing and stacking of special-shaped nanoparticles, which specifically comprises the following steps:

[0009] Step 1: Prepare nanoparticle functional inks of different shapes;

[0010] Step 2: Cleaning and debugging of substrate and inkjet printing system;

[0011] Step 3: Inkjet printing stacking;

[0012] Design BMP images with different printing stacking forms; place the cleaned substrate on a heating platform; place functional inks of nanoparticles of different shapes in different printing channels of the inkjet printing system, and adjust the piezoelectric ceramic waveform to generate stable ink droplets; set printing parameters and use different printing channels in sequence to deposit on the substrate according to the preset BMP image to form a heterogeneous nanoparticle printing stacking film;

[0013] Step 4: annealing the film;

[0014] The prepared irregular nanoparticle printed stacked film is placed in a high-temperature tubular annealing furnace for annealing to obtain a stacked film thermocouple.

[0015] Wherein, in step 1, the average particle size of the nanoparticles is preferably 30nm-50nm; the shape of the nanoparticles is preferably spherical, square, sheet or rod-shaped.

[0016] Wherein, in step 1, the mass fraction of the nanoparticle functional ink is preferably 5%-20%.

[0017] Wherein, in step 2, the nozzle diameter of the inkjet printing system is preferably 40 μm-100 μm.

[0018] Among them, in step three, the printing stacking form is preferably horizontal stacking, vertical stacking, five-point stacking or X-shaped stacking.

[0019] Among them, in step three, the piezoelectric ceramic waveform is preferably: positive voltage 50V-70V, negative voltage -80V--110V, reference voltage 0V-15V, positive voltage rise time 5ms-15ms, positive voltage duration 15ms-40ms, positive pressure fall time 20ms-40ms, negative pressure duration 20ms-40ms, negative pressure rise time 5ms-15ms.

[0020] Among them, in step three, the printing parameters are preferably set to: speed 1mm / s-20mm / s, dot spacing 0.02mm-0.12mm, substrate temperature 140℃-160℃.

[0021] Among them, in step three, after each nanoparticle functional ink is printed and the solvent is evaporated, the next nanoparticle functional ink is printed, and each nanoparticle functional ink needs to be repositioned before printing.

[0022] When repositioning, it is preferred to use an industrial camera with a top-down perspective to calibrate and position the printing start point of the last deposited film.

[0023] Among them, in step 4, the annealing temperature is preferably 800°C-1200°C, and the annealing time is preferably 30min-180min.

[0024] The beneficial effects of the present invention are:

[0025] The present invention proposes a method for improving the thermoelectric properties of thin films based on the printing and stacking of shaped nanoparticles. The stacking structure and mixing ratio of shaped nanoparticles are controlled by inkjet printing technology, thereby improving the quality of the film, achieving crack-free and firmly attached film deposition, and obtaining a crack-free, firmly attached and highly ordered stacked film of shaped nanoparticles printed. In addition, the present invention also optimizes the film structure and greatly enhances the thermoelectric properties of the thin film thermocouple. Test results show that the Seebeck coefficient of the stacked thin film thermocouple prepared by the present invention is increased by 25%-45%. The present invention is not only efficient, but also simple to operate, easy to implement, and highly controllable, providing a new technical path for improving the thermoelectric properties of thin film thermocouples. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the printing stacking form of stacked films printed with special-shaped nanoparticles.

[0027] Figure 2 Print the morphology of stacked films for shaped nanoparticles.

[0028] Figure 3 SEM characterization image of the stacked film printed with special-shaped nanoparticles after thermal annealing.

[0029] Figure 4 The thermoelectric potential output curves of spherical, square, five-point stacked and X-stacked thin film thermocouples. DETAILED DESCRIPTION

[0030] In order to further understand the present invention, preferred embodiments of the present invention are described below. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0031] The present invention provides a method for improving the thermoelectric properties of thin films based on printing and stacking of special-shaped nanoparticles, and the specific implementation steps are as follows:

[0032] Step 1: Prepare nanoparticle functional inks of different shapes;

[0033] The present invention uses ultrasonic technology to evenly disperse nanoparticles of different shapes into a mixed organic solvent composed of ethylene glycol and isopropanol, and obtains functional inks of nanoparticles of various shapes after filtering through a filter membrane.

[0034] The average particle size of the nanoparticles used is preferably 30nm-50nm; the shape of the nanoparticles used is preferably spherical, square, sheet or rod, etc., but not limited thereto.

[0035] The mass fraction of the obtained nanoparticle functional ink is preferably 5%-20%, and more preferably 10%.

[0036] Wherein, in the mixed organic solvent, the mass ratio of ethylene glycol to isopropanol is preferably 50%-100%, more preferably 50%.

[0037] Among them, in the ultrasonic technology, the ultrasonic dispersion parameters set are preferably: dispersion power 180W-220W, dispersion time 2h-4h, water bath temperature 5℃-15℃;

[0038] Among them, when filtering with a membrane, a 0.45μm PTFE filter membrane is used to filter the ink.

[0039] In the process of configuring functional inks of nanoparticles of different shapes, no sedimentation phenomenon was observed after the ink was left to stand for 24 hours; the ink has excellent stability, printability and rheological properties, provides a stable ink drop sequence for the inkjet printing stacking process, and ensures the smoothness and film-forming quality of the inkjet printing stacking.

[0040] Step 2: Experimental pretreatment, including substrate cleaning and inkjet printing system cleaning and debugging;

[0041] The cleaning method of the substrate is as follows: immersing the substrate in a cleaning device filled with anhydrous ethanol, performing ultrasonic cleaning for 10 minutes, and drying with a hot air gun after cleaning;

[0042] The cleaning and debugging method of the inkjet printing system is as follows: put anhydrous ethanol into the ink storage bottle, use positive and negative pressure to repeatedly flush the printing channel and nozzle to wash away residual ink and impurities. After cleaning, use anhydrous ethanol for debugging to check whether the system can generate stable ink droplets.

[0043] The nozzle diameter of the inkjet printing system is preferably 40 μm-100 μm, more preferably 80 μm.

[0044] It should be noted that the preprocessing steps of the experiment must strictly follow the regulations to ensure that the continuity of the inkjet printing experiment process and the accuracy of the experimental results are not affected.

[0045] Step 3: Inkjet printing stacking;

[0046] Design BMP images with different printing stacking forms; place the cleaned substrate on a heating platform; place nanoparticle functional inks of different shapes in different printing channels of the inkjet printing system, and adjust the piezoelectric ceramic waveform to generate stable ink droplets; set printing parameters and use different printing channels in sequence to deposit on the substrate according to the preset BMP image to form a special-shaped nanoparticle printed stacked film; after each nanoparticle functional ink is printed and the solvent is evaporated, print the next nanoparticle functional ink, and each nanoparticle functional ink needs to be repositioned before printing. When repositioning, it is preferred to use an industrial camera with a top-down perspective to calibrate and position the printing starting point of the last deposited film.

[0047] Among them, the printing stacking form is preferably horizontal stacking, vertical stacking, five-point stacking or X-type stacking.

[0048] Among them, the piezoelectric ceramic waveform is preferably: positive voltage 50V-70V, negative voltage -80V--110V, reference voltage 0V-15V, positive voltage rise time 5ms-15ms, positive voltage duration 15ms-40ms, positive pressure fall time 20ms-40ms, negative pressure duration 20ms-40ms, negative pressure rise time 5ms-15ms.

[0049] The printing parameters are preferably set as follows: speed 1 mm / s-20 mm / s, dot spacing 0.02 mm-0.12 mm, substrate temperature 140°C-160°C.

[0050] The purpose of the present invention using different printing stacking forms is to achieve stacking and mixing of nanoparticles of different shapes in different structures and proportions, thereby obtaining a film with a diversified stacking structure. This method not only optimizes the quality of the film and ensures that the film is crack-free and firmly attached, but also improves the interface bonding performance between the new ink and the original film through the secondary wetting of the deposited film by the newly sprayed nanoparticle ink of other shapes. In addition, the secondary wetting can also adjust the microstructure of the film, such as the size and distribution of the grains, thereby further enhancing the performance of the film.

[0051] In addition, the present invention can control the ink drop size and printing strategy by adjusting the piezoelectric ceramic waveform and printing parameters, thereby expanding the diversity and flexibility of the experiment.

[0052] Step 4: annealing the film;

[0053] The prepared irregular nanoparticle printed stacked film is placed in a high-temperature tubular annealing furnace for annealing to obtain a stacked film thermocouple.

[0054] The annealing parameters are set as follows: the annealing temperature is preferably 800° C.-1200° C., and the annealing time is preferably 30 min-180 min.

[0055] The present invention transforms the original deposited film into a thermocouple circuit with conductivity through annealing treatment; in this process, the density of the film is improved, the grain size is increased, and the porosity is reduced.

[0056] In summary, the method for improving the thermoelectric properties of thin films based on the printing and stacking of shaped nanoparticles of the present invention can significantly improve the thermoelectric properties of thin film thermocouples based on the printing and stacking of shaped nanoparticles, and the Seebeck coefficient thereof is increased by 25%-45%.

[0057] The present invention proposes the concept of printing stacking for the first time. Different from the traditional method of improving the thermoelectric properties of thin film thermocouples by selecting high-performance materials or improving the annealing process, printing stacking aims to achieve printing and stacking films of special-shaped nanoparticles by adjusting printing parameters and formulating printing strategies, thereby effectively improving the film quality and optimizing the structure, thereby improving its thermoelectric properties.

[0058] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0059] The terms used in the present invention generally have the meanings commonly understood by those of ordinary skill in the art, unless otherwise specified. In order to enable those of ordinary skill in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with embodiments.

[0060] In the following examples, various processes and methods not described in detail are conventional methods known in the art. Unless otherwise specified, the materials, reagents, devices, instruments, equipment, etc. used in the following examples can be obtained from commercial sources.

[0061] Example 1

[0062] A method for improving the thermoelectric properties of thin films based on printing and stacking of special-shaped nanoparticles, the specific implementation steps are as follows:

[0063] 1. Add spherical and square ITO nanoparticles at a mass fraction of 10% into a mixed organic solvent consisting of ethylene glycol and isopropanol (mass ratio of 50%), and disperse them ultrasonically to obtain two uniform and stable inks, namely, spherical ITO nanoparticle functional ink and square ITO nanoparticle functional ink; clean the ceramic substrate, and clean and debug the inkjet printing equipment;

[0064] 2. Design BMP images with different printing stacking forms, including horizontal stacking, vertical stacking, five-point stacking and X-shaped stacking; place the cleaned substrate on a heating platform; place two shapes of ITO nanoparticle functional inks in different printing channels of the inkjet printing system, and adjust the piezoelectric ceramic waveform to generate a stable ink drop sequence: positive pressure 60V, negative pressure -90V, reference voltage 5V, positive pressure rise time 8ms, positive pressure duration 25ms, positive pressure drop time 28ms, negative pressure duration 28ms, negative pressure rise time 10ms; set printing parameters: speed 5mm / s, dot spacing 0.06mm, substrate temperature 150℃; and according to the preset BMP image, first print the spherical ITO nanoparticle functional ink, after the solvent is evaporated to form a deposited film, reposition the printing starting point, print the square ITO nanoparticle functional ink on the surface of the original spherical film, and obtain the irregular nanoparticle printed stacked film after the solvent is evaporated;

[0065] 3. Place the prepared stacked thin film printed with shaped nanoparticles in a high-temperature tubular annealing furnace for annealing to obtain a stacked thin film thermocouple, wherein the annealing temperature is 1200° C. and the annealing time is 60 min.

[0066] 4. Thermoelectric characteristics test;

[0067] After annealing, the stacked thin film thermocouples were wired and then placed in a tubular resistance furnace for thermoelectric properties testing. The thermoelectric properties testing program was set to a heating rate of 10°C / min, from room temperature to 1100°C, and then naturally cooled after keeping warm for 1 hour.

[0068] This embodiment uses spherical ITO nanoparticle functional ink and square ITO nanoparticle functional ink to perform printing and stacking experiments on the surface of a ceramic substrate, and obtains high-quality deposited stacked films in various stacking forms. Among them, the printing and stacking forms of the special-shaped nanoparticle printed stacked films are as follows: Figure 1 As shown, there are four printing stacking forms, namely horizontal stacking, vertical stacking, five-point stacking and X-type stacking.

[0069] The present invention uses a digital microscope to observe the morphology of the stacked thin film printed with irregular nanoparticles. The results are as follows: Figure 2 shown. Figure 2The deposited films prepared by four preset printing stacking methods and the sintered films obtained by sintering at 1200℃ for 60min are shown. Figure 2 It can be clearly seen that the particles on the surface of the film are arranged in an orderly manner. At the same time, the film is intact without cracks and is firmly attached to the substrate.

[0070] The present invention can obtain a crack-free, firmly attached and highly ordered irregular nanoparticle printed stacked film.

[0071] The present invention uses SEM to observe the crystal phase changes of the stacked thin films printed with irregular nanoparticles after thermal annealing. The results are as follows Figure 3 shown. Figure 3 The SEM images of the spherical and square single-component nanoparticle films and the stacked films obtained by printing the two nanoparticles in a horizontal stack are shown in the figure. Figure 3 It can be seen that the two single-component films have obvious pores and large porosity, while the film surface printed by stacking has no obvious pores, a denser structure, and a better sintering effect.

[0072] The present invention obtains the thermoelectric potential output of spherical, square, five-point stacked and X-type stacked thin film thermocouples through thermoelectric property testing. The results are as follows: Figure 4 shown. Figure 4 The thermoelectric potential output curves of spherical, square, five-point stacked and X-type stacked thin film thermocouples tested at 1100°C. Figure 4 It can be observed that the thermoelectric potential output of the two stacked thin film thermocouples is significantly higher than that of the two single-component thin films. After calculation, the average Seebeck coefficient of the stacked thin film thermocouple is 38.07% higher than that of the single-component thin film, indicating that the stacking structure significantly improves the thermoelectric performance of the film. It is confirmed that the method of printing and stacking of special-shaped nanoparticles can effectively improve the thermoelectric properties of thin films.

[0073] In summary, the present invention adopts a combination of functional inks of nanoparticles of different shapes and successfully prepares printed stacked thin film thermocouples on the surface of the substrate. The thermoelectric properties test results show that the Seebeck coefficient of the thin film thermocouple can be effectively improved by the method of printing and stacking of special-shaped nanoparticles. The Seebeck coefficient is increased by 25%-45%, which verifies the feasibility of the printing and stacking technology and its positive effect on improving the thermoelectric properties of thin film thermocouples.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein, but these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving the thermoelectric properties of thin films based on printing and stacking of special-shaped nanoparticles, characterized in that: The following steps are involved: Step 1: Prepare nanoparticle functional inks of different shapes; Step 2: Cleaning and debugging of substrate and inkjet printing system; Step 3: Inkjet printing stacking; Design BMP images with different printing stacking forms; place the cleaned substrate on a heating platform; place functional inks of nanoparticles of different shapes in different printing channels of the inkjet printing system, and adjust the piezoelectric ceramic waveform to generate stable ink droplets; Setting printing parameters and using different printing channels in sequence to deposit heterogeneous nanoparticles on the substrate according to the preset BMP image to form a printed stacked film; Step 4: annealing the film; The prepared irregular nanoparticle printed stacked film is placed in a high-temperature tubular annealing furnace for annealing to obtain a stacked film thermocouple.

2. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step 1, the average particle size of the nanoparticles is 30nm-50nm; the shape of the nanoparticles is spherical, square, flake or rod-shaped.

3. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step 1, the mass fraction of the nanoparticle functional ink is 5%-20%.

4. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step 2, the nozzle diameter of the inkjet printing system is 40 μm-100 μm.

5. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step three, the printing stacking form is horizontal stacking, vertical stacking, five-point stacking or X-shaped stacking.

6. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step three, the piezoelectric ceramic waveform is: positive voltage 50V-70V, negative voltage -80V--110V, reference voltage 0V-15V, positive voltage rise time 5ms-15ms, positive voltage duration 15ms-40ms, positive pressure drop time 20ms-40ms, negative pressure duration 20ms-40ms, negative pressure rise time 5ms-15ms.

7. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step three, the printing parameters are set as: speed 1 mm / s-20 mm / s, dot spacing 0.02 mm-0.12 mm, substrate temperature 140°C-160°C.

8. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step three, after each nanoparticle functional ink is printed and the solvent is evaporated, the next nanoparticle functional ink is printed, and each nanoparticle functional ink needs to be repositioned before printing.

9. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 8, characterized in that: During repositioning, an industrial camera with a top-down perspective is used to calibrate the printing starting point of the last deposited film.

10. The method for improving thin film thermoelectric properties based on printing and stacking of special-shaped nanoparticles according to claim 1, characterized in that: In step 4, the annealing temperature is 800° C.-1200° C., and the annealing time is 30 min-180 min.

Citation Information

Patent Citations

  • Method for fabricating thermoelectric powder having a bimodal size distribution

    KR1020130074788A

  • Method for producing particles, method for coating with particles or slurry, secondary battery or method for producing secondary battery, all-solid-state battery or method for producing all-solid-state battery, LED or method for producing LED, and phosphor sheet or method for producing phosphor sheet