Method for producing bonded photocatalyst, and bonded photocatalyst
By introducing a solid medium between the hydrogen-producing photocatalyst and the oxygen-producing photocatalyst and increasing its coating rate, an efficient bonding photocatalyst is formed, and a problem of low catalytic activity in the prior art is solved, and an efficient water decomposition reaction is achieved.
Patent Information
- Application Number
- CN202380024759.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-12
AI Technical Summary
The existing hydrogen-producing photocatalysts and oxygen-producing photocatalysts have low catalytic activity in water decomposition reactions, and the selection range for redox media is narrow, and the electron-receptive efficiency is low, which affects the water decomposition efficiency.
By introducing a solid medium between the hydrogen-producing photocatalyst and the oxygen-producing photocatalyst, the organic carboxylic acid compound is bonded with the solid medium or its precursor through photoelectrodeposition, impregnation and loading method or precipitation method, the solid medium is improved by increasing the production of solid medium by using the organic carboxylic acid compound and the solid medium or its precursor by photoelectrodeposition, impregnation and loading method. The coverage ratio of the electron-capture surface area of the oxygen photocatalyst is more than 40%, forming an efficient bonding photocatalyst.
It significantly improves the catalytic activity and efficiency of the water decomposition reaction, can efficiently decompose water into oxygen and hydrogen, and improves the yield of the water decomposition reaction.
Smart Images

Figure BDA0005020242290000391 
Figure HDA0005020242310000011 
Figure HDA0005020242310000012
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a conjugated photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst, a conjugated photocatalyst, an oxygen-producing photocatalyst conjugated with the solid medium, a method for manufacturing the oxygen-producing photocatalyst conjugated with the solid medium, a photocatalyst complex, an application of the conjugated photocatalyst, and a method for manufacturing hydrogen. Background Art
[0002] In recent years, the technology of using photocatalysts and sunlight to decompose water to produce hydrogen and oxygen has attracted attention. When decomposing water using photocatalysts, it is preferred to use a photocatalyst that catalyzes both the reduction reaction of water (reduction reaction of protons) and the oxidation reaction of water, but the types of such photocatalysts are limited, and there is a tendency for the water decomposition activity to be low.
[0003] Therefore, a method of efficiently decomposing water by using a photocatalyst that catalyzes a reduction reaction of water (hydrogen-generating photocatalyst) and a photocatalyst that catalyzes an oxidation reaction of water (oxygen-generating photocatalyst) in combination has been studied.
[0004] For example, a system that uses a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst to irradiate visible light to decompose water to produce both hydrogen and oxygen is called a Z-Scheme. In the Z-Scheme, for example, a photocatalyst that combines an oxygen-producing photocatalyst that decomposes water using visible light to produce oxygen, a hydrogen-producing photocatalyst that decomposes water using visible light to produce hydrogen, and a redox medium is used. Moreover, the Z-Scheme using this photocatalyst repeatedly performs the following cycle, that is, the electrons generated by the oxygen-producing photocatalyst that do not participate in the reduction of water reduce the redox medium, and the reduced redox medium is oxidized by the holes generated by the hydrogen-producing photocatalyst that do not participate in the oxidation of water to restore the cycle of the redox medium before reduction, thereby being able to completely decompose water (hydrogen: oxygen = 2:1 (stoichiometric ratio)).
[0005] However, in order for the Z scheme using the above hydrogen-generating photocatalyst and oxygen-generating photocatalyst to exert a catalytic effect, a redox mediator (such as Fe 3+ / Fe 2+ or I - / IO 3 - ), and there are problems such as low electron transfer efficiency of the redox medium and low water decomposition activity. In addition, it is necessary to select an appropriate photocatalyst for the redox potential of the redox medium, and there is also a problem of a narrow range of photocatalyst selection.
[0006] On the other hand, as a junction-type photocatalyst that does not use a redox medium, for example, a photocatalyst layer is proposed in Patent Document 1, which comprises: a first photocatalyst particle of a visible light responsive type for hydrogen production, a second photocatalyst particle of a visible light responsive type for oxygen production, and conductive particles, wherein the conductive particles are arranged between the first photocatalyst particle and the second photocatalyst particle, have a Fermi level at a position more negative than the electronic energy level at the upper end of the valence band of the first photocatalyst particle and more positive than the electronic energy level at the lower end of the conduction band of the second photocatalyst particle, and are capable of storing electrons and holes, and the conductive particles are configured in a manner connected to the first photocatalyst particle and the second photocatalyst particle.
[0007] In addition, Non-Patent Document 1 proposes that ZnRh 2 O 4 / Au / BiVO 4 The formed hierarchical structure of the Z-scheme photocatalyst.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Publication No. 2017-124394
[0011] Non-patent literature
[0012] Non-patent literature 1: Toshihiro Takashima et al., J. Mater. Chem. A, 2019, 7, 10372-10378 Summary of the invention
[0013] Problems to be solved by the present invention
[0014] A junction-type photocatalyst in which a hydrogen-generating photocatalyst and an oxygen-generating photocatalyst are joined via a metal or a metal oxide has a very simple structure and exhibits high catalytic activity in a decomposition reaction of water or the like under visible light irradiation, but further improvement of the catalytic activity is required.
[0015] The present invention has been made in view of the above-mentioned situation, and provides a junction-type photocatalyst having a higher catalytic activity than a conventional junction-type photocatalyst.
[0016] Technical means of solving problems
[0017] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by the following junction type photocatalyst and method for producing the junction type photocatalyst.
[0018] That is, the present invention relates to the following 1. to 7.
[0019] 1. A method for producing a junction type photocatalyst, which is a method for producing a junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst,
[0020] The method for producing the junction type photocatalyst comprises the following steps 1:
[0021] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation supporting method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0022] 2. A junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst,
[0023] The coverage rate of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more.
[0024] 3. A method for producing an oxygen-generating photocatalyst bonded with a solid medium, comprising the step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0025] 4. An oxygen-generating photocatalyst joined with a solid medium, wherein the coverage of the solid medium with respect to the electron-capturing surface area of the oxygen-generating photocatalyst is 40% or more.
[0026] 5. A photocatalyst composite comprising the above-mentioned junction-type photocatalyst on a substrate.
[0027] 6. Use of the above-mentioned conjugated photocatalyst as a photocatalyst for water decomposition or a photocatalyst for organic matter decomposition.
[0028] 7. A method for producing hydrogen, comprising irradiating the junction-type photocatalyst or the photocatalyst complex with light in the presence of water or alcohol.
[0029] Effects of the Invention
[0030] The junction type photocatalyst of the present invention increases the coverage of the solid medium with respect to the electron-capturing surface area of the oxygen-generating photocatalyst, thereby improving the catalytic activity and being able to decompose water into oxygen and hydrogen at a high water-splitting reaction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The Au-BiVO of Example 1 4 SEM image of .
[0032] Figure 2 This is a SEM image of the junction-type photocatalyst of Example 1.
[0033] Figure 3 This is the volume particle size distribution of the conjugated photocatalyst (conjugated particles) of Example 1, etc.
[0034] Figure 4 The Ru-supported SrTiO 3 and Au-BiVO 4 Volume particle size distribution of mixed samples, etc. DETAILED DESCRIPTION
[0035] Hereinafter, the present invention will be described in detail.
[0036] <Conjugation-type photocatalyst>
[0037] The junction type photocatalyst of the present invention has a solid medium between the hydrogen generation photocatalyst and the oxygen generation photocatalyst. From the viewpoint of improving catalytic activity, the coverage of the solid medium with respect to the electron capture surface area of the oxygen generation photocatalyst of the junction type photocatalyst of the present invention is 40% or more.
[0038] Specifically, the oxygen-generating photocatalyst is directly or indirectly bonded to a portion of the solid medium, the hydrogen-generating photocatalyst is directly or indirectly bonded to another portion of the solid medium, and the hydrogen-generating photocatalyst and the oxygen-generating photocatalyst are bonded at least via the solid medium.
[0039] In addition, the above-mentioned solid medium and the above-mentioned hydrogen-producing photocatalyst are preferably joined via an ionic polymer, and the above-mentioned solid medium preferably has an ionic group, and the above-mentioned solid medium and the above-mentioned hydrogen-producing photocatalyst are joined via the ionic group possessed by the above-mentioned solid medium (preferably the ionic group introduced into the above-mentioned solid medium) and an ionic polymer having a charge opposite to that of the above-mentioned ionic group.
[0040] In one embodiment of the conjugated photocatalyst of the present invention, the solid medium has an ionic group, the hydrogen-generating photocatalyst has the ionic polymer having a charge opposite to that of the ionic group, and the solid medium is conjugated to the hydrogen-generating photocatalyst through ionic bonds between the ionic group and the ionic polymer.
[0041] In addition, in one embodiment of the conjugated photocatalyst of the present invention, the solid medium has an ionic group, the hydrogen-producing photocatalyst has an ionic polymer A, and the hydrogen-producing photocatalyst also has an ionic polymer B with a charge opposite to that of the ionic group through the ionic polymer A, and the solid medium is conjugated to the hydrogen-producing photocatalyst through the ionic bond between the ionic group and the ionic polymer B.
[0042] In addition, in one embodiment of the conjugated photocatalyst of the present invention, the solid medium has an ionic group, and the solid medium also has an ionic polymer B having a charge opposite to the charge of the above-mentioned ionic group through the above-mentioned ionic group, and the hydrogen-producing photocatalyst has an ionic polymer A. The above-mentioned solid medium is conjugated to the above-mentioned hydrogen-producing photocatalyst through the ionic bond between the above-mentioned ionic polymer B possessed by the above-mentioned solid medium and the above-mentioned ionic polymer A possessed by the above-mentioned hydrogen-producing photocatalyst.
[0043] When the ionic groups of the solid medium are anionic groups, the ionic polymer A is an anionic polymer and the ionic polymer B is a cationic polymer. When the ionic groups of the solid medium are cationic groups, the ionic polymer A is a cationic polymer and the ionic polymer B is an anionic polymer.
[0044] In the present invention, "joining" refers to the state in which the oxygen-generating photocatalyst and the hydrogen-generating photocatalyst are integrated to the extent that they are not separated during the photocatalytic reaction. In addition, in the present invention, "electron capture surface" refers to the exposed crystal surface in various structures of the oxygen-generating photocatalyst where excited electrons are most likely to gather.
[0045] The hydrogen-generating photocatalyst is not particularly limited, and examples thereof include TiO 2 、SrTiO 3 ,La 2 Ti 2 O 7 、SnNb 2 O 6 , and metal oxides such as compounds doped with one or more metals such as Cr, Sb, Ta, Ir, and La; LaTiO 2 N、BaTaO 2 N、BaNbO 2 N、TaON、Ta 3 N 5 , and Ge 3 N 4 Metal oxynitrides or metal nitrides; CuGaS 2 、CuInS 2 、Cu(Ga、In)S 2 、CuGaSe 2 、CuInSe 2 、Cu(Ga、In)Se 2 , Cu 2 ZnSnS 4 (CZTS), and Cu 2 ZnSn(S,Se) 4Metal sulfides, metal selenides or metal sulfide selenides; La 5 Ti 2 QUR 5 O 7 ,La 5 Ti 2 S 5 O 7 ,La 5 Ti 2 CuSe 5 O 7 , and La 5 Ti 2 G E 5 O 7 Such metal oxide sulfides or metal oxide selenides, etc. These can be used alone or in combination of two or more. Among these, from the viewpoint of improving catalytic activity, preferably one or more selected from metal oxides, more preferably one or more selected from transition metal oxides, further preferably one or more selected from oxides of elements belonging to Group 4 of the periodic table, and further preferably SrTiO 3 .
[0046] The oxygen-generating photocatalyst is not particularly limited, and examples thereof include BiVO 4 、TiO 2 , WO 3 、SrTiO 3 、Ag 3 PO 4 、SnNb 2 O 6 、Bi 2 WO 6 , Fe 2 TiO 5 , Fe 2 O 3 、Bi 2 MoO 6 , and metal oxides such as compounds doped with one or more metals such as Cr, Ni, Sb, Nb, Th, Mo, and W; Ta 3 N 5 , and Ge 3 N 4 Metal nitrides such as LaTiO 2 N、BaTaO 2 N、BaNbO 2N, and metal oxynitrides such as TaON, etc. These can be used alone or in combination. Among these, from the viewpoint of improving catalytic activity, preferably one or more selected from metal oxides, more preferably one or more selected from oxides of transition metals, further preferably one or more selected from oxides of one or more elements belonging to Groups 4 and 5 of the periodic table, more preferably BiVO 4 .
[0047] The hydrogen-generating photocatalyst and the oxygen-generating photocatalyst preferably have a promoter on the surface, thereby promoting the reduction and oxidation reactions of water and the like, and improving the generation efficiency of hydrogen and oxygen.
[0048] Examples of the co-catalyst for the hydrogen generation photocatalyst include transition metals such as Pt, Pd, Ru, Ni, Au, Fe, Ir, and Rh; NiO, RuO 2 、IrO 2 and Rh 2 O 3 Other metal oxides; NiS, and MoS 2 , etc.; Cr-Rh composite oxides, etc. These can be used alone or in combination of two or more. Among these, from the viewpoint of hydrogen generation efficiency, preferably one or more selected from transition metals, more preferably one or more selected from metals belonging to Group 10 of the periodic table, and further preferably Ru.
[0049] As the co-catalyst of the above oxygen-generating photocatalyst, there can be mentioned transition metals such as Mn, Fe, Co, Ir, Ru, Rh, Ni, Sb, Nb, Th and Cr; oxides and hydroxides of these transition metals; etc. These can be used alone or in combination of two or more. Among these, from the viewpoint of oxygen generation efficiency, one or more selected from oxides of transition metals are preferred.
[0050] Examples of a method for supporting the co-catalyst on the surface of the hydrogen-generating photocatalyst or the oxygen-generating photocatalyst include photoelectrochemical deposition, impregnation, adsorption, precipitation, hydrogen reduction, and electroless plating.
[0051] The impregnation method and the adsorption method are methods in which a photocatalyst is dispersed in a solution in which a promoter precursor is dissolved, and the promoter precursor is adsorbed on the surface of the photocatalyst. Examples of the promoter precursor include chlorides, nitrates and amine salts of the transition metals.
[0052] It is preferred that the promoter precursor is supported on the surface of the photocatalyst and then reduced. The promoter precursor is reduced to a metallic state, thereby improving the activity. Examples of methods for reducing the promoter precursor include photoreduction and chemical reduction.
[0053] The photoreduction method is a method of reducing the promoter precursor adsorbed on the photocatalyst by utilizing excited electrons generated in the photocatalyst by irradiating the photocatalyst with ultraviolet light or visible light. In addition, the chemical reduction method is a method of reducing the promoter precursor under a hydrogen gas flow at about 400°C or below, preferably 300°C or below. The promoter supported on the surface of the photocatalyst is in the form of particles, and the amount of the supported promoter can be appropriately adjusted.
[0054] The solid medium is a material that can store excited electrons generated by the oxygen-generating photocatalyst that are not involved in the reduction of water, etc. and holes generated by the hydrogen-generating photocatalyst that are not involved in the oxidation of water, etc., and can cause charge recombination reactions between the excited electrons and the holes.
[0055] As the above-mentioned solid medium, transition metals such as gold, silver, copper, nickel, titanium, manganese, rhodium, palladium, ruthenium and iridium can be cited; transition metal compounds such as oxides, nitrides and carbides of these transition metals; doped metal oxides such as tin-doped indium oxide (ITO), zinc oxide doped with metals (B, Al, Ga), fluorine-doped tin oxide, and antimony-doped tin oxide, etc. These can be used alone or in combination. Among these, from the viewpoint of improving catalytic activity, it is preferred to include one or more transition metals or their compounds, more preferably one or more transition metals or their compounds selected from elements belonging to Group 11 of the periodic table, further preferably one or more gold or silver, and further preferably gold.
[0056] The electron capture surface of the above-mentioned oxygen-generating photocatalyst depends on the composition and crystal system of the material. As a method for determining the electron capture surface, for example, a semiconductor crystal grain as a material of the oxygen-generating photocatalyst is brought into contact with a precursor solution of a metal such as Pt, Au or Ag, and is loaded with metal particles precipitated by a photoprecipitation method, and a method of confirming the crystal surface of the precipitated metal particles using a SEM (scanning electron microscope) or a TEM (transmission electron microscope). The identification of the crystal surface of the precipitated metal particles can be carried out, for example, by determining the attributable crystal plane spacing based on the lattice fringes observed based on TEM.
[0057] The electron-capturing surface of oxygen-generating photocatalysts, such as BiVO 4 (monoclinic scheelite crystal) is the {010} plane or the {040} plane, and in the case of TiO 2(rutile crystal) is {110} face, and in TiO 2 (anatase crystal) is {101} face, and in WO 3 (monoclinic crystal) is the {002} plane, and in SrTiO 3 (perovskite crystal) is {110} plane, and Ag 3 PO 4 (cubic crystal) is the {110} face.
[0058] In the above-mentioned junction-type photocatalyst, it is preferable that the above-mentioned hydrogen-generating photocatalyst is selectively joined to the above-mentioned solid medium.
[0059] <Method for producing a junction-type photocatalyst>
[0060] The manufacturing method of the present invention is a manufacturing method of a junction type photocatalyst, which allows a solid medium to be bonded to the surface of an oxygen-generating photocatalyst, and then allows a hydrogen-generating photocatalyst to be bonded to the surface of the solid medium. The manufacturing method of the junction type photocatalyst is a manufacturing method of a junction type photocatalyst having the solid medium between the hydrogen-generating photocatalyst and the oxygen-generating photocatalyst.
[0061] The method for producing the junction-type photocatalyst includes the following step 1.
[0062] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0063] Specifically, the following production methods (I) and (II) further comprising steps 2, 3, and 4 or steps 2', 3', and 4' are preferred.
[0064] That is, as a method for producing a conjugated photocatalyst of the present invention, preferably, for example, (I) a method for producing a conjugated photocatalyst comprising the following steps 1 to 4 can be cited. However, step 2 and step 3 are not sequential. Step 3 can be performed after step 2, step 2 can be performed after step 3, or can be performed simultaneously.
[0065] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0066] Step 2: A step of introducing an ionic group into the solid medium to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic group.
[0067] Step 3: A step of introducing an ionic polymer having a charge opposite to that of the ionic group into the hydrogen generation photocatalyst
[0068] Step 4: A step of mixing the oxygen-generating photocatalyst obtained in step 2 to which the solid medium having the ionic group is bonded and the hydrogen-generating photocatalyst introduced with the ionic polymer obtained in step 3
[0069] In addition, as a method for producing a conjugated photocatalyst of the present invention, a method for producing a conjugated photocatalyst comprising the following steps 1, 2', 3' and 4' can be preferably cited, for example. Wherein, step 2' and step 3' are not sequential. Step 3' can be performed after step 2', step 2' can be performed after step 3', or can be performed simultaneously.
[0070] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0071] Step 2': introducing an ionic group into the solid medium, and then reacting an ionic polymer having a charge opposite to that of the ionic group with the ionic group to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic polymer
[0072] Step 3': a step of introducing an ionic polymer having a charge opposite to that of the ionic polymer into the hydrogen generation photocatalyst
[0073] Step 4': a step of mixing the oxygen-generating photocatalyst obtained in step 2' and the solid medium having the ionic polymer bonded thereto with the hydrogen-generating photocatalyst introduced thereto obtained in step 3'
[0074] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation supporting method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[0075] Step 1 is a step of manufacturing an oxygen-generating photocatalyst joined with a solid medium.
[0076] In the above step 1, the method for bonding (supporting) the solid medium on the surface of the oxygen-generating photocatalyst is not particularly limited, and it is preferred to use, for example, at least one method selected from the group consisting of photoelectrochemical deposition, impregnation support, and precipitation.
[0077] The photoelectrochemical deposition method is a method of irradiating a dispersion liquid containing a photocatalyst, a metal salt (precursor of a solid medium), and an organic carboxylic acid compound, reducing the metal salt, and precipitating and bonding (carrying) metal particles or metal compound particles (solid medium) on the surface of the photocatalyst. As the precursor of the solid medium, ionic salts of media such as silver nitrate and gold halide (tetrachloroauric acid) can be cited.
[0078] The above-mentioned impregnation loading method refers to the following method: a solution or dispersion in which a metal salt (precursor of a solid medium) and an organic carboxylic acid compound are dissolved or dispersed is mixed with a photocatalyst, and then the solvent is removed by filtration separation, decantation or solid-liquid separation based on centrifugation, or distillation of the solvent under heating or reduced pressure, etc., so that the metal salt is loaded on the surface of the photocatalyst, and then the metal particles or metal compound particles (solid medium) are bonded (loaded) on the surface of the photocatalyst by calcining or reducing the metal salt.
[0079] The above-mentioned precipitation method refers to a method of bonding (supporting) the metal particles or metal compound particles (solid medium) obtained by reducing a metal salt (precursor of a solid medium) in a solution containing an organic carboxylic acid compound with a photocatalyst.
[0080] From the viewpoint of increasing the coverage of the solid medium on the electron-capturing surface of the oxygen-generating photocatalyst to 40% or more, the photoelectrochemical deposition method is preferred.
[0081] The above-mentioned photoelectric deposition method is a method of irradiating a dispersion liquid containing an oxygen-generating photocatalyst, an organic carboxylic acid compound, and a solid medium or its precursor, so that the above-mentioned solid medium is bonded (supported) on the above-mentioned oxygen-generating photocatalyst. It is believed that at this time, electrons and holes are generated in the photocatalyst by irradiation with light, and the electrons cause the reduction and precipitation of the solid medium, and the holes cause the oxidation of water, etc.
[0082] As the solvent used in the above dispersion, water is preferred. In order to promote consumption of holes, a lower alcohol such as methanol, ethanol, or 2-propanol may be used as an auxiliary agent (sacrificial agent).
[0083] It is speculated that the organic carboxylic acid compound helps the reduction of the metal salt (precursor of the solid medium) and also serves as an auxiliary agent for bonding (supporting) the solid medium on the oxygen-generating photocatalyst. In addition, by using the organic carboxylic acid compound, the coverage of the solid medium with respect to the electron capture surface of the oxygen-generating photocatalyst is improved. For example, in BiVO 4In the case of (monoclinic scheelite crystal), the selectivity for the {010} plane as the electron-capturing plane is improved, the solid medium can be bonded to the oxygen-generating photocatalyst in a dense state, and the catalytic activity can be improved.
[0084] As the above-mentioned organic carboxylic acid compound, from the viewpoint of bonding the above-mentioned solid medium to the above-mentioned oxygen-generating photocatalyst in a dense state, it is preferred that it contains at least one selected from ether carboxylic acid, fatty acid, hydroxymonocarboxylic acid and polycarboxylic acid, and more preferably contains ether carboxylic acid. Specifically, the following organic carboxylic acid compounds 1) to 4) can be cited.
[0085] 1) Ether carboxylic acid
[0086] Examples of the ether carboxylic acid include compounds represented by the following general formula (1).
[0087] R 1 -O-(EO) n -CH 2 COOH(1)
[0088] In the above general formula (1), from the viewpoint of water solubility and auxiliary agent function, R 1 Preferably, it is a linear or branched alkyl or alkenyl group having 4 to 22 carbon atoms, more preferably a linear or branched alkyl or alkenyl group having 8 to 18 carbon atoms, and still more preferably a linear or branched alkyl group (alkyl ether carboxylic acid) having 8 to 18 carbon atoms. In addition, from the viewpoint of water solubility and auxiliary agent function, the average number of added moles n of EO (ethyleneoxy group) is preferably 1 to 25, more preferably 2 to 12, and still more preferably 3 to 8.
[0089] Examples of the ether carboxylic acid include polyoxyethylene (4.5) lauryl ether acetic acid, and the ether carboxylic acid may be a potassium salt, a sodium salt, or an ammonium salt thereof.
[0090] 2) Fatty acids
[0091] Preferred examples of the fatty acid include fatty acids represented by the following general formula (2).
[0092] R 2 -COOH(2)
[0093] In the above general formula (2), from the viewpoint of water solubility and auxiliary agent function, R 2 It is preferably a linear or branched alkyl or alkenyl group having 4 to 22 carbon atoms, more preferably a linear or branched alkyl or alkenyl group having 8 to 22 carbon atoms, and still more preferably a linear or branched alkyl or alkenyl group having 12 to 18 carbon atoms.
[0094] Examples of the fatty acid include oleic acid, and potassium salts, sodium salts, or ammonium salts thereof may be used.
[0095] 3) Hydroxymonocarboxylic acid
[0096] The hydroxymonocarboxylic acid preferably has a hydrocarbon group having 2 to 12 carbon atoms, and more preferably has a hydrocarbon group having 3 to 8 carbon atoms, from the viewpoint of water solubility and auxiliary agent function.
[0097] Examples of the hydroxymonocarboxylic acid include glycolic acid, lactic acid, glyceric acid, gluconic acid, and pantothenic acid.
[0098] 4) Polycarboxylic acid
[0099] From the viewpoint of water solubility and auxiliary agent function, the polyvalent carboxylic acid preferably has a hydrocarbon group having 2 to 12 carbon atoms, and more preferably has a hydrocarbon group having 3 to 8 carbon atoms.
[0100] The polycarboxylic acid is preferably a dicarboxylic acid, and examples thereof include malic acid, tartaric acid, oxalic acid, malonic acid, maleic acid, succinic acid, and glutaric acid. The tricarboxylic acid includes citric acid.
[0101] The organic carboxylic acid compounds 1) to 4) above may be used alone or in combination of two or more.
[0102] In the above step 1, it is preferred that in the dispersion liquid containing the photocatalyst, the metal salt (precursor of the solid medium) and the organic carboxylic acid compound, from the viewpoint of increasing the coverage of the solid medium on the oxygen-generating photocatalyst and improving the catalytic activity, 100 parts by mass or more of the organic carboxylic acid compound is contained (mixed) in a dispersion liquid containing the photocatalyst, the metal salt (precursor of the solid medium) and the organic carboxylic acid compound, more preferably 500 parts by mass or more, and further preferably 1000 parts by mass or more. From the same viewpoint, it is preferably 100,000 parts by mass or less, more preferably 50,000 parts by mass or less, and further preferably 20,000 parts by mass or less. It is preferably 100 parts by mass or more and 100,000 parts by mass or less, more preferably 500 parts by mass or more and 50,000 parts by mass or less, and further preferably 1000 parts by mass or more and 20,000 parts by mass or less.
[0103] In the above-mentioned step 1, from the viewpoint of increasing the coverage of the solid medium on the oxygen-generating photocatalyst and improving the catalytic activity, it is preferred that in the above-mentioned dispersion, relative to 100 parts by mass of the above-mentioned oxygen-generating photocatalyst, 0.1 parts by mass or more of the above-mentioned solid medium or its precursor (metal salt) is contained (mixed), more preferably 1 part by mass or more, and further preferably 5 parts by mass or more. From the same viewpoint, it is preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, and further preferably 100 parts by mass or less. It is preferably 0.1 parts by mass or more and 1000 parts by mass or less, more preferably 1 part by mass or more and 500 parts by mass or less, and further preferably 5 parts by mass or more and 100 parts by mass or less.
[0104] The irradiated light may be sunlight or artificial light (fluorescent lamp, UV lamp, LED, mercury lamp, xenon lamp, metal halide lamp, sodium lamp, halogen lamp, etc.). From the viewpoint of increasing the coverage of the solid medium on the oxygen-generating photocatalyst, the wavelength of the light is preferably 180 to 1000 nm, more preferably 300 to 800 nm.
[0105] The irradiation light intensity is preferably 1 mW / cm from the viewpoint of increasing the coverage of the solid medium on the electron-capturing surface of the oxygen-generating photocatalyst. 2 More preferably, 2 mW / cm 2 More preferably, 5 mW / cm 2 From the same viewpoint, it is preferably 200 mW / cm 2 Below, more preferably 100 mW / cm 2 Below, more preferably 50 mW / cm 2 the following.
[0106] Step 2: A step of introducing an ionic group into the above-mentioned solid medium (hereinafter referred to as "Form 1") to obtain an oxygen-generating photocatalyst bonded to the solid medium having the above-mentioned ionic group.
[0107] In order to introduce the ionic group into the above-mentioned solid medium, a compound containing a group having affinity for the solid medium and an ionic group can be used. Specifically, when the above-mentioned solid medium contains gold (atom), silver, or platinum, from the viewpoint of affinity with the above-mentioned metal, a thiol compound having an ionic group, a selenium compound having an ionic group, and a thiol compound having an ionic group are preferred, and a thiol compound having an ionic group is more preferred.
[0108] The mercapto compound having the above-mentioned ionic group has at least one ionic group (ionic substituent). Among the above-mentioned ionic groups, examples of anionic groups include sulfonic acid groups, phosphonic acid groups, phosphoric acid groups, and carboxyl groups, and examples of cationic groups include ammonium groups. Among them, from the viewpoint of improving catalytic activity, mercapto compounds having ammonium groups and carboxyl groups are preferred.
[0109] From the same viewpoint, the ionic group is more preferably an anionic group, and even more preferably a carboxylate anion (carboxyl group).
[0110] As the mercapto compound having the above-mentioned ionic group, from the viewpoint of improving the catalytic activity, it is preferred to have an alkylene group having 1 or more carbon atoms, more preferably 2 or more carbon atoms. In addition, from the same viewpoint, it is preferred to have an alkylene group having 18 or less carbon atoms, more preferably 14 or less carbon atoms, and further preferably 8 or less carbon atoms.
[0111] The mercapto compound having an ionic group preferably has two or less mercapto groups, and more preferably has one mercapto group, from the viewpoint of improving the catalytic activity.
[0112] When the mercapto compound having the above-mentioned ionic group has an acidic group, it may be an acid, a salt, or a mixture thereof.
[0113] As the mercapto compound having the above-mentioned ionic group, for example, thiomalic acid, 3-mercaptopropionic acid, thioglycolic acid, (11-mercaptoundecyl)trimethylammonium, etc. are preferably used.
[0114] In the above-mentioned step 2, relative to 100 mass parts of the oxygen-producing photocatalyst joined (loaded) to the above-mentioned solid medium, from the viewpoint of improving the catalytic activity, it is preferably contained (mixed) with 0.1 mass parts or more of the mercapto compound having the above-mentioned ionic group, and more preferably 1 mass parts or more. In addition, from the same viewpoint, it is preferably 100 mass parts or less, and more preferably 50 mass parts or less. It is preferred to react with 0.1 mass parts or more and 100 mass parts or less, and more preferably 1 mass parts or more and 50 mass parts or less.
[0115] Step 2': a step of introducing an ionic group into the solid medium ("method 1"), and then reacting an ionic polymer having a charge opposite to that of the ionic group with the ionic group (hereinafter referred to as "method 2"), thereby obtaining an oxygen-generating photocatalyst bonded to a solid medium having the ionic polymer.
[0116] Similar to the above-mentioned method 1, an ionic group is introduced into the above-mentioned solid medium, and then an ionic polymer having a charge opposite to the charge of the above-mentioned ionic group is reacted with the above-mentioned ionic group (ionic bonding) ("method 2"), thereby obtaining an oxygen-producing photocatalyst joined to a solid medium into which the ionic group derived from the above-mentioned ionic polymer is introduced.
[0117] As a method for introducing ionic groups into the above-mentioned solid medium and causing an ionic polymer having a charge opposite to that of the above-mentioned ionic groups to react with the above-mentioned ionic groups (ionic bonding), for example, the following method can be cited: (i) mixing and reacting an oxygen-producing photocatalyst joined (supported) to a solid medium with a mercapto compound having an anionic group, thereby introducing the anionic group into the solid medium, and causing a polymer having a cationic group having a charge opposite to that of the above-mentioned anionic group (hereinafter also referred to as a "cationic polymer") to mix and react with it (ionic bonding).
[0118] In addition, as other methods, the following methods can be cited: (ii) reacting an oxygen-producing photocatalyst bonded (supported) to a solid medium with a thiol compound having a cationic group, thereby introducing the cationic group into the above-mentioned solid medium, and mixing and reacting (ionic bonding) with a polymer having an anionic group with a charge opposite to that of the above-mentioned cationic group (hereinafter also referred to as "anionic polymer")
[0119] By these methods, the solid medium has an ionic group and an ionic polymer, and the ionic group and the ionic polymer are ionically bonded.
[0120] It should be noted that the above-mentioned ionic polymer refers to a cationic polymer or an anionic polymer. As described later, ionic polymer A and ionic polymer B are used for convenience in order to distinguish the ionicity of the ionic polymer. That is, when ionic polymer A is a cationic polymer, it means that ionic polymer B is an anionic polymer, and when ionic polymer A is an anionic polymer, it means that ionic polymer B is a cationic polymer.
[0121] As the cationic polymer, from the viewpoint of improving the catalytic activity, for example, a polymer having a quaternary ammonium group can be cited. Specifically, a polymer having a quaternary ammonium group is preferred, and more preferably comprises one or more selected from cationized polysaccharides, polymers of diallyl quaternary ammonium salts or copolymers thereof, polymers of (meth)acryloyloxyethyl quaternary ammonium salts or copolymers thereof, polymers of (meth)acrylamidepropyl quaternary ammonium salts or copolymers thereof, and polymers of dimethylamine epichlorohydrin. Further preferred examples include (a) cationized cellulose, (b) cationized guar gum, (c) at least one selected from diallyl quaternary ammonium salt polymers and diallyl quaternary ammonium salt / acrylamide copolymers, or (d) (meth)acryloyloxyethyl quaternary ammonium salt polymers and (meth)acryloyloxyethyl quaternary ammonium salt / acrylamide copolymers, (e) dimethylamine epichlorohydrin polymers, and the above (c) is particularly preferred. The quaternary ammonium group also includes a tertiary amine to which a proton is added.
[0122] (a) Cationized cellulose:
[0123] The degree of cationic substitution of the cationized cellulose is preferably 0.01 to 1, i.e., from the viewpoint of improving catalytic activity, the average value per anhydroglucose unit is preferably 0.01 to 1, more preferably 0.02 to 0.5. In addition, from the viewpoint of improving catalytic activity, the weight average molecular weight of the cationized cellulose is preferably about 100,000 to 8,000,000.
[0124] Examples of commercially available products of (a) include "POIZC-80H (manufactured by Kao Corporation)" and "Polymer JR-400" (manufactured by The Dow Chemical Company).
[0125] (b) Cationized guar gum:
[0126] From the viewpoint of improving the catalytic activity, the degree of cationic substitution of the cationized guar gum is preferably 0.01 to 1, more preferably 0.02 to 0.5, and cationic groups are introduced into the sugar unit.
[0127] Examples of commercially available products of (b) include "Jaguar C-13C" marketed by Rhodia Inc. under the trade name "Jaguar".
[0128] (c) Diallyl quaternary ammonium salt polymers and diallyl quaternary ammonium salt / acrylamide copolymers:
[0129] The weight average molecular weight of the diallyl quaternary ammonium salt polymer is preferably about 30,000 to 1,000,000 from the viewpoint of improving catalytic activity, and the weight average molecular weight of the diallyl quaternary ammonium salt / acrylamide copolymer is preferably about 30,000 to 2,000,000, more preferably about 1,000,000 to 2,000,000 from the viewpoint of improving catalytic activity.
[0130] Examples of commercially available products of (c) include "Merquat 100 (weight average molecular weight: 150,000)" and "Merquat 550 (weight average molecular weight: 1,600,000)" marketed by Lubrizol under the trade name "Merquat".
[0131] (d) (Meth)acryloyloxyethyl quaternary ammonium salt polymer and (meth)acryloyloxyethyl quaternary ammonium salt / acrylamide copolymer:
[0132] The weight average molecular weight of the methacryloyloxyethyl quaternary ammonium salt / acrylamide copolymer is preferably about 100,000 to 10,000,000, and more preferably about 2,000,000 to 6,000,000, from the viewpoint of improving the catalytic activity.
[0133] (e) Dimethylamine epichlorohydrin polymer (poly-2-hydroxypropyldimethylammonium chloride):
[0134] The weight average molecular weight of the dimethylamine-epichlorohydrin polymer is preferably about 1,000 to 100,000, more preferably about 3,000 to 10,000, from the viewpoint of improving the catalytic activity.
[0135] Examples of commercially available products of (e) include "Cation Master PD-7 (weight average molecular weight: 50,000)" commercially available under the trade name "Cation Master" by Yokkaichi Kosei Co., Ltd.
[0136] As the anionic polymer, a polymer having a sulfate group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group or a carboxyl group is preferred. Among them, from the viewpoint of improving the catalytic activity, a polymer having a sulfonic acid group (sulfonic acid polymer) or a polymer having a carboxyl group (carboxylic acid polymer) is preferred.
[0137] As the polymer having a sulfonic acid group, sodium polystyrene sulfonate is preferred.
[0138] As the carboxylic acid polymer, a carboxylic acid polymer having a structural unit derived from an anionic group-containing monomer selected from acrylate, methacrylate and maleate is preferred. It should be noted that the carboxylic acid polymer is preferably a polymer composed of the anionic group-containing monomer, or may be a copolymer of the anionic group-containing monomer and a monomer other than the anionic group-containing monomer.
[0139] As monomers other than the above-mentioned anionic group-containing monomers, for example, alkyl (meth)acrylates such as methyl (meth)acrylate and ethyl (meth)acrylate, N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, isopropyl (meth)acrylamide, N-substituted (meth)acrylamide such as tert-butyl (meth)acrylate, vinyl ethers such as methyl vinyl ether and butyl vinyl ether, styrene, ethylene, propylene, isobutylene and other olefin hydrocarbons can be cited. These can be used alone or in combination of two or more. Among these, alkyl (meth)acrylates such as methyl (meth)acrylate and ethyl (meth)acrylate are preferred.
[0140] In addition, in this specification, "(meth)acrylic acid" means "acrylic acid or methacrylic acid".
[0141] From the viewpoint of improving catalytic activity, the weight average molecular weight (Mw) of the carboxylic acid polymer is preferably 1000 or more, more preferably 5000 or more, and even more preferably 10000 or more. From the same viewpoint, it is preferably 500000 or less, more preferably 100000 or less, even more preferably 50000 or less, and even more preferably 35000 or less.
[0142] From the viewpoint of improving catalytic activity, the weight average molecular weight (Mw) of the polymer having a sulfonic acid group is preferably 10,000 or more, more preferably 50,000 or more, and even more preferably 100,000 or more. From the same viewpoint, it is preferably 5,000,000 or less, more preferably 2,000,000 or less, even more preferably 1,000,000 or less, and even more preferably 600,000 or less.
[0143] In addition, in this specification, the weight average molecular weight (Mw) of the said cationic polymer and the said anionic polymer is a value calculated|required by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0144] In the above-mentioned step 2', relative to 100 parts by mass of the oxygen-producing photocatalyst joined (loaded) with the above-mentioned solid medium into which the ionic groups are introduced, from the viewpoint of improving the photocatalytic activity, it is preferred to contain (mix) 5 parts by mass or more of the above-mentioned ionic polymer, and more preferably 10 parts by mass or more. In addition, from the same viewpoint, it is preferably less than 500 parts by mass, and more preferably less than 100 parts by mass.
[0145] Step 3: A step of introducing an ionic polymer having a charge opposite to the charge of the ionic group into the hydrogen generation photocatalyst.
[0146] Step 3': a step of introducing an ionic polymer having a charge opposite to that of the ionic polymer into the hydrogen generation photocatalyst.
[0147] The step 3 is a step of introducing an ionic polymer having a charge opposite to the charge of the ionic group of the solid medium in the step 2 into the hydrogen generation photocatalyst.
[0148] For example, in the case where the ionic group possessed by the above-mentioned solid medium in the above-mentioned step 2 is an anionic group, the above-mentioned hydrogen-producing photocatalyst can be mixed and dispersed by using a polymer having a cationic group, thereby introducing an ionic polymer having an opposite charge. Alternatively, the above-mentioned hydrogen-producing photocatalyst can be mixed and dispersed by using a polymer having an anionic group, and then mixed and dispersed with a polymer having a cationic group, thereby introducing an ionic polymer having an opposite charge.
[0149] That is, a conjugated photocatalyst has a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst, wherein the solid medium has an ionic group, and the hydrogen-producing photocatalyst has an ionic polymer B having a charge opposite to the charge of the ionic group via an ionic polymer A, and the solid medium is conjugated to the hydrogen-producing photocatalyst through the ionic bond between the ionic group and the ionic polymer B.
[0150] That is, the ionic polymer possessed by the hydrogen-producing photocatalyst is an ionic polymer A, and an ionic polymer B having a charge opposite to the charge of the ionic group is provided through the ionic polymer A, and the solid medium is connected to the hydrogen-producing photocatalyst through the ionic bond between the ionic group and the ionic polymer B.
[0151] It should be noted that when the ionic group is an anionic group, the ionic polymer A is an anionic polymer, and the ionic polymer B is a cationic polymer. In addition, when the ionic group is a cationic group, the ionic polymer A is a cationic polymer, and the ionic polymer B is an anionic polymer.
[0152] In addition, the above-mentioned step 3' is the following step: for the ionic groups possessed by the above-mentioned solid medium in the above-mentioned step 2', the above-mentioned hydrogen-producing photocatalyst is mixed and dispersed together with an ionic polymer having a charge opposite to that of the above-mentioned ionic groups, thereby introducing the ionic polymer having a charge opposite to that of the above-mentioned ionic groups into the above-mentioned hydrogen-producing photocatalyst.
[0153] For example, in the case where the ionic group possessed by the above-mentioned solid medium in the above-mentioned step 2' is an anionic group, by further using a polymer having a cationic group, mixing and dispersing, so that the above-mentioned solid medium has a cationic polymer, the above-mentioned hydrogen-producing photocatalyst can be mixed and dispersed using a polymer having anionic groups, thereby introducing an ionic polymer with an opposite charge, or the above-mentioned hydrogen-producing photocatalyst can be mixed and dispersed using a polymer having a cationic group, and then mixed and dispersed with a polymer having anionic groups, thereby introducing an ionic polymer with an opposite charge.
[0154] That is, a bonding type photocatalyst has a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst, the solid medium has an ionic group and an ionic polymer B, the ionic group is bonded to the ionic polymer B, the hydrogen-producing photocatalyst has an ionic polymer A with a charge opposite to that of the ionic polymer B, and the solid medium is bonded to the hydrogen-producing photocatalyst through the ionic bond between the ionic polymer B of the solid medium and the ionic polymer A of the hydrogen-producing photocatalyst.
[0155] That is, the ionic polymer possessed by the hydrogen-producing photocatalyst is an ionic polymer A, the solid medium has the ionic group and an ionic polymer B having a charge opposite to that of the ionic polymer A, the ionic group is combined with the ionic polymer B, and the solid medium is bonded to the hydrogen-producing photocatalyst through the ionic bond between the ionic polymer B possessed by the solid medium and the ionic polymer A possessed by the hydrogen-producing photocatalyst.
[0156] It should be noted that when the ionic group is an anionic group, the ionic polymer A is an anionic polymer, and the ionic polymer B is a cationic polymer. In addition, when the ionic group is a cationic group, the ionic polymer A is a cationic polymer, and the ionic polymer B is an anionic polymer.
[0157] As the ionic polymer, the anionic polymer or the cationic polymer in the embodiment 2 can be used.
[0158] In the above-mentioned step 3 and the above-mentioned step 3', from the viewpoint of improving the catalytic activity, relative to 100 parts by mass of the above-mentioned hydrogen-producing photocatalyst, it is preferred to contain (mix) 5 parts by mass or more of the above-mentioned ionic polymer, and more preferably 20 parts by mass or more. In addition, from the same viewpoint, it is preferably 500 parts by mass or less, and more preferably 100 parts by mass or less. It is preferred to contain (mix) 5 parts by mass or more and 500 parts by mass or less of the above-mentioned ionic polymer, and more preferably to use 20 parts by mass or more and 100 parts by mass or less.
[0159] Step 4: A step of mixing the oxygen-generating photocatalyst obtained in step 2 and to which the solid medium having the ionic group is bonded (supported) and the hydrogen-generating photocatalyst obtained in step 3 and to which the ionic polymer is introduced.
[0160] Step 4': a step of mixing the oxygen-generating photocatalyst obtained in step 2' and bonded with the solid medium having the ionic polymer, and the hydrogen-generating photocatalyst introduced with the ionic polymer obtained in step 3'.
[0161] In the above steps 4 and 4', the hydrogen-producing photocatalyst introduced with the above-mentioned ionic polymer obtained in the above steps 3 and 3' is mixed with the oxygen-producing photocatalyst bonded (supported) with the solid medium having the above-mentioned ionic group, thereby enabling the oxygen-producing photocatalyst and the hydrogen-producing photocatalyst to be bonded via the solid medium.
[0162] For example, when using an oxygen-producing photocatalyst conjugated (supported) with a solid medium into which anionic groups have been introduced, a hydrogen-producing photocatalyst into which cationic groups have been introduced from a cationic polymer can be used. Also, when using an oxygen-producing photocatalyst conjugated (supported) with a solid medium into which cationic groups have been introduced, a hydrogen-producing photocatalyst into which anionic groups have been introduced from anionic polymer can be used.
[0163] In the above-mentioned step 4, from the viewpoint of improving the catalytic activity, the mixing mass ratio (the hydrogen-producing photocatalyst introduced with the above-mentioned ionic polymer obtained in the above-mentioned step 3 / the oxygen-producing photocatalyst joined (supported) to the solid medium having the above-mentioned ionic group obtained in the above-mentioned step 2) is preferably greater than 0.01, more preferably greater than 0.05, and further preferably greater than 0.07. From the same viewpoint, it is preferably less than 10, more preferably less than 5, and further preferably less than 1. It is preferably greater than 0.01 and less than 10, more preferably greater than 0.05 and less than 5, and further preferably greater than 0.07 and less than 1.
[0164] In addition, in the above-mentioned step 4', from the viewpoint of improving the catalytic activity, the mixing mass ratio (the hydrogen-producing photocatalyst introduced with the above-mentioned ionic polymer obtained in the above-mentioned step 3' / the oxygen-producing photocatalyst bonded with the solid medium having the above-mentioned ionic polymer obtained in the above-mentioned step 2') is preferably greater than 0.01, more preferably greater than 0.05, and further preferably greater than 0.07. From the same viewpoint, it is preferably less than 10, more preferably less than 5, and further preferably less than 1. It is preferably greater than 0.01 and less than 10, more preferably greater than 0.05 and less than 5, and further preferably greater than 0.07 and less than 1.
[0165] In the above-mentioned step 4 and step 4', by adjusting the above-mentioned mixing mass ratio, in any case of embodiments 1 and 2, the solid medium and the hydrogen-producing photocatalyst are connected via the ionic polymer. Through the above-mentioned ionic polymer, the electrostatic interaction exerts a strong effect, and the hydrogen-producing photocatalyst and the oxygen-producing photocatalyst are not separated but connected via the solid medium, so the catalytic activity is improved, and water can be decomposed into oxygen and hydrogen with a high water decomposition reaction efficiency.
[0166] (Coverage and selectivity of solid media in junction-type photocatalysts and oxygen-generating photocatalysts)
[0167] In the conjugated photocatalyst of the present invention and / or the oxygen-generating photocatalyst of the present invention, the coverage of the solid medium relative to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more. From the viewpoint of improving catalytic activity, it is preferably 50% or more, more preferably 55% or more, and further preferably 58% or more. The upper limit is preferably 100% or less. From the viewpoint of improving the adhesion and light transmittance of the solid medium, it is more preferably 95% or less, and further preferably 90% or less.
[0168] In the above-mentioned conjugated photocatalyst and / or the above-mentioned oxygen-producing photocatalyst, from the viewpoint of improving catalytic activity, improving the adhesion and transmittance of the solid medium, the coverage rate of the above-mentioned solid medium relative to the electron capture surface area of the above-mentioned oxygen-producing photocatalyst is preferably greater than 40% and less than 100%, more preferably greater than 50% and less than 95%, and further preferably greater than 55% and less than 90%.
[0169] By using the manufacturing method of step 1, that is, using at least one method selected from the group consisting of photoelectric deposition, impregnation support, and precipitation of an organic carboxylic acid compound and a solid medium or its precursor, the above-mentioned coverage rate can be made to be above 40%. The coverage rate can be further increased by, for example, increasing the content of the organic carboxylic acid compound relative to the solid medium or its precursor, or extending the irradiation time in the photoelectric deposition method.
[0170] In the above-mentioned junction-type photocatalyst and / or the above-mentioned oxygen-generating photocatalyst, from the viewpoint of improving catalytic activity, the junction selectivity of the above-mentioned solid medium relative to the electron capture surface area of the above-mentioned oxygen-generating photocatalyst is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, further preferably 90% or more, and from the viewpoint of manufacturability, it is 100% or less, preferably 99.5% or less. The junction selectivity can be improved by, for example, the type of manufacturing method in the above-mentioned step 1, preferably using a photoelectrodeposition method.
[0171] The coverage and the junction selectivity can be obtained by the method of the following example.
[0172] <Method for producing oxygen-generating photocatalyst>
[0173] The method for producing the oxygen-generating photocatalyst is the same method as step 1 of the method for producing the junction-type photocatalyst described above.
[0174] <Photocatalyst complex>
[0175] The photocatalyst composite of the present invention comprises the above-mentioned junction-type photocatalyst on a substrate.
[0176] The above-mentioned substrate is not particularly limited as long as it is a substrate on which the above-mentioned junction-type photocatalyst can be fixed, and examples thereof include ceramic substrates such as alumina; glass substrates such as soda-lime glass and borosilicate glass; quartz substrates; metal substrates such as titanium, copper, tin, iron, aluminum and stainless steel; organic substrates such as methacrylic resin, polyurethane resin, phenolic resin, melamine resin, urea-formaldehyde resin, polyester resin, polycarbonate resin, fluororesin, polyethylene, polypropylene, polystyrene, polyamide, polyimide, polyacetal, polyvinyl chloride and polyvinylidene chloride; fiber substrates such as glass fiber and carbon fiber; natural substrates such as paper, bamboo and wood, etc.
[0177] The substrate preferably has pores, and more preferably has continuous pores, so that hydrogen generated by a water decomposition reaction on the surface of the junction-type photocatalyst can reach the outside through the pores, thereby enabling more efficient production of hydrogen.
[0178] There is no particular limitation on the method for producing the photocatalyst complex, and examples thereof include: (1) applying a dispersion containing the above-mentioned conjugated photocatalyst on a substrate, drying it, and calcining it as needed to fix the above-mentioned conjugated photocatalyst on the substrate; (2) applying a dispersion containing the above-mentioned oxygen-producing photocatalyst on a substrate, drying it, and calcining it as needed to fix the above-mentioned oxygen-producing photocatalyst on the substrate; and then, conjugating the above-mentioned solid medium to the surface of the above-mentioned oxygen-producing photocatalyst by the same method as above; and then, conjugating the above-mentioned hydrogen-producing photocatalyst to the surface of the above-mentioned solid medium.
[0179] <Application of Conjugated Photocatalyst and Photocatalyst Composite>
[0180] The conjugated photocatalyst and photocatalyst complex of the present invention can be used not only as a photocatalyst for catalyzing the decomposition reaction of water and alcohol, but also as a photocatalyst for catalyzing the decomposition reaction of organic matter. For example, they can be used as environmental purifiers, antibacterial / fungicides, deodorants or antifouling agents for detoxifying harmful organic compounds, bacteria, and malodorous substances, and for detoxifying inorganic compounds (ammonium ions, ammonia, nitrate ions and nitrite ions, etc.).
[0181] <Method for producing hydrogen>
[0182] There is no particular limitation on the method for producing hydrogen using the above-mentioned conjugated photocatalyst or the above-mentioned photocatalyst complex of the present invention, and an example thereof is the following method for producing hydrogen, which includes the step of irradiating the above-mentioned conjugated photocatalyst or the above-mentioned photocatalyst complex with light in the presence of water or alcohol, causing water or alcohol to undergo a decomposition reaction to produce at least hydrogen.
[0183] The irradiated light may be any one of sunlight or artificial light (fluorescent lamp, UV lamp, LED, mercury lamp, xenon lamp, metal halide lamp, sodium lamp, halogen lamp, etc.). The wavelength of the light is preferably 180 to 1000 nm, more preferably 300 to 800 nm, from the viewpoint of promoting the decomposition reaction. From the viewpoint of promoting the decomposition reaction, the irradiance of the light is preferably 1 μW / m 2 More preferably, 1mW / m 2 From the viewpoint of promoting the decomposition reaction, the decomposition reaction temperature is preferably 0° C. or higher, more preferably 15° C. or higher.
[0184] The amount of hydrogen generated by the junction-type photocatalyst or the photocatalyst complex of the present invention (per 55 mg of the catalyst) is preferably 0.05 (μmol·h -1 ) or more, more preferably 0.1 (μmol·h -1 ) or more, more preferably 0.20 (μmol·h -1 ) or more, the upper limit is not particularly limited, and is preferably 1 (mol·h -1 )the following.
[0185] Regarding the above-mentioned embodiment, the present invention further discloses the following aspects. [1]
[0187] A method for manufacturing a junction type photocatalyst, wherein a solid medium is bonded to the surface of an oxygen-generating photocatalyst, and then a hydrogen-generating photocatalyst is bonded to the surface of the solid medium, wherein the method for manufacturing a junction type photocatalyst is a method for manufacturing a junction type photocatalyst having the solid medium between the hydrogen-generating photocatalyst and the oxygen-generating photocatalyst.
[0188] The method for producing the junction type photocatalyst comprises the following steps 1:
[0189] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation supporting method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof. [2]
[0191] The method for producing a junction-type photocatalyst according to [1], wherein the solid medium and the hydrogen-generating photocatalyst are joined via an ionic polymer. [3]
[0193] The method for producing a conjugated photocatalyst according to [1] or [2], wherein the solid medium has an ionic group, and the solid medium and the hydrogen-generating photocatalyst are conjugated via an ionic polymer having a charge opposite to that of the ionic group. [4]
[0195] The method for producing a junction-type photocatalyst according to any one of [1] to [3], wherein in the step 1, when the photoelectric deposition method is used, the step includes irradiating a dispersion liquid containing an oxygen-generating photocatalyst in addition to the organic carboxylic acid compound and the solid medium or a precursor thereof. [5]
[0197] The method for producing a junction-type photocatalyst according to any one of [1] to [4], wherein the organic carboxylic acid compound is at least one selected from the group consisting of ether carboxylic acids, fatty acids, hydroxymonocarboxylic acids, and polycarboxylic acids. [6]
[0199] The method for producing a junction-type photocatalyst according to any one of [1] to [5], wherein the organic carboxylic acid compound comprises an ether carboxylic acid,
[0200] The solid medium comprises gold. [7]
[0202] A method for producing a junction type photocatalyst, which is a method for producing a junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst.
[0203] The solid medium has ionic groups,
[0204] The hydrogen-generating photocatalyst has the ionic polymer having a charge opposite to that of the ionic group.
[0205] The solid medium is bonded to the hydrogen-generating photocatalyst through the ionic bond between the ionic group and the ionic polymer.
[0206] The solid medium contains gold, and the method for producing the junction-type photocatalyst comprises the following steps 1:
[0207] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of photoelectrodeposition, impregnation support, and precipitation using an organic carboxylic acid compound containing ether carboxylic acid and the solid medium or a precursor thereof. [8]
[0209] A method for producing a junction type photocatalyst, which is a method for producing a junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst.
[0210] The solid medium has ionic groups,
[0211] The hydrogen-producing photocatalyst comprises an ionic polymer A,
[0212] The hydrogen-generating photocatalyst further comprises an ionic polymer B having a charge opposite to that of the ionic group through the ionic polymer A.
[0213] The solid medium is bonded to the hydrogen-generating photocatalyst through the ionic bond between the ionic group and the ionic polymer B.
[0214] The solid medium contains gold, and the method for producing the junction-type photocatalyst comprises the following step 1:
[0215] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of photoelectrodeposition, impregnation support, and precipitation using an organic carboxylic acid compound containing ether carboxylic acid and the solid medium or a precursor thereof. [9]
[0217] A method for producing a junction type photocatalyst, which is a method for producing a junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst.
[0218] The solid medium has an ionic group, and the solid medium further has an ionic polymer B having a charge opposite to that of the ionic group through the ionic group.
[0219] The hydrogen-producing photocatalyst comprises the ionic polymer A,
[0220] The solid medium and the hydrogen-generating photocatalyst are bonded to each other through an ionic bond between the ionic polymer B of the solid medium and the ionic polymer A of the hydrogen-generating photocatalyst.
[0221] The solid medium contains gold, and the method for producing the junction-type photocatalyst comprises the following steps 1:
[0222] Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of photoelectrodeposition, impregnation support, and precipitation using an organic carboxylic acid compound containing ether carboxylic acid and the solid medium or a precursor thereof.
[10]
[0224] The method for producing a conjugated photocatalyst according to any one of [1] to [9], further comprising the following steps 2 to 4, wherein step 2 and step 3 are not performed in sequence.
[0225] Step 2: a step of introducing an ionic group into the solid medium to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic group.
[0226] Step 3: a step of introducing an ionic polymer having a charge opposite to that of the ionic group into the hydrogen-generating photocatalyst,
[0227] Step 4: A step of mixing the oxygen-generating photocatalyst obtained in step 2 to which the solid medium having the ionic group is bonded and the hydrogen-generating photocatalyst obtained in step 3 to which the ionic polymer is introduced.
[11]
[0229] The method for producing a conjugated photocatalyst according to any one of [1] to [9], further comprising the following steps 2', 3' and 4', wherein step 2' and step 3' are not performed sequentially,
[0230] Step 2': a step of introducing an ionic group into the solid medium, and further reacting an ionic polymer having a charge opposite to that of the ionic group with the ionic group to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic polymer.
[0231] Step 3': a step of introducing an ionic polymer having a charge opposite to that of the ionic polymer into the hydrogen-generating photocatalyst,
[0232] Step 4': a step of mixing the oxygen-generating photocatalyst obtained in step 2' and bonded with the solid medium having the ionic polymer, and the hydrogen-generating photocatalyst introduced with the ionic polymer obtained in step 3'.
[12]
[0234] A method for producing a conjugated photocatalyst according to any one of [1] to
[11] , wherein the solid medium is a transition metal or a compound thereof, preferably a transition metal comprising gold, silver, copper, nickel, titanium, manganese, rhodium, palladium, ruthenium and iridium, more preferably gold or silver, and even more preferably gold.
[13]
[0236] The method for producing a junction-type photocatalyst according to any one of [1] to
[12] , wherein the hydrogen-generating photocatalyst is a metal oxide, preferably TiO 2 、SrTiO 3 ,La 2 Ti 2 O 7 、SnNb 2 O 6 , and compounds doped with one or more metals selected from Cr, Sb, Ta, Ir, and La, more preferably SrTiO 3 .
[14]
[0238] The method for producing a junction-type photocatalyst according to any one of [1] to
[13] , wherein the oxygen-generating photocatalyst is a metal oxide, preferably BiVO 4 、TiO 2 , WO 3 、SrTiO 3 、Ag 3 PO 4 、SnNb 2 O 6 、Bi 2WO 6 , Fe 2 TiO 5 , Fe 2 O 3 、Bi 2 MoO 6 , and compounds doped with one or more metals selected from the group consisting of Cr, Ni, Sb, Nb, Th, Mo, and W, more preferably BiVO 4 .
[15]
[0240] A method for producing a conjugated photocatalyst according to any one of [1] to
[14] , wherein, in step 1, the amount of the organic carboxylic acid compound is preferably greater than 100 parts by mass and less than 100,000 parts by mass, more preferably greater than 500 parts by mass and less than 50,000 parts by mass, and further preferably greater than 1,000 parts by mass and less than 20,000 parts by mass, relative to 100 parts by mass of the solid medium or its precursor (metal salt).
[16]
[0242] A method for manufacturing a conjugated photocatalyst according to any one of [1] to
[15] , wherein, in step 1, the solid medium or its precursor (metal salt) is preferably at least 0.1 parts by mass and at most 1000 parts by mass, more preferably at least 1 parts by mass and at most 500 parts by mass, and further preferably at least 5 parts by mass and at most 100 parts by mass, relative to 100 parts by mass of the oxygen-producing photocatalyst.
[17]
[0244] The method for producing a junction-type photocatalyst according to any one of
[10] to
[16] , wherein when the ionic group is introduced into the solid medium in the step 2 or the step 2', a mercapto compound having an ionic group is used.
[18]
[0246] According to the method for manufacturing a conjugated photocatalyst described in
[17] , when an ionic group is introduced into the solid medium in the step 2 or the step 2', the mercapto compound having an ionic group is preferably reacted in an amount of not less than 0.1 parts by mass and not more than 100 parts by mass, and more preferably not less than 1 parts by mass and not more than 50 parts by mass, relative to 100 parts by mass of the oxygen-producing photocatalyst conjugated (loaded) to the solid medium.
[19]
[0248] A method for manufacturing a conjugated photocatalyst according to any one of
[10] to
[18] , wherein in step 3 and step 3', the ionic polymer is preferably contained (mixed) in an amount of 5 parts by mass or more and 500 parts by mass or less relative to 100 parts by mass of the hydrogen-producing photocatalyst, and more preferably 20 parts by mass or more and 100 parts by mass or less.
[20]
[0250] A method for producing a conjugated photocatalyst according to any one of
[10] ,
[12] to
[19] , wherein in step 4, the mixing mass ratio (the hydrogen-producing photocatalyst introduced with the ionic polymer obtained in step 3 / the oxygen-producing photocatalyst conjugated (supported) with the solid medium having the ionic group obtained in step 2) is preferably greater than 0.01 and less than 10, more preferably greater than 0.05 and less than 5, and further preferably greater than 0.07 and less than 1. [twenty one]
[0252] A method for manufacturing a conjugated photocatalyst according to any one of
[11] to
[19] , wherein in the step 4', the mixing mass ratio (the hydrogen-producing photocatalyst introduced with the ionic polymer obtained in the step 3' / the oxygen-producing photocatalyst conjugated with a solid medium having the ionic polymer obtained in the step 2') is preferably greater than 0.01 and less than 10, more preferably greater than 0.05 and less than 5, and further preferably greater than 0.07 and less than 1. [twenty two]
[0254] A method for manufacturing a conjugated photocatalyst according to any one of [1] to
[21] , wherein the coverage of the solid medium relative to the electron capture surface area of the oxygen-producing photocatalyst is greater than 40%, preferably greater than 40% and less than 100%, more preferably greater than 50% and less than 95%, and further preferably greater than 55% and less than 90%. [twenty three]
[0256] A junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst,
[0257] The coverage of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more, preferably 40% or more and 100% or less, more preferably 50% or more and 95% or less, and further preferably 55% or more and 90% or less. [twenty four]
[0259] According to the conjugated photocatalyst described in
[23] , the conjugation selectivity of the solid medium to the electron capture surface of the oxygen-producing photocatalyst is greater than 60%, preferably greater than 60% and less than 100%, more preferably greater than 80% and less than 100%, and further preferably greater than 90% and less than 99.5%.
[25]
[0261] The conjugated photocatalyst according to
[23] or
[24] , wherein the solid medium and the hydrogen-generating photocatalyst are conjugated via an ionic polymer.
[26]
[0263] The conjugated photocatalyst according to
[23] or
[24] , wherein the solid medium has an ionic group,
[0264] The solid medium and the hydrogen-generating photocatalyst are connected via an ionic polymer having a charge opposite to that of the ionic group.
[27]
[0266] The conjugated photocatalyst according to
[23] or
[24] , wherein the solid medium has an ionic group,
[0267] The hydrogen-generating photocatalyst has the ionic polymer having a charge opposite to that of the ionic group.
[0268] The solid medium is bonded to the hydrogen-generating photocatalyst through ionic bonds between the ionic groups and the ionic polymer.
[28]
[0270] The conjugated photocatalyst according to
[23] or
[24] , wherein the solid medium has an ionic group,
[0271] The hydrogen-producing photocatalyst comprises an ionic polymer A,
[0272] The hydrogen-generating photocatalyst further comprises an ionic polymer B having a charge opposite to that of the ionic group through the ionic polymer A.
[0273] Through the ionic bond between the ionic group and the ionic polymer B, the solid medium is bonded to the hydrogen-generating photocatalyst.
[29]
[0275] The conjugated photocatalyst according to
[23] or
[24] , wherein the solid medium has an ionic group, and the solid medium further has an ionic polymer B having a charge opposite to that of the ionic group via the ionic group,
[0276] The hydrogen-producing photocatalyst comprises an ionic polymer A,
[0277] The solid medium and the hydrogen-generating photocatalyst are bonded to each other through an ionic bond between the ionic polymer B included in the solid medium and the ionic polymer A included in the hydrogen-generating photocatalyst.
[30]
[0279] The conjugation-type photocatalyst according to any one of
[26] to
[29] , wherein the ionic group is an anionic group or a cationic group.
[31]
[0281] The conjugated photocatalyst according to
[30] , wherein the anionic group is preferably a sulfonic acid group, a phosphonic acid group, a phosphoric acid group, or a carboxyl group, more preferably a sulfonic acid group or a carboxyl group, and the cationic group is a quaternary ammonium group.
[32]
[0283] The conjugated photocatalyst according to
[28] or
[29] , wherein the ionic group is an anionic group,
[0284] The ionic polymer A is an anionic polymer,
[0285] The ionic polymer B is a cationic polymer.
[33]
[0287] The conjugated photocatalyst according to
[28] or
[29] , wherein the ionic group is a cationic group,
[0288] The ionic polymer A is a cationic polymer,
[0289] The ionic polymer B is an anionic polymer.
[34]
[0291] According to the conjugated photocatalyst described in
[32] or
[33] , the anionic polymer preferably comprises a polymer having a sulfate group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group or a carboxyl group, and more preferably comprises a polymer having a sulfonic acid group (sulfonic acid polymer) or a polymer having a carboxyl group (carboxylic acid polymer).
[35]
[0293] A conjugated photocatalyst according to any one of
[32] to
[34] , wherein the cationic polymer preferably comprises a polymer having a quaternary ammonium group, more preferably comprises one or more selected from a cationic polysaccharide, a polymer of diallyl quaternary ammonium salt or a copolymer thereof, a polymer of (meth)acryloyloxyethyl quaternary ammonium salt or a copolymer thereof, a polymer of (meth)acrylamidepropyl quaternary ammonium salt or a copolymer thereof, and a polymer of dimethylamine epichlorohydrin, and further preferably comprises (a) cationized cellulose, (b) cationized guar gum, (c) at least one selected from a diallyl quaternary ammonium salt polymer and a diallyl quaternary ammonium salt / acrylamide copolymer, (d) a (meth)acryloyloxyethyl quaternary ammonium salt polymer, a (meth)acryloyloxyethyl quaternary ammonium salt / acrylamide copolymer, or (e) a dimethylamine epichlorohydrin polymer.
[36]
[0295] The conjugation-type photocatalyst according to any one of
[23] to
[35] , wherein the hydrogen-generating photocatalyst is a metal oxide.
[37]
[0297] The conjugated photocatalyst according to
[36] , wherein the metal oxide is preferably selected from TiO 2 、SrTiO 3 ,La 2 Ti 2 O 7 、SnNb 2 O 6 , and compounds doped with one or more metals selected from Cr, Sb, Ta, Ir and La, more preferably SrTiO 3 .
[38]
[0299] The conjugation-type photocatalyst according to any one of
[23] to
[37] , wherein the oxygen-generating photocatalyst is a metal oxide.
[39]
[0301] The conjugated photocatalyst according to
[38] , wherein the metal oxide is preferably BiVO 4 、TiO 2 , WO 3 、SrTiO 3 、Ag 3 PO 4 、SnNb 2 O 6 、Bi 2 WO 6 , Fe 2 TiO 5 , Fe 2 O 3 、Bi2 MoO 6 , and compounds doped with one or more metals selected from Cr, Ni, Sb, Nb, Th, Mo and W, more preferably BiVO 4 .
[40]
[0303] The junction-type photocatalyst according to any one of
[23] to
[39] , wherein the solid medium is a transition metal or a compound thereof.
[41]
[0305] The conjugated photocatalyst according to any one of
[23] to
[40] , wherein the solid medium preferably contains a transition metal selected from the group consisting of gold, silver, copper, nickel, titanium, manganese, rhodium, palladium, ruthenium and iridium, more preferably contains gold or silver, and even more preferably contains gold.
[42]
[0307] The conjugated photocatalyst according to any one of
[23] to
[41] is formed by conjugating the solid medium to the oxygen-generating photocatalyst by using an organic carboxylic acid compound and a solid medium or a precursor thereof by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method.
[43]
[0309] An oxygen-producing photocatalyst joined with a solid medium, wherein the coverage of the solid medium relative to the electron capture surface area of the oxygen-producing photocatalyst is greater than 40%, preferably greater than 40% and less than 100%, more preferably greater than 50% and less than 95%, and further preferably greater than 55% and less than 90%.
[44]
[0311] The oxygen-producing photocatalyst bonded with a solid medium according to
[43] , wherein the bonding selectivity of the solid medium to the electron capture surface is greater than 60%, preferably greater than 60% and less than 100%, more preferably greater than 80% and less than 100%, and further preferably greater than 90% and less than 99.5%.
[45]
[0313] The oxygen-generating photocatalyst bonded with a solid medium according to
[43] or
[44] is formed by bonding the solid medium to the oxygen-generating photocatalyst by using an organic carboxylic acid compound and the solid medium or its precursor by at least one method selected from the group consisting of photoelectrochemical deposition, impregnation support, and precipitation.
[46]
[0315] A method for producing an oxygen-producing photocatalyst bonded with a solid medium is the method for producing an oxygen-producing photocatalyst bonded with a solid medium as described in any one of
[43] to
[45] , the method comprising:
[0316] A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation supporting method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
[47]
[0318] The method for producing an oxygen-generating photocatalyst bonded to a solid medium according to
[46] , wherein, when the photoelectric deposition method is used, the method comprises a step of irradiating a dispersion liquid containing an oxygen-generating photocatalyst in addition to the organic carboxylic acid compound and the solid medium or a precursor thereof.
[48]
[0320] The method for producing an oxygen-generating photocatalyst bonded to a solid medium according to
[46] or
[47] , wherein the organic carboxylic acid compound is at least one selected from ether carboxylic acids, fatty acids, hydroxymonocarboxylic acids, and polycarboxylic acids.
[0321] [49. The method for producing an oxygen-generating photocatalyst bonded to a solid medium according to any one of
[46] to
[48] , wherein the organic carboxylic acid compound comprises an ether carboxylic acid and the solid medium comprises gold.
[50]
[0323] A method for producing an oxygen-producing photocatalyst bonded to a solid medium according to any one of
[46] to
[49] , wherein the amount of the organic carboxylic acid compound is preferably greater than 100 parts by mass and less than 100,000 parts by mass, more preferably greater than 500 parts by mass and less than 50,000 parts by mass, and further preferably greater than 1,000 parts by mass and less than 20,000 parts by mass, relative to 100 parts by mass of the solid medium or its precursor (metal salt).
[51]
[0325] A method for manufacturing an oxygen-producing photocatalyst bonded with a solid medium according to any one of
[46] to
[50] , wherein, relative to 100 parts by mass of the oxygen-producing photocatalyst, the solid medium or its precursor (metal salt) is preferably greater than 0.1 parts by mass and less than 1000 parts by mass, more preferably greater than 1 part by mass and less than 500 parts by mass, and further preferably greater than 5 parts by mass and less than 100 parts by mass.
[52]
[0327] A photocatalyst composite comprising the conjugated photocatalyst according to any one of
[23] to
[42] on a substrate.
[53]
[0329] Use of the conjugated photocatalyst according to any one of
[23] to
[42] as a photocatalyst for water decomposition or a photocatalyst for organic matter decomposition.
[54]
[0331] A method for producing hydrogen, comprising irradiating the junction type photocatalyst according to any one of
[23] to
[42] or the photocatalyst complex according to
[52] with light in the presence of water or alcohol.
[0332] Example
[0333] The present invention will be specifically described below based on Examples. Unless otherwise specified, reagents manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. were used.
[0334] (Example 1)
[0335] <Bismuth vanadate (BiVO 4 ) Preparation>
[0336] Dissolve 6.06 g of bismuth nitrate pentahydrate and 1.46 g of ammonium vanadate in 50 mL of 2 mol / L nitric acid. Then, add ammonia water dropwise until the pH is 2.0, and add 0.12 g of sodium chloride to make a yellow-orange dispersion. Transfer the dispersion to a fluororesin container and react in an autoclave at 170°C for 24 hours. After the reaction is completed, separate the precipitate by suction filtration, wash the precipitate with deionized water, filter, and dry under reduced pressure. The dried sample is calcined in an electric furnace at 500°C for 2 hours to obtain a yellow powder of BiVO 4 The prepared BiVO was confirmed by SEM (JSM-IT500HR, manufactured by JEOL Ltd.) 4 The particles had a decahedral structure with the {010} plane as the basal plane. In addition, the crystal system was confirmed to be a monoclinic scheelite crystal by powder X-ray diffraction measurement (MiniFlex II diffractometer manufactured by Rigaku Corporation).
[0337] <Au-BiVO 4 Preparation>
[0338] 150 mg of the prepared BiVO 4It was added to a glass container, dispersed in 20 mL of deionized water, and 18.8 mg of tetrachloroauric acid tetrahydrate and 7.76 mL of AKYPO RLM-45NV (manufactured by Kao Corporation, sodium laureth-4.5 acetate, active ingredient 24%) were added. While stirring with a stirring blade, it was irradiated with a 300 W solar simulator (manufactured by PECCELL Corporation, PEC-L01, current value 7.5 A) for 5 minutes to cause a reaction. The irradiation light intensity at a set wavelength of 435 nm obtained by a photometer (manufactured by HIOKI E.E. Corporation, H3664) was 40 mW / cm 2 ². After the reaction was completed, the precipitate was separated by suction filtration, and the obtained precipitate was washed with deionized water and then filtered and dried under reduced pressure to obtain green powder Au-BiVO 4 . For the prepared Au-BiVO 4 particles, SEM observation was carried out. As Figure 1 shown, an image in which an Au layer was selectively formed on the {010} plane of BiVO 4 was obtained. The obtained observation image was analyzed using ImageJ, and the bonding selectivity of Au to the {010} plane of the surface of BiVO 4 was calculated to be 99%, and the coverage rate of Au on the {010} plane was 60%.
[0339] <Preparation of MPA-treated Au-BiVO 4 >
[0340] 50 mg of the prepared Au-BiVO 4 was added to a glass container, dispersed in 5 mL of deionized water, and 12 μL of 3-mercaptopropionic acid (MPA) was added. It was stirred with a stirring blade for 2 hours. After the reaction was completed, the precipitate was separated by suction filtration, and the obtained precipitate was washed with deionized water and then filtered and dried under reduced pressure to obtain green powder MPA-treated Au-BiVO 4 .
[0341] <Preparation of cation-modified Au-BiVO 4 >
[0342] 50 mg of the prepared MPA-treated Au-BiVO 4 was added to a glass container and dispersed in 1 mL of a 0.8 wt% aqueous solution of the cationic polymer Merquat 100 (manufactured by Lubrizol) (pure polymer amount 8.0 mg). It was stirred with a stirring blade for 2 hours. Thereafter, the precipitate was separated by suction filtration, and the obtained precipitate was washed with deionized water and then filtered and dried under reduced pressure to obtain green powder cation-modified Au-BiVO 4。The volume particle size distribution in water of the obtained cation-modified Au-BiVO was evaluated using laser diffraction scattering measurement (LA960 manufactured by Horiba, Ltd.), and the results are as 4 shown below. Figure 3 所示。
[0343] <Preparation of Ru-supported SrTiO 3 >
[0344] 120 mg of SrTiO 3 (manufactured by Kanto Chemical Co., Inc.) was added to a glass container, dispersed in 160 mL of deionized water, 2.2 mg of ruthenium chloride n-hydrate was added, and ultrasonic dispersion treatment was performed for 15 minutes. 20 mL of methanol was added to the obtained dispersion, and while bubbling with argon at 20 mL / min for 60 minutes, light irradiation was performed with a 300 W xenon lamp for 120 minutes to cause a reaction, and Ru was supported on SrTiO 3 . After completion of the reaction, the precipitate was separated by suction filtration, the obtained precipitate was washed with deionized water, filtered, and dried under reduced pressure to obtain gray powder of Ru-supported SrTiO 3 .
[0345] <Preparation of anion-modified Ru-supported SrTiO 3 >
[0346] 100 mg of the prepared Ru-supported SrTiO 3 was added to a glass container and dispersed in 1.13 mL (0.05 g of pure polymer amount) of a 4 mass% aqueous solution of Poiz 520 (weight average molecular weight: 21,000, copolymer of sodium acrylate / sodium maleate, manufactured by Kao Corporation) as an anionic polymer, and ultrasonic irradiation was performed for 30 minutes. Thereafter, the dispersion was suction-filtered, and the solid matter was recovered. After washing the recovered matter with deionized water, it was filtered and dried under reduced pressure to obtain gray powder of anion-modified Ru-supported SrTiO 3 . The volume particle size distribution in water of the obtained anion-modified Ru-supported SrTiO 3 was evaluated, and the results are as Figure 3 shown below.
[0347] <Preparation of bonded photocatalyst>
[0348] 50 mg of the prepared cation-modified Au-BiVO 4 and 5 mg of anion-modified Ru-supported SrTiO 3 were added to a glass container and dispersed in 1 mL of deionized water. After stirring for 30 minutes, it was allowed to stand, and it was observed that all the particles in the dispersion settled. The volume particle size distribution of the obtained particles was measured, and the results are as Figure 3 shown below. From Ru-supported SrTiO 3The particle components do not exist alone, confirming that Au-BiVO 4 With Ru supported SrTiO 3 The particles (joined particles) were coated on a silicon substrate and then dried and observed by SEM. Figure 2 As shown, the BiVO 3 Ru-supported SrTiO is formed on the Au formed on the {010} surface. 4 The observed images were analyzed using ImageJ to calculate the Au to BiVO 3 The bonding selectivity of the surface to the {010} plane was 99%, and the coverage of Au on the {010} plane was 60%.
[0349] <Evaluation of Water-Splitting Activity of Junction-Type Photocatalyst>
[0350] The obtained bonded particles were added to 180 mL of water, bubbled with argon at 20 mL / min for 30 minutes, and then illuminated with a 300 W xenon lamp. The generated gas was analyzed by a gas chromatograph with a TCD detector. The illumination was continued for 5 hours, and the average hydrogen production rate was calculated. The results are shown in Table 1.
[0351] (Comparative Example 1)
[0352] In the preparation of Au-BiVO 4 When the Au-BiVO was prepared, 0.36 mL of methanol was added as a hole sacrificial reagent (auxiliary agent) instead of AKYPORLM-45NV. 4 3-mercaptopropionic acid treatment and cation modification were performed, and Ru-supported SrTiO 3 A sample was prepared in the same manner as in Example 1 except for the above. Figure 4 It shows that Ru supports SrTiO 3 and Au-BiVO 4 Volume particle size distribution results of the mixed samples. Au-BiVO 4 The volume particle size distribution of the sample showed a distribution in the unobserved region of 1 to 5 μm, indicating that the mixed sample was not uniformly composited, and part of Ru supported SrTiO 3 Suspension.
[0353] (Example 2)
[0354] When preparing the junction type photocatalyst, Au-BiVO 4 3-mercaptopropionic acid treatment and cation modification were performed without Ru-supported SrTiO 3 A conjugated photocatalyst was prepared by the same operation as in Example 1 except for the anion modification.
[0355] (Example 3)
[0356] In the preparation of Au-BiVO 4 A junction-type photocatalyst was prepared by the same operation as in Example 1 except that 1.55 mL of FR-14 (manufactured by Kao Corporation) was added as potassium oleate instead of AKYPO RLM-45NV.
[0357] (Example 4)
[0358] <Cation-modified Ru supported SrTiO 3 Preparation>
[0359] The anion-modified Ru prepared in the same manner as in Example 1 was loaded onto SrTiO 3 50 mg of the powder was dispersed in 1 mL of a 0.8 mass % aqueous solution of Merquat 100 (manufactured by Lubrizol) as a cationic polymer (pure polymer amount 8.0 mg), and stirred for 10 minutes with a stirring plate. After the reaction was completed, the precipitate was separated by suction filtration. The obtained precipitate was washed with deionized water and dried under reduced pressure to obtain a gray powder of cation-modified Ru-supported SrTiO 3 .
[0360] <Preparation of Junction-Type Photocatalyst>
[0361] As in Example 1, 50 mg of the prepared MPA-treated Au-BiVO 4 , 5mg cation modified Ru supported SrTiO 3 , dispersed in 1 mL of deionized water and stirred for 30 minutes, thereby preparing a conjugated photocatalyst.
[0362] (Example 5)
[0363] In the preparation of Au-BiVO 4 A junction-type photocatalyst was prepared by the same operation as in Example 1 except that the light irradiation was performed at a current value of 8.0 A for 8 minutes.
[0364] (Example 6)
[0365] <Cation-modified Ru supported SrTiO 3 Preparation>
[0366] The Ru-supported SrTiO prepared in the same manner as in Example 1 was 350 mg of the powder was dispersed in 1 mL of a 0.8 mass % aqueous solution of Merquat 100 (manufactured by Lubrizol) as a cationic polymer (pure polymer amount 8.0 mg), and ultrasonic irradiation was performed for 30 minutes. Thereafter, the dispersion was filtered to recover the solid. The recovered product was washed with deionized water, filtered, and dried under reduced pressure to obtain a gray powder of cation-modified Ru-supported SrTiO 3 .
[0367] <Preparation of Junction-Type Photocatalyst>
[0368] As in Example 1, 50 mg of the prepared MPA-treated Au-BiVO 4 , 5mg cation modified Ru supported SrTiO 3 , dispersed in 1 mL of deionized water and stirred for 30 minutes, thereby preparing a conjugated photocatalyst.
[0369] (Example 7)
[0370] In the preparation of Au-BiVO 4 When the light was irradiated for 3 minutes at a current value of 8.0 A. Except for this, the same operation as in Example 6 was followed to prepare a junction type photocatalyst.
[0371] For Examples 1 to 7 and Comparative Example 1, Au was used to bond BiVO 4 Table 1 shows the calculation results of the bonding selectivity to the {010} plane of the surface, the coverage of Au on the {010} plane, and the evaluation results of the water decomposition activity.
[0372] It should be noted that the obtained SEM images were analyzed according to the following steps: The image analysis software used was a compression package FIJI developed based on ImageJ (National Institutes of Health, USA).
[0373] Au for BiVO 4 Calculation method of bonding selectivity toward {010} plane on the surface
[0374] 1. Randomly cut out 10 areas corresponding to the {010} plane from the SEM image and obtain 10 cropped image data.
[0375] 2. Randomly cut out 10 areas corresponding to the {110} and {011} planes from the SEM image, and obtain 10 images of cut-out image data.
[0376] 3. Run the Trainable Weka Segmentation (TWS) function on all image data, specifying Au and BiVO 4 And the background part of these three areas.
[0377] 4. Conduct 3 types of learning through TWS.
[0378] 5. As classified image data, output 10 images of {010} surfaces, 10 images of {110} surfaces, and 10 images of {011} surfaces.
[0379] 6. Based on the image data of the Au region output by TWS classification, the Au coating area on the {010} plane and the Au coating area on the {110} and {011} planes are calculated using the Area value in the Analyze Particles function.
[0380] 7. The junction selectivity (%) was calculated based on: Au coating area on {010} plane / (Au coating area on {010} plane + Au coating area on {110} and {011} planes)×100, and obtained as the average value of 10 images.
[0381] Calculation method of Au coverage on {010} surface
[0382] Ten regions corresponding to the {010} plane were randomly cut out from the SEM image, and 10 images of cut-out image data were obtained.
[0383] 2. Run the Trainable Weka Segmentation (TWS) function on all image data, specifying Au, BiVO 4 And the background part of these three areas.
[0384] 3. Conduct 3 types of learning through TWS.
[0385] 4. Output 10 classified image data.
[0386] 5. Calculate the area of the {010} plane using the Area value in the Analyze Particles function of the cropped image data. Calculate the Au coating area using the Area value in the same function based on the image data of the Au region output by TWS classification.
[0387] 6. Calculated based on coverage (%) = Au coverage area / {010} plane area × 100, and obtained as an average value of 10 images.
[0388] [Table 1]
[0389]
[0390] The evaluation results in Table 1 confirm that the use of organic carboxylic acid compounds can increase the coverage of the solid medium relative to the electron capture surface area of the oxygen-producing photocatalyst. The conjugated photocatalysts of Examples 1 to 7, in which the coverage of the solid medium relative to the electron capture surface area of the oxygen-producing photocatalyst is 42 to 98%, have superior water decomposition activity compared to the conjugated photocatalyst of Comparative Example 1, in which the coverage is 7%.
[0391] Industrial Applicability
[0392] The junction-type photocatalyst of the present invention is useful as a photocatalyst for decomposing water or organic matter.
Claims
1. A method for producing a junction type photocatalyst, which is a method for producing a junction type photocatalyst having a solid medium between a hydrogen-producing photocatalyst and an oxygen-producing photocatalyst, The method for producing the junction type photocatalyst comprises the following steps 1: Step 1: A step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation supporting method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
2. The method for producing a junction-type photocatalyst according to claim 1, wherein: In the step 1, when the photoelectric deposition method is used, the step includes irradiating light to a dispersion liquid containing an oxygen-generating photocatalyst in addition to the organic carboxylic acid compound and the solid medium or a precursor thereof.
3. The method for producing a junction-type photocatalyst according to claim 1 or 2, wherein: The organic carboxylic acid compound is at least one selected from the group consisting of ether carboxylic acids, fatty acids, hydroxymonocarboxylic acids, and polycarboxylic acids.
4. The method for producing a junction-type photocatalyst according to any one of claims 1 to 3, wherein: The organic carboxylic acid compound comprises an ether carboxylic acid, and the solid medium comprises gold.
5. The method for producing a junction-type photocatalyst according to any one of claims 1 to 4, further comprising the following steps 2 to 4, wherein: Process 2 and process 3 are not sequential. Step 2: a step of introducing an ionic group into the solid medium to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic group. Step 3: a step of introducing an ionic polymer having a charge opposite to that of the ionic group into the hydrogen-generating photocatalyst, Step 4: A step of mixing the oxygen-generating photocatalyst obtained in step 2 to which the solid medium having the ionic group is bonded and the hydrogen-generating photocatalyst obtained in step 3 to which the ionic polymer is introduced.
6. The method for producing a junction-type photocatalyst according to any one of claims 1 to 4, further comprising the following steps 2', 3' and 4', wherein: Process 2' and process 3' are not sequential. Step 2': a step of introducing an ionic group into the solid medium, and then reacting an ionic polymer having a charge opposite to that of the ionic group with the ionic group to obtain an oxygen-generating photocatalyst bonded to the solid medium having the ionic polymer. Step 3': a step of introducing an ionic polymer having a charge opposite to that of the ionic polymer into the hydrogen-generating photocatalyst, Step 4': a step of mixing the oxygen-generating photocatalyst obtained in step 2' and bonded with the solid medium having the ionic polymer, and the hydrogen-generating photocatalyst introduced with the ionic polymer obtained in step 3'.
7. The method for producing a junction-type photocatalyst according to claim 5 or 6, wherein: When an ionic group is introduced into the solid medium in the step 2 or the step 2', a mercapto compound having an ionic group is used.
8. The method for producing a junction-type photocatalyst according to any one of claims 1 to 7, wherein: The coverage rate of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more.
9. A junction type photocatalyst having a solid medium between a hydrogen-generating photocatalyst and an oxygen-generating photocatalyst, The coverage rate of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more.
10. The junction-type photocatalyst according to claim 9, wherein The bonding selectivity of the solid medium to the electron capturing surface of the oxygen-generating photocatalyst is 60% or more.
11. The junction-type photocatalyst according to claim 9 or 10, wherein The solid medium and the hydrogen-generating photocatalyst are bonded via an ionic polymer.
12. The junction-type photocatalyst according to claim 9 or 10, wherein The solid medium has an ionic group, and the solid medium and the hydrogen-generating photocatalyst are bonded via an ionic polymer having a charge opposite to that of the ionic group.
13. A method for producing an oxygen-generating photocatalyst bonded with a solid medium, comprising the step of bonding the solid medium to the oxygen-generating photocatalyst by at least one method selected from the group consisting of a photoelectrochemical deposition method, an impregnation support method, and a precipitation method using an organic carboxylic acid compound and a solid medium or a precursor thereof.
14. The method for producing an oxygen-generating photocatalyst bonded with a solid medium according to claim 13, wherein: When the photoelectric deposition method is used, the method includes irradiating light to a dispersion liquid containing an oxygen-generating photocatalyst in addition to the organic carboxylic acid compound and the solid medium or a precursor thereof.
15. The method for producing an oxygen-generating photocatalyst bonded with a solid medium according to claim 13 or 14, wherein: The organic carboxylic acid compound is at least one selected from the group consisting of ether carboxylic acids, fatty acids, hydroxymonocarboxylic acids, and polycarboxylic acids.
16. The method for producing an oxygen-generating photocatalyst bonded with a solid medium according to any one of claims 13 to 15, wherein: The organic carboxylic acid compound comprises an ether carboxylic acid, The solid medium comprises gold.
17. The method for producing an oxygen-generating photocatalyst bonded with a solid medium according to any one of claims 13 to 16, wherein: The coverage rate of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more.
18. An oxygen-generating photocatalyst bonded with a solid medium, wherein: The coverage rate of the solid medium with respect to the electron capture surface area of the oxygen-generating photocatalyst is 40% or more.
19. The oxygen-generating photocatalyst bonded with a solid medium according to claim 18, wherein: The bonding selectivity of the solid medium to the electron capturing surface is 60% or more. 20 . A photocatalyst composite comprising the conjugated photocatalyst according to claim 9 on a substrate.
21. Use of the conjugated photocatalyst according to any one of claims 9 to 12 as a photocatalyst for water decomposition or a photocatalyst for organic matter decomposition.
22. A method for producing hydrogen, comprising irradiating light to the junction type photocatalyst according to any one of claims 9 to 12 or the photocatalyst composite according to claim 20 in the presence of water or alcohol.