Fluorine-containing copolymer

By adjusting the composition and process parameters of the fluorinated copolymer, the wear resistance and durability of the wafer carrier were solved, achieving excellent performance and low fluoride ion leaching under high temperature and high pressure conditions, making it suitable for the efficient manufacture of aesthetically pleasing injection-molded parts.

CN118946602APending Publication Date: 2024-11-12DAIKIN INDUSTRIES LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380029065.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-26
Filing Date
2023-03-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing fluorinated copolymers, when used in wafer carriers, lack sufficient resistance to abrasion, ozone, and solvent cracking, and are prone to wear and strength reduction during repeated use.

Method used

By adjusting the content of hexafluoropropylene units and fluoroalkyl vinyl ether units in the fluorinated copolymer, controlling the melt flow rate and the number of functional groups, and optimizing the molding conditions, a copolymer containing tetrafluoroethylene, hexafluoropropylene, and fluoroalkyl vinyl ether units is formed.

Benefits of technology

It improves the aesthetics and durability of injection molding, enhances wear resistance at 105℃, high-temperature rigidity at 97.5℃, creep resistance, ozone resistance and solvent cracking resistance, and reduces fluoride ion leaching, making it suitable for use in high-temperature and chemical environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051938530000071
    Figure BDA0005051938530000071
  • Figure BDA0005051938530000201
    Figure BDA0005051938530000201
  • Figure BDA0005051938530000261
    Figure BDA0005051938530000261
Patent Text Reader

Abstract

Provided is a fluorine-containing copolymer containing tetrafluoroethylene units, hexafluoropropylene units, and fluoro (alkyl vinyl ether) units, in which the content of hexafluoropropylene units is 11.2-13.2 mass% with respect to the total monomer units, and the content of fluoro (alkyl vinyl ether) units is 11.2-13.2 mass% with respect to the total monomer units. The content of fluoro (alkyl vinyl ether) units is 0-0.4 mass% with respect to the total monomer units, the melt flow rate at 372 DEG C is 10.0-17.0 g / 10 minutes, and the total number of-CF2H, carbonyl group-containing terminal groups,-CF2, and-CH2OH is 90 or less with respect to the number of carbon atoms per 106 main chains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to fluorine-containing copolymers. Background Art

[0002] Patent Document 1 describes a fluorinated copolymer having copolymer units derived from tetrafluoroethylene [TFE] and copolymer units derived from hexafluoropropylene [HFP], which is characterized by exhibiting the following properties (a) and (b).

[0003] (a) The melting point of the thermal melting curve obtained by a single heating by differential scanning calorimetry is within the range of 240°C to 280°C, and the melting point peak area accounts for 60% or more of the melting heat area.

[0004] (b) The product of MFR (g / 10 minutes) and resin pressure (MPa) is 40 or less.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2008 / 047759 Summary of the invention

[0008] Problems to be solved by the invention

[0009] An object of the present invention is to provide a fluorine-containing copolymer which can be molded at a high injection speed by an injection molding method to obtain a beautiful injection-molded body, and can obtain a molded body which has excellent abrasion resistance at 105°C, rigidity at a high temperature of 97.5°C, creep resistance, durability against repeated loads, tensile creep resistance at 105°C, ozone resistance, solvent crack resistance, ductility to a tensile force applied at 125°C, and is not prone to elution of fluorine ions into a chemical solution such as hydrogen peroxide.

[0010] Means for solving problems

[0011] According to the present invention, there is provided a fluorinated copolymer, which is a fluorinated copolymer containing tetrafluoroethylene units, hexafluoropropylene units and fluoro(alkyl vinyl ether) units, wherein the content of the hexafluoropropylene units is 11.2% by mass to 13.2% by mass relative to all monomer units, the content of the fluoro(alkyl vinyl ether) units is 0% by mass to 0.4% by mass relative to all monomer units, the melt flow rate at 372°C is 10.0g / 10min to 17.0g / 10min, and the total amount of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH is relative to every 10 6 The number of carbon atoms in the main chain is less than 90.

[0012] Effects of the Invention

[0013] According to the present invention, there can be provided a fluorine-containing copolymer which can be molded at a high injection speed by an injection molding method to obtain a beautiful injection-molded body, and can obtain a molded body which has excellent wear resistance at 105°C, rigidity at a high temperature of 97.5°C, creep resistance, durability against repeated loads, tensile creep resistance at 105°C, ozone resistance, solvent crack resistance, ductility to a tensile force applied at 125°C, and is not prone to elution of fluorine ions into a chemical solution such as hydrogen peroxide. DETAILED DESCRIPTION

[0014] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0015] The fluorine-containing copolymer of the present invention contains tetrafluoroethylene (TFE) units, hexafluoropropylene (HFP) units and fluoro(alkyl vinyl ether) (FAVE) units.

[0016] Fluororesins are used as a material for forming wafer carriers because of their excellent chemical resistance. However, when the fluorinated copolymer described in Patent Document 1 is used as a material for forming wafer carriers, the durability to ozone and concentrated hydrochloric acid is not sufficient, and there is a problem of cracking. In addition, during repeated use of the wafer carrier, there is also a problem of abrasion or reduction in strength of the wafer carrier. Therefore, it is required to improve the wear resistance and durability to repeated loads of the wafer carrier.

[0017] It was found that by adjusting the content of HFP units and FAVE units, melt flow rate and number of functional groups of the fluorinated copolymer containing TFE units, HFP units and FAVE units to an extremely limited range, the injection moldability of the fluorinated copolymer is significantly improved, and by using such a fluorinated copolymer, it is possible to obtain a molded body with excellent wear resistance at 105°C, rigidity at high temperature of 97.5°C, creep resistance, durability to repeated loads, tensile creep resistance at 105°C, ozone resistance, solvent crack resistance, ductility to tensile force applied at 125°C, and difficulty in eluting fluorine ions into a liquid such as hydrogen peroxide. Therefore, by using the fluorinated copolymer of the present invention, injection molded bodies such as large wafer carriers with thin-walled parts can be beautifully manufactured with high productivity. Furthermore, by using the disclosed fluorinated copolymer, a molded body that is not easy to crack, not easy to wear, and not easy to reduce strength even in contact with ozone and concentrated hydrochloric acid can be obtained.

[0018] The fluorinated copolymer of the present invention is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using existing processing machines such as an extruder and an injection molding machine.

[0019] Examples of FAVE constituting the FAVE unit include those selected from the general formula (1):

[0020] CF2=CFO(CF2CFY 1 O) p -(CF2CF2CF2O) q -Rf (1)

[0021] (Where Y 1 represents F or CF3, Rf represents a perfluoroalkyl group having 1 to 5 carbon atoms, p represents an integer of 0 to 5, and q represents an integer of 0 to 5. ) and the general formula (2):

[0022] CFX=CXOCF2OR 1 (2)

[0023] (wherein, X is the same or different and represents H, F or CF3, R 1 It represents a linear or branched fluoroalkyl group having 1 to 6 carbon atoms which may contain 1 to 2 atoms of at least one kind selected from the group consisting of H, Cl, Br and I, or a cyclic fluoroalkyl group having 5 or 6 carbon atoms which may contain 1 to 2 atoms of at least one kind selected from the group consisting of H, Cl, Br and I. At least one of the group consisting of monomers represented by ).

[0024] Among them, as the above-mentioned FAVE, the monomer represented by the general formula (1) is preferred, more preferably at least one selected from the group consisting of perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether) (PEVE) and perfluoro(propyl vinyl ether) (PPVE), further preferably at least one selected from the group consisting of PEVE and PPVE, and particularly preferably PPVE.

[0025] The content of the HFP unit in the fluorinated copolymer is 11.2% to 13.2% by mass relative to the total monomer units, preferably 11.3% by mass or more, more preferably 11.4% by mass or more, further preferably 11.5% by mass or more, preferably 13.1% by mass or less, more preferably 13.0% by mass or less, further preferably 12.9% by mass or less, further preferably 12.8% by mass or less, particularly further preferably 12.7% by mass or less, particularly preferably 12.6% by mass or less, and most preferably 12.5% ​​by mass or less. When the content of the HFP unit is too small, a molded product having excellent abrasion resistance at 105°C, ozone resistance, solvent crack resistance, and ductility to a tensile force applied at 125°C cannot be obtained. When the content of the HFP unit is too large, a molded product having excellent rigidity at a high temperature of 97.5°C, creep resistance, durability to repeated loads, and tensile creep resistance at 105°C cannot be obtained.

[0026] The content of the FAVE unit of the fluorinated copolymer is 0% to 0.4% by mass relative to all monomer units, preferably 0.3% by mass or less, further preferably 0.2% by mass or less, and particularly preferably 0.1% by mass or less. By making the content of the FAVE unit within the above range, a molded body having excellent wear resistance at 105°C, rigidity at 97.5°C, creep resistance, durability to repeated loads, tensile creep resistance at 105°C, ozone resistance, and solvent crack resistance can be obtained. When the content of the FAVE unit is too much, a molded body having excellent rigidity at 97.5°C, creep resistance, and tensile creep resistance at 105°C can not be obtained.

[0027] The content of the TFE unit of the fluorinated copolymer is preferably 86.3% by mass or more relative to all monomer units, more preferably 86.5% by mass or more, further preferably 86.7% by mass or more, further preferably 87.0% by mass or more, particularly preferably 87.3% by mass or more, most preferably 87.4% by mass or more, preferably 88.8% by mass or less, more preferably 88.7% by mass or less, further preferably 88.6% by mass or less, further preferably 88.5% by mass or less. In addition, the content of the TFE unit can be selected so that the total content of the HFP unit, the FAVE unit, the TFE unit and other monomer units is 100% by mass.

[0028] The fluorinated copolymer of the present invention may contain the above three monomer units, and may be a copolymer containing only the above three monomer units or a copolymer containing the above three monomer units and other monomer units.

[0029] The other monomer is not particularly limited as long as it is a monomer copolymerizable with TFE, HFP and FAVE, and may be a fluorine-containing monomer or a non-fluorine-containing monomer.

[0030] The fluorine-containing monomer is preferably selected from the group consisting of chlorotrifluoroethylene, vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoroisobutylene, CH2=CZ 1 (CF2) n Z 2 (Where Z 1 H or F, Z 2 is H, F or Cl, n is an integer from 1 to 10), CF2=CF-O-CH2-Rf 2 (Where Rf 2 At least one selected from the group consisting of an alkyl perfluorovinyl ether derivative represented by a perfluoroalkyl group having 1 to 5 carbon atoms, perfluoro-2,2-dimethyl-1,3-dioxole [PDD], and perfluoro-2-methylene-4-methyl-1,3-dioxolane [PMD].

[0031] As CH2=CZ 1 (CF2) n Z 2 The monomers shown include CH2=CFCF3, CH2=CH-C4F9, CH2=CH-C6F 13 , CH2=CF-C3F6H, etc.

[0032] As non-fluorine-containing monomers, hydrocarbon monomers that can be copolymerized with TFE, HFP and FAVE can be cited. As hydrocarbon monomers, for example, olefins such as ethylene, propylene, butylene, and isobutylene can be cited; alkyl vinyl ethers such as ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, and cyclohexyl vinyl ether can be cited; vinyl acetate, vinyl propionate, vinyl n-butyrate, vinyl isobutyrate, vinyl valerate, vinyl pivalate, vinyl hexanoate, vinyl octanoate, vinyl decanoate, vinyl versatate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl benzoate, vinyl p-tert-butylbenzoate, vinyl cyclohexanecarboxylate, vinyl monochloroacetate , vinyl adipate, vinyl acrylate, vinyl methacrylate, vinyl crotonate, vinyl sorbate, vinyl cinnamate, vinyl undecylenate, vinyl hydroxyacetate, vinyl hydroxypropionate, vinyl hydroxybutyrate, vinyl hydroxyvalerate, vinyl hydroxyisobutyrate, vinyl hydroxycyclohexanecarboxylate and other vinyl esters; alkyl allyl ethers such as ethyl allyl ether, propyl allyl ether, butyl allyl ether, isobutyl allyl ether, cyclohexyl allyl ether; alkyl allyl esters such as ethyl allyl ester, propyl allyl ester, butyl allyl ester, isobutyl allyl ester, cyclohexyl allyl ester, etc.

[0033] As a non-fluorine-containing monomer, it can also be a hydrocarbon monomer containing a functional group that can be copolymerized with TFE, HFP and FAVE. As a hydrocarbon monomer containing a functional group, for example, hydroxyalkyl vinyl ethers such as hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxyisobutyl vinyl ether, and hydroxycyclohexyl vinyl ether can be cited; non-fluorine-containing monomers having a glycidyl group such as glycidyl vinyl ether and glycidyl allyl ether; non-fluorine-containing monomers having an amino group such as aminoalkyl vinyl ether and aminoalkyl allyl ether; non-fluorine-containing monomers having an amide group such as (methyl) acrylamide and hydroxymethyl acrylamide; bromine-containing olefins, iodine-containing olefins, bromine-containing vinyl ethers, iodine-containing vinyl ethers; non-fluorine-containing monomers having a nitrile group, etc.

[0034] The content of other monomer units in the fluorinated copolymer of the present invention is preferably 0 to 2.5 mass % based on all monomer units, more preferably 1.0 mass % or less, further preferably 0.5 mass % or less, particularly preferably 0.1 mass % or less.

[0035] The melt flow rate (MFR) of the fluorinated copolymer is 10.0 g / 10 minutes to 17.0 g / 10 minutes, preferably 10.1 g / 10 minutes or more, more preferably 10.5 g / 10 minutes or more, further preferably 12.0 g / 10 minutes or more, further preferably 12.5 g / 10 minutes or more, particularly preferably 13.0 g / 10 minutes or more, and most preferably 13.5 g / 10 minutes or more, preferably 16.5 g / 10 minutes or less, more preferably 15.0 g / 10 minutes or less, further preferably 14.5 g / 10 minutes or less, particularly preferably 14.0 g / 10 minutes or less, and most preferably 13.5 g / 10 minutes or less. If the MFR is too low, a molded body having excellent rigidity at a high temperature of 97.5° C. cannot be obtained, and a beautiful injection molded body cannot be obtained by molding at a high injection speed by injection molding. When the MFR is too high, a molded product excellent in abrasion resistance at 105° C., durability against repeated loads, ozone resistance, solvent crack resistance, and ductility against a tensile force applied at 125° C. cannot be obtained.

[0036] In the present invention, the melt flow rate is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a die having an inner diameter of 2 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D-1238.

[0037] The MFR can be adjusted by adjusting the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, etc., used when polymerizing the monomers.

[0038] The fluorinated copolymer has a relative 6 The total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH with the number of main chain carbon atoms is 90 or less. The total number of these functional groups is preferably 80 or less, 70 or less, 60 or less, 50 or less, 40 or less, 30 or less, 25 or less, or less than 21. By making the total number of these functional groups within the above range, a molded body with excellent ozone resistance and less fluoride ion dissolution into a liquid such as hydrogen peroxide can be obtained.

[0039] Examples of carbonyl-containing terminal groups include -COF, -COOH, -COOR (R is an alkyl group), -CONH2, and -O(C=O)OR (R is an alkyl group). The type of the alkyl group (R) possessed by -COOR and -O(C=O)OR is determined by the polymerization initiator and chain transfer agent used in the manufacture of the fluorinated copolymer, and is, for example, an alkyl group having 1 to 6 carbon atoms such as -CH3.

[0040] The identification of the types of the functional groups and the measurement of the number of the functional groups can be performed using infrared spectroscopy.

[0041] The number of functional groups is specifically determined by the following method. First, the fluorinated copolymer is formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the fluorinated copolymer and a differential spectrum from a background spectrum of a fully fluorinated copolymer without functional groups. The number of functional groups in the fluorinated copolymer relative to each 1×10 6 The number of functional groups N per carbon atom.

[0042] N=I×K / t(A)

[0043] I: Absorbance

[0044] K: Correction coefficient

[0045] t: film thickness (mm)

[0046] For reference, absorption frequencies, molar absorption coefficients, and correction coefficients for some functional groups are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low-molecular model compounds.

[0047] [Table 1]

[0048] Table 1

[0049]

[0050] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are several tens of kaise (cm2) lower than the absorption frequencies of -CF2H, -COF, free -COOH, and bound -COOH, -COOCH3, and -CONH2 shown in the table, respectively. -1 ).

[0051] For example, the functional group number of -COF is the absorption frequency 1883 cm due to -CF2COF. -1 The number of functional groups obtained from the absorption peak at 1840 cm-1 due to -CH2COF -1 The total number of functional groups found from the absorption peak at .

[0052] Alternatively, the number of -CF2H groups can be measured using a nuclear magnetic resonance apparatus at a temperature of (melting point of the polymer + 20)°C. 19 In F-NMR measurement, it was determined from the peak integral value of -CF2H group.

[0053] Functional groups such as -CF2H groups are functional groups present at the main chain ends or side chain ends of the fluorinated copolymer and functional groups present in the main chain or in the side chain. These functional groups are introduced into the fluorinated copolymer, for example, by a chain transfer agent or a polymerization initiator used when manufacturing the fluorinated copolymer. For example, when an alcohol is used as a chain transfer agent or a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced into the main chain ends of the fluorinated copolymer. In addition, by polymerizing a monomer having a functional group, the above-mentioned functional group is introduced into the side chain ends of the fluorinated copolymer.

[0054] By subjecting the fluorinated copolymer having such functional groups to a wet heat treatment, a fluorination treatment, or the like, a fluorinated copolymer having the number of functional groups within the above range can be obtained. The fluorinated copolymer of the present invention is preferably subjected to a wet heat treatment or a fluorination treatment, and more preferably to a fluorination treatment. The fluorinated copolymer of the present invention also preferably has a -CF3 terminal group.

[0055] The melting point of the fluorinated copolymer is preferably 220° C. to 290° C., more preferably 240° C. to 280° C. When the melting point is within the above range, a more beautiful injection molded body can be obtained by molding at a high injection speed by injection molding, and a molded body with better wear resistance at 105° C., rigidity at a high temperature of 97.5° C., creep resistance, durability against repeated loads, tensile creep resistance at 105° C., ozone resistance, solvent crack resistance, ductility against a tensile force applied at 125° C., and less prone to elution of fluoride ions into a chemical solution can be obtained.

[0056] In the present invention, the melting point can be measured using a differential scanning calorimeter [DSC].

[0057] The amount of fluorine ions released from the fluorinated copolymer of the present invention as detected in an immersion test in hydrogen peroxide water is preferably 4.0 ppm or less, more preferably 3.0 ppm or less, and further preferably 2.8 ppm or less, based on mass.

[0058] In the present invention, the immersion test in hydrogen peroxide can be carried out as follows: using a fluorinated copolymer, a test piece having a weight equivalent to 10 pieces of a molded body (15 mm × 15 mm × 0.2 mm) is prepared, and a polypropylene bottle containing the test piece and 15 g of a 3 mass % hydrogen peroxide solution is placed in a constant temperature bath at 95°C and left for 20 hours.

[0059] The fluorinated copolymer of the present invention can also be produced by any polymerization method such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. In these polymerization methods, various conditions such as temperature and pressure, polymerization initiator, chain transfer agent, solvent, and other additives can be appropriately set according to the desired composition and amount of the fluorinated copolymer.

[0060] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical initiator can be used.

[0061] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:

[0062] Dialkyl peroxycarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate and di-sec-butyl peroxydicarbonate;

[0063] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;

[0064] Dialkyl peroxides such as di-tert-butyl peroxide;

[0065] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.

[0066] Examples of the di[fluoro(or fluorochloro)acyl]peroxides include diacyl peroxides represented by [(RfCOO)-]2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).

[0067] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydroperfluorohexanoyl)peroxide, di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetrafluorooctanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluorovaleranoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, and di(ω-chloro-hexafluorobutyryl)peroxide. , di(ω-chloro-decafluorohexanoyl)peroxide, di(ω-chloro-tetrafluorooctanoyl)peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutyryl)peroxide, di(trichlorooctafluorohexanoyl)peroxide, di(tetrachloroundecanoyl)peroxide, di(pentachlorotetrafluorodecanoyl)peroxide, di(undecachlorotriacontanoyl)peroxide, and the like.

[0068] As the water-soluble free radical polymerization initiator, it can be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., tert-butyl peroxymaleate, tert-butyl hydroperoxide, etc. It can also contain a reducing agent such as sulfites, and its amount can be 0.1 to 20 times that of the peroxide.

[0069] If an oil-soluble free radical polymerization initiator is used as a polymerization initiator, the generation of -COF and -COOH can be avoided, and the total number of -COF and -COOH of the fluorinated copolymer can be easily adjusted to the above range, so it is preferred. In addition, if an oil-soluble free radical polymerization initiator is used, it is also easy to adjust the total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH to the above range. In particular, it is preferred to manufacture the fluorinated copolymer by suspension polymerization using an oil-soluble free radical polymerization initiator. As an oil-soluble free radical polymerization initiator, it is preferred to select at least one of the groups consisting of dialkyl peroxycarbonates and di[fluorine (or chlorofluoride) acyl] peroxides, and more preferably at least one of the groups consisting of di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate and di(ω-hydrogen-dodecanoyl) peroxide.

[0070] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol, ethanol, and 2,2,2-trifluoroethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane; 3-fluorobenzotrifluoride, etc. The amount added can vary depending on the chain transfer constant of the compound used, and is usually used in the range of 0.01 to 20 parts by mass relative to 100 parts by mass of the solvent.

[0071] For example, when dialkyl peroxycarbonates, di[fluoro(or chlorofluoro)acyl]peroxides, etc. are used as polymerization initiators, the molecular weight of the obtained fluorinated copolymer becomes too high, and it is sometimes difficult to adjust the desired melt flow rate, but a chain transfer agent can be used to adjust the molecular weight. It is particularly preferred to manufacture the fluorinated copolymer by suspension polymerization using a chain transfer agent such as alcohols and an oil-soluble free radical polymerization initiator.

[0072] Examples of the solvent include water, a mixed solvent of water and alcohol, etc. Alternatively, the monomer used for polymerization of the fluorinated copolymer of the present invention may be used as the solvent.

[0073] In suspension polymerization, in addition to water, fluorine-based solvents can also be used. As fluorine-based solvents, hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, CF2ClCF2CFHCl, etc.; chlorofluoroalkanes such as CF2ClCFClCF2CF3, CF3CFClCFClCF3, etc.; perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, CF3CF2CF2CF2CF2CF3, etc. perfluoroalkanes, etc., among which perfluoroalkanes are preferred. From the aspects of suspensibility and economy, the amount of fluorine-based solvent used is preferably 10 to 100 parts by mass relative to 100 parts by mass of the solvent.

[0074] The polymerization temperature is not particularly limited and may be 0° C. to 100° C. In addition, when the decomposition rate of the polymerization initiator is too fast, such as when dialkyl peroxycarbonates, di[fluoro(or chlorofluoro)acyl]peroxides, etc. are used as the polymerization initiator, it is preferred to adopt a relatively low polymerization temperature such as a range of 0° C. to 35° C.

[0075] The polymerization pressure is appropriately determined according to other polymerization conditions such as the type of solvent used, the amount of solvent, the vapor pressure, the polymerization temperature, etc., and can generally be 0 MPaG to 9.8 MPaG. The polymerization pressure is preferably 0.1 MPaG to 5 MPaG, more preferably 0.5 MPaG to 2 MPaG, and further preferably 0.5 MPaG to 1.5 MPaG. In addition, when the polymerization pressure is 1.5 MPaG or more, the production efficiency can be improved.

[0076] As the additive in the polymerization, for example, a suspension stabilizer can be cited. As a suspension stabilizer, as long as it is an existing known suspension stabilizer, there is no particular limitation, and methylcellulose, polyvinyl alcohol, etc. can be used. If a suspension stabilizer is used, the suspended particles generated by the polymerization reaction are stably dispersed in the aqueous medium, so even if a reaction tank made of SUS that is not subjected to anti-adhesion treatments such as glass lining is used, the suspended particles are not easily attached to the reaction tank. Therefore, a reaction tank that withstands high pressure can be used, so polymerization under high pressure can be carried out, and production efficiency can be improved. In contrast, when polymerization is carried out without using a suspension stabilizer, if a reaction tank made of SUS that is not subjected to anti-adhesion treatment is used, the suspended particles are likely to adhere and reduce production efficiency. The concentration of the suspension stabilizer relative to the aqueous medium can be appropriately adjusted according to the conditions.

[0077] In the case of obtaining an aqueous dispersion containing a fluoropolymer by polymerization, the dry fluoropolymer can be recovered by precipitating, cleaning, and drying the fluoropolymer contained in the aqueous dispersion. In addition, in the case of obtaining a fluoropolymer in the form of a slurry by polymerization, the dry fluoropolymer can be recovered by taking out the slurry from the reaction vessel and cleaning and drying. By drying, the fluoropolymer can be recovered in the form of a powder.

[0078] The fluorinated copolymer obtained by polymerization can be formed into pellets. There is no particular limitation on the molding method for forming the pellets, and a conventionally known method can be used. For example, there can be cited a method in which the fluorinated copolymer is melt-extruded using a single-screw extruder, a twin-screw extruder, or a tandem extruder, and the fluorinated copolymer is cut into a predetermined length to form pellets. The extrusion temperature during melt extrusion needs to be changed according to the melt viscosity and the manufacturing method of the fluorinated copolymer, and is preferably the melting point of the fluorinated copolymer + 20°C to the melting point of the fluorinated copolymer + 140°C. There is no particular limitation on the cutting method of the fluorinated copolymer, and conventionally known methods such as a wire cutting method, a heat cutting method, an underwater cutting method, and a sheet cutting method can be used. The volatile components in the pellets can also be removed by heating the obtained pellets (degassing treatment). The obtained pellets can also be treated by contacting with warm water at 30°C to 200°C, steam at 100°C to 200°C, or hot air at 40°C to 200°C.

[0079] The fluorinated copolymer obtained by polymerization can also be heated to a temperature of 100°C or above in the presence of air and water (wet heat treatment). As a method for wet heat treatment, for example, the following method can be cited: using an extruder, while supplying air and water, the fluorinated copolymer obtained by polymerization is melted and extruded. By wet heat treatment, the thermally unstable functional groups such as -COF and -COOH of the fluorinated copolymer can be converted into thermally more stable -CF2H, and the total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH of the fluorinated copolymer can be easily adjusted to the above range. In addition to air and water, the conversion reaction to -CF2H can be promoted by heating the fluorinated copolymer in the presence of an alkali metal salt. However, it should be noted that, depending on the use of the fluorinated copolymer, contamination caused by alkali metal salts should be avoided.

[0080] The fluorinated copolymer obtained by polymerization can also be subjected to fluorination treatment. From the perspective of obtaining a molded body with excellent ozone resistance and in which fluoride ions are not easily eluted into a liquid such as hydrogen peroxide, it is preferred to subject the fluorinated copolymer to fluorination treatment. The fluorination treatment can be carried out by contacting the fluorinated copolymer that has not been fluorinated with a fluorinated compound. Through the fluorination treatment, thermally unstable functional groups such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and thermally relatively stable functional groups such as -CF2H of the fluorinated copolymer can be converted into thermally extremely stable -CF3. As a result, the total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH of the fluorinated copolymer can be easily adjusted to the above range.

[0081] The fluorine-containing compound is not particularly limited, and a fluorine radical source that generates fluorine radicals under fluorination conditions can be cited. As the above-mentioned fluorine radical source, F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, fluorinated halogens (such as IF5, ClF3), etc. can be cited.

[0082] The fluorine free radical source such as F2 gas can be 100% concentration, but from the aspect of safety, it is preferably mixed with an inert gas and diluted to 5% to 50% by mass for use, and more preferably diluted to 15% to 30% by mass for use. As the above-mentioned inert gas, nitrogen, helium, argon, etc. can be cited, and nitrogen is preferred from the aspect of economy.

[0083] The conditions of the fluorination treatment are not particularly limited, and the fluorinated copolymer in a molten state may be brought into contact with the fluorinated compound, but it may be generally carried out at a temperature below the melting point of the fluorinated copolymer, preferably at 20°C to 220°C, and more preferably at 100°C to 200°C. The above-mentioned fluorination treatment is generally carried out for 1 hour to 30 hours, preferably for 5 hours to 25 hours. The fluorination treatment is preferably a treatment in which the fluorinated copolymer that has not been fluorinated is brought into contact with fluorine gas (F2 gas).

[0084] The fluorinated copolymer of the present invention may be mixed with other components as required to obtain a composition. Other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, dehydrofluorination agents, etc.

[0085] As fillers, for example, silicon dioxide, kaolin, clay, organic clay, talc, mica, aluminum oxide, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, glass fibers, etc. can be cited. As conductive agents, carbon black, etc. can be cited. As plasticizers, dioctyl phthalate, pentaerythritol, etc. can be cited. As processing aids, carnauba wax, sulfone compounds, low molecular weight polyethylene, fluorine-based additives, etc. can be cited. As dehydrofluorination agents, organic onium, amidines, etc. can be cited.

[0086] As the other components, other polymers other than the above-mentioned fluorinated copolymers may be used. Examples of the other polymers include fluorinated resins other than the above-mentioned fluorinated copolymers, fluorinated rubbers, and non-fluorinated polymers.

[0087] Examples of the method for producing the composition include a method of dry-mixing the fluorinated copolymer and other components; a method of preliminarily mixing the fluorinated copolymer and other components in a mixer and then melt-kneading them in a kneader, melt extruder or the like; and the like.

[0088] The fluorinated copolymer of the present invention or the above-mentioned composition can be used as a processing aid, a molding material, etc., and is preferably used as a molding material. In addition, the aqueous dispersion, solution, suspension, and copolymer / solvent system of the fluorinated copolymer of the present invention can also be used, and they can be applied as a coating, or used for encapsulation, impregnation, and film casting. However, the fluorinated copolymer of the present invention is preferably used as the above-mentioned molding material because it has the above-mentioned characteristics.

[0089] The fluorinated copolymer of the present invention or the above composition may be molded to obtain a molded product.

[0090] The method for molding the above-mentioned fluorinated copolymer or the above-mentioned composition is not particularly limited, and injection molding, extrusion molding, compression molding, blow molding, transfer molding, rotational molding, roll lining molding, etc. can be cited. As a molding method, among them, preferably extrusion molding, compression molding, injection molding or transfer molding, from the aspect of being able to produce a molded body with high productivity, more preferably injection molding, extrusion molding or transfer molding, further preferably injection molding. That is, as a molded body, preferably an extrusion molded body, a compression molded body, an injection molded body or a transfer molded body, from the aspect of being able to produce with high productivity, more preferably an injection molded body, an extrusion molded body or a transfer molded body, further preferably an injection molded body. By molding the fluorinated copolymer of the present invention by injection molding, a beautiful molded product can be obtained.

[0091] Examples of the molded article containing the fluorinated copolymer of the present invention include nuts, bolts, joints, films, bottles, washers, wire coatings, tubes, hoses, pipes, valves, sheets, seals, gaskets, tanks, rollers, containers, cocks, connectors, filter cases, filter covers, flow meters, pumps, wafer carriers, wafer cassettes, and the like.

[0092] The fluorinated copolymer, the above composition or the above molded article of the present invention can be used for the following purposes, for example.

[0093] Films for food packaging, lining materials for fluid delivery pipelines used in food manufacturing processes, gaskets, sealing materials, sheets and other fluid delivery components for food manufacturing equipment;

[0094] Chemical plugs, packaging films, lining materials, gaskets, sealing materials, thin plates and other reagent delivery components for fluid delivery pipelines used in chemical manufacturing processes;

[0095] Lining components for the inner surface of liquid tanks and piping in chemical equipment and semiconductor factories;

[0096] O (square) rings / tubes / gaskets, valve core materials, hoses, sealing materials, etc. used in automobile fuel systems and peripheral devices; fuel delivery components such as hoses and sealing materials used in automobile AT devices;

[0097] Flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in car engines and peripheral devices of automobiles; other automobile components such as automobile brake hoses, air conditioning hoses, radiator hoses, wire covering materials, etc.;

[0098] Semiconductor manufacturing equipment O (square) rings, tubes, gaskets, valve core materials, hoses, sealing materials, rollers, gaskets, diaphragms, joints and other semiconductor device liquid delivery components;

[0099] Coating rollers, hoses, tubes, ink containers and other coating and ink components for coating equipment;

[0100] Food and beverage conveying components such as tubes or hoses for food and beverages, tubes, hoses, belts, gaskets, joints, etc., food packaging materials, and glass cooking equipment;

[0101] Waste liquid transmission components such as pipes and hoses used for waste liquid transmission;

[0102] Components for high-temperature liquid transmission such as pipes and hoses used for high-temperature liquid transmission;

[0103] Steam piping components such as pipes and hoses used for steam piping;

[0104] Pipe corrosion protection tapes such as tapes wrapped around pipes on ship decks, etc.

[0105] Various covering materials such as wire covering materials, optical fiber covering materials, transparent surface covering materials and back-side agents provided on the light incident side surface of photovoltaic elements of solar cells;

[0106] Diaphragms of diaphragm pumps and sliding components such as various sealing gaskets;

[0107] Weather-resistant covers for agricultural films, various roofing materials, sidewalls, etc.;

[0108] Interior materials used in the construction field, non-combustible fireproof safety glass and other glass covering materials;

[0109] Lining materials for laminated steel sheets used in the home appliance field, etc.

[0110] Further examples of the fuel delivery member used in the fuel system of the above-mentioned automobile include fuel hoses, filler hoses, evaporator hoses, etc. The above-mentioned fuel delivery member can also be used as a fuel delivery member for sour gasoline, alcohol fuel, and fuel added with gasoline additives such as methyl tert-butyl ether resistance and amine resistance.

[0111] The chemical plug and packaging film have excellent chemical resistance to acids, etc. In addition, as the chemical liquid conveying member, an anti-corrosion tape wound around the chemical equipment piping can also be cited.

[0112] Examples of the molded article include automobile radiator water chambers, chemical tanks, bellows, partitions, rollers, gasoline tanks, waste liquid transport containers, high temperature liquid transport containers, fisheries and fish farming tanks, and the like.

[0113] Examples of the molded bodies include automobile bumpers, door trims, instrument panels, food processing equipment, cooking machines, waterproof and oil-proof glass, lighting-related instruments, indicator panels and housings of OA instruments, electrically illuminated signboards, display screens, liquid crystal display screens, mobile phones, printer chassis, electrical and electronic components, groceries, trash cans, bathtubs, integrated bathrooms, ventilation fans, lighting frames, and the like.

[0114] The molded product containing the fluorinated copolymer of the present invention is excellent in abrasion resistance at 105°C, rigidity at a high temperature of 97.5°C, creep resistance, durability against repeated loads, tensile creep resistance at 105°C, ozone resistance, solvent crack resistance, and ductility against a tensile force applied at 125°C, and can therefore be suitably used in wafer carriers, filter covers, membranes, wire coatings, and the like.

[0115] The molded article containing the fluorinated copolymer of the present invention can be suitably used as a compressed member such as a gasket or a sealing gasket. The compressed member of the present invention may be a gasket or a sealing gasket.

[0116] The size and shape of the compressed member of the present invention can be appropriately set according to the purpose, and there is no particular limitation. The shape of the compressed member of the present invention can be, for example, annular. In addition, the compressed member of the present invention can have a circular, elliptical, quadrilateral with rounded corners, etc. shape when viewed from above, and has a through hole in its central portion.

[0117] The compressed member of the present invention is preferably used as a member for constituting a non-aqueous electrolyte battery. The compressed member of the present invention is particularly suitable as a member used in a state of contact with a non-aqueous electrolyte in a non-aqueous electrolyte battery. That is, the compressed member of the present invention may have a liquid contact surface with the non-aqueous electrolyte in the non-aqueous electrolyte battery.

[0118] The nonaqueous electrolyte battery is not particularly limited as long as it is a battery having a nonaqueous electrolyte, and examples thereof include lithium ion secondary batteries, lithium ion capacitors, etc. In addition, members constituting the nonaqueous electrolyte battery include sealing members, insulating members, and the like.

[0119] The non-aqueous electrolyte is not particularly limited, and one or more of known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc. can be used. The non-aqueous electrolyte battery can further include an electrolyte. The electrolyte is not particularly limited, and LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc. can be used.

[0120] The compressed member of the present invention can be preferably used as a sealing member such as a sealing gasket or a sealing pad, or an insulating member such as an insulating gasket or an insulating pad. A sealing member is a member used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating member is a member used for electrical insulation. The compressed member of the present invention can also be a member used for both sealing and insulation purposes.

[0121] The compressed member of the present invention can be suitably used as a sealing member for a non-aqueous electrolyte battery or an insulating member for a non-aqueous electrolyte battery. In addition, the compressed member of the present invention has excellent insulating properties because it contains the above-mentioned fluorinated copolymer. Therefore, when the compressed member of the present invention is used as an insulating member, it is firmly attached to two or more conductive members to prevent short circuits for a long time.

[0122] The fluorinated copolymer of the present invention can be suitably used as a material for forming an electric wire coating. A coated electric wire having a coating layer containing the fluorinated copolymer of the present invention has almost no fluctuation in outer diameter and is therefore excellent in electrical properties.

[0123] The covered electric wire comprises a core wire and a covering layer disposed around the core wire and containing the fluorinated copolymer of the present invention. For example, an extruded body formed by melt-extruding the fluorinated copolymer of the present invention on the core wire can be used as the covering layer. The covered electric wire is suitable for LAN cables (Ethernet Cables), high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is suitable for transmission cables such as LAN cables (Ethernet Cables) and high-frequency transmission cables.

[0124] As the material of the core wire, a metal conductor material such as copper or aluminum can be used. The core wire preferably has a diameter of 0.02 mm to 3 mm. The core wire diameter is more preferably 0.04 mm or more, further preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire diameter is more preferably 2 mm or less.

[0125] As specific examples of the core wire, AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 μm), AWG-26 (solid copper wire with a diameter of 404 μm), AWG-24 (solid copper wire with a diameter of 510 μm), AWG-22 (solid copper wire with a diameter of 635 μm), etc. can be used.

[0126] The thickness of the coating layer is preferably 0.1 mm to 3.0 mm, and the thickness of the coating layer is also preferably 2.0 mm or less.

[0127] As a high-frequency transmission cable, a coaxial cable can be cited. A coaxial cable generally has a structure in which an inner conductor, an insulating coating, an outer conductor layer and a protective coating are sequentially stacked from the core to the periphery. The molded body containing the fluorinated copolymer of the present invention can be suitably used as an insulating coating containing a fluorinated copolymer. The thickness of each layer in the above structure is not particularly limited. Generally, the diameter of the inner conductor is about 0.1 mm to 3 mm, the thickness of the insulating coating is about 0.3 mm to 3 mm, the thickness of the outer conductor layer is about 0.5 mm to 10 mm, and the thickness of the protective coating is about 0.5 mm to 2 mm.

[0128] The coating layer may contain air bubbles, and the air bubbles are preferably uniformly distributed in the coating layer.

[0129] The average bubble diameter of the bubbles is not limited, and is, for example, preferably 60 μm or less, more preferably 45 μm or less, further preferably 35 μm or less, further preferably 30 μm or less, particularly preferably 25 μm or less, and particularly preferably 23 μm or less. In addition, the average bubble diameter is preferably 0.1 μm or more, more preferably 1 μm or more. The average bubble diameter can be obtained by obtaining an electron microscope image of a cross section of the wire, calculating the diameter of each bubble by image processing, and averaging them.

[0130] The foaming rate of the coating layer may be 20% or more. More preferably, it is 30% or more, further preferably, it is 33% or more, and further preferably, it is 35% or more. The upper limit is not particularly limited, for example, it is 80%. The upper limit of the foaming rate may be 60%. The foaming rate is a value calculated as ((specific gravity of the wire coating material - specific gravity of the coating layer) / specific gravity of the wire coating material) × 100. The foaming rate can be appropriately adjusted according to the application by, for example, adjusting the amount of gas inserted in the extruder described later, or by selecting the type of dissolved gas.

[0131] The covered electric wire may also have other layers between the core wire and the covering layer, and may further have other layers (outer layers) around the covering layer. When the covering layer contains bubbles, the electric wire of the present invention may also be a two-layer structure (skin-foam) in which a non-foam layer is inserted between the core wire and the covering layer; a two-layer structure (foam-skin) in which a non-foam layer is covered on the outer layer; and a three-layer structure (skin-foam-skin) in which a non-foam layer is covered on the outer layer of the skin-foam. The non-foam layer is not particularly limited, and may be a resin layer composed of TFE / HFP copolymers, TFE / PAVE copolymers, TFE / ethylene copolymers, vinylidene fluoride polymers, polyolefin resins such as polyethylene [PE], and polyvinyl chloride [PVC].

[0132] The covered electric wire can be produced, for example, by heating a fluorinated copolymer using an extruder and extruding the fluorinated copolymer in a molten state onto a core wire to form a covering layer.

[0133] When forming the coating, it is also possible to heat the fluorinated copolymer, under the molten state of the fluorinated copolymer, introduce gas into the fluorinated copolymer, thereby forming the above-mentioned coating containing bubbles. As the gas, for example, a mixture of gases such as difluorochloromethane, nitrogen, carbon dioxide or the above-mentioned gases can be used. The gas can be introduced into the heated fluorinated copolymer in the form of pressurized gas, or it can be produced by mixing a chemical foaming agent in the fluorinated copolymer. The gas dissolves in the molten state of the fluorinated copolymer.

[0134] Furthermore, the fluorinated copolymer of the present invention can be suitably used as a material for products for high-frequency signal transmission.

[0135] The high-frequency signal transmission product is not particularly limited as long as it is a product used for the transmission of high-frequency signals, and examples thereof include (1) insulating plates of high-frequency circuits, insulating materials of connecting components, molded plates such as printed wiring boards, (2) molded bodies such as bases and antenna covers of high-frequency vacuum tubes, and (3) coated wires such as coaxial cables and LAN cables. The high-frequency signal transmission product can be suitably used in equipment that utilizes microwaves, particularly 3 GHz to 30 GHz microwaves, such as satellite communication equipment and mobile phone base stations.

[0136] In the above-mentioned products for high-frequency signal transmission, the fluorinated copolymer of the present invention can be suitably used as an insulator since it has a low dielectric loss tangent.

[0137] As the above-mentioned (1) molded plate, a printed wiring board is preferred from the aspect of obtaining good electrical characteristics. The above-mentioned printed wiring board is not particularly limited, and examples thereof include printed wiring boards of electronic circuits such as mobile phones, various computers, and communication equipment. As the above-mentioned (2) molded body, a radome is preferred from the aspect of low dielectric loss.

[0138] The fluorinated copolymer of the present invention can be suitably used for a film.

[0139] The film of the present invention is useful as a release film. The release film can be produced by molding the fluorinated copolymer of the present invention by melt extrusion molding, calendaring molding, compression molding, cast molding, etc. From the perspective of obtaining a uniform film, the release film can be produced by melt extrusion molding.

[0140] The film of the present invention can be applied to the surface of a roller used in OA equipment. In addition, the fluorinated copolymer of the present invention can be formed into a necessary shape by extrusion molding, compression molding, press molding, etc., and formed into a sheet, film, or tube, and used as a surface material for OA equipment rollers or OA equipment belts, etc. In particular, thin-walled tubes and films can be produced by melt extrusion molding.

[0141] The fluorinated copolymer of the present invention can also be suitably used in tubes, bottles and the like.

[0142] Although the embodiments have been described above, it should be understood that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.

[0143] <1> According to a first aspect of the present invention, there is provided a fluorinated copolymer comprising a tetrafluoroethylene unit, a hexafluoropropylene unit and a fluoro(alkyl vinyl ether) unit, wherein:

[0144] The content of the hexafluoropropylene unit is 11.2% to 13.2% by mass based on the total monomer units.

[0145] The content of the fluoro(alkyl vinyl ether) unit is 0% by mass to 0.4% by mass based on the total monomer units.

[0146] The melt flow rate at 372°C is 10.0 g / 10 min to 17.0 g / 10 min,

[0147] The total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH is relative to every 10 6 The number of carbon atoms in the main chain is less than 90.

[0148] <2> According to a second aspect of the present invention, there is provided the fluorinated copolymer according to the first aspect, wherein the content of the hexafluoropropylene units is from 11.5 to 12.5 mass % based on the total monomer units.

[0149] <3> According to a third aspect of the present invention, there is provided the fluorinated copolymer according to the first aspect or the second aspect, wherein the content of the fluorinated (alkyl vinyl ether) unit is 0 mass % to 0.1 mass % based on all monomer units.

[0150] <4> According to a fourth aspect of the present invention, there is provided a fluorinated copolymer according to any one of the first to third aspects, wherein the melt flow rate at 372° C. is from 10.5 to 16.5 g / 10 min.

[0151] <5> According to a fifth aspect of the present invention, there is provided a fluorinated copolymer according to any one of the first to fourth aspects, wherein the fluorinated (alkyl vinyl ether) unit is a perfluoro (propyl vinyl ether) unit.

[0152] <6> According to a sixth aspect of the present invention, there is provided an injection-molded article comprising the fluorinated copolymer according to any one of the first to fifth aspects.

[0153] <7> According to a seventh aspect of the present invention, there is provided a covered electric wire comprising a covering layer containing the fluorinated copolymer according to any one of the first to fifth aspects.

[0154] <8> According to an eighth aspect of the present invention, there is provided a molded article comprising the fluorinated copolymer according to any one of the first to fifth aspects, wherein the molded article is a wafer carrier, a filter cover, a film or a wire coating.

[0155] Example

[0156] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.

[0157] Each numerical value in the examples was measured by the following method.

[0158] (Content of monomer units)

[0159] The content of each monomer unit of the fluorinated copolymer is measured using an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker BioSpin) or an infrared absorption analyzer (Spectrum One manufactured by Perkin Elmer).

[0160] (Melt Flow Rate (MFR))

[0161] The MFR of the fluorinated copolymer was determined by measuring the mass (g / 10 minutes) of the polymer flowing out from a die having an inner diameter of 2 mm and a length of 8 mm at 372°C and a load of 5 kg using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D-1238.

[0162] (Amount of -CF2H)

[0163] The number of -CF2H groups in the fluorinated copolymer was measured using a nuclear magnetic resonance apparatus AVANCE-300 (manufactured by Bruker BioSpin) at a temperature of (melting point of the polymer + 20)°C. 19 In F-NMR measurement, it was determined from the peak integral value of -CF2H group.

[0164] (Amount of -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2)

[0165] The dry powder or pellets obtained in the examples and comparative examples are formed by cold pressing to produce films with a thickness of 0.25 mm to 0.3 mm. The film is scanned 40 times by a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] and analyzed to obtain an infrared absorption spectrum. The obtained infrared absorption spectrum is compared with the infrared absorption spectrum of a known film to determine the type of terminal group. In addition, the absorption peak of a specific functional group that appears in the differential spectrum between the obtained infrared absorption spectrum and the infrared absorption spectrum of a known film is calculated according to the following formula (A) for every 1×10 6 The number of functional groups N per carbon atom.

[0166] N=I×K / t(A)

[0167] I: Absorbance

[0168] K: Correction coefficient

[0169] t: film thickness (mm)

[0170] For reference, the absorption frequency, molar absorption coefficient and correction coefficient of the functional groups in the examples are shown in Table 2. The molar absorption coefficient was determined from the FT-IR measurement data of the low molecular model compound.

[0171] [Table 2]

[0172] Table 2

[0173]

[0174] (-OC(=O)OR(carbonate group) number)

[0175] The analysis was performed using the method described in International Publication No. 2019 / 220850. The absorption frequency was set to 1817 cm -1 The number of -OC(=O)OR (carbonate groups) was calculated in the same manner as the method for calculating the number of functional groups N, except that the molar absorptivity was set to 170 (l / cm / mol) and the correction factor was set to 1426.

[0176] (Melting Point)

[0177] Regarding the melting point of the fluorinated copolymer, a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd.) was used to perform the first temperature increase from 200°C to 350°C at a temperature increase rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and then the second temperature increase from 200°C to 350°C was performed again at a temperature increase rate of 10°C / min. The melting point was determined from the peak of the melting curve generated in the second temperature increase process.

[0178] Comparative Example 1

[0179] 40.25 kg of deionized water and 0.380 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, 40.25 kg of HFP was added to the autoclave in a vacuum state, and the autoclave was heated to 32.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.932 MPa, and then 0.31 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.932 MPa, and the set pressure was maintained by continuously adding TFE. 0.380 kg of methanol was added 1.5 hours after the start of polymerization. 0.31 kg of DHP was added 2 hours and 4 hours after the start of polymerization to reduce the internal pressure by 0.001 MPa, and 0.24 kg was added 6 hours later to reduce the internal pressure by 0.001 MPa. Thereafter, 0.07 kg of DHP was added every 2 hours until the reaction was completed.

[0180] In addition, when the additional amount of TFE reached 6.0 kg and 18.1 kg, 0.380 kg of methanol was added to the autoclave, respectively. Then, when the additional amount of TFE reached 40.25 kg, the polymerization was terminated. After the polymerization was completed, unreacted TFE and HFP were released to obtain a wet powder. Thereafter, the wet powder was washed with pure water and dried at 150° C. for 10 hours to obtain 46.4 kg of dry powder.

[0181] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.

[0182] After degassing the obtained pellets at 200°C for 8 hours in an electric furnace, the pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 200°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced into atmospheric pressure. 0.5 hours after the introduction of F2 gas, the gas was temporarily evacuated and F2 gas was introduced again. After a further 0.5 hours, the gas was evacuated again and F2 gas was introduced again. After that, the above-mentioned F2 gas introduction and evacuation operations were continued once for 1 hour, and the reaction was carried out at a temperature of 200°C for 8 hours. After the reaction was completed, the reactor was fully replaced with N2 gas, the fluorination reaction was terminated, and pellets were obtained. Using the obtained pellets, various physical properties were measured by the above method. The results are shown in Table 3.

[0183] Comparative Example 2

[0184] 945 g of deionized water and 8.5 g of methanol were added to an autoclave with a stirrer of 4 L, and the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, 945 g of HFP was added to the autoclave in a vacuum state, and the autoclave was heated to 25.5 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.830 MPa, and then 29.4 g of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.830 MPa, and the set pressure was maintained by continuously adding TFE. 8.5 g of methanol was added 1.5 hours after the start of polymerization. DHP29.4 g was added 2 hours and 4 hours after the start of polymerization, and the internal pressure was reduced by 0.002 MPa. 22.6 g was added after 6 hours, and the internal pressure was reduced by 0.002 MPa. Thereafter, 6.0 g of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.002 MPa each time.

[0185] In addition, when the additional amount of TFE reached 140 g, 8.5 g of methanol was added to the autoclave. Then, when the additional amount of TFE reached 454 g, the polymerization was terminated. After the polymerization was completed, unreacted TFE and HFP were released to obtain a wet powder. Thereafter, the wet powder was washed with pure water and dried at 150° C. for 10 hours to obtain 506 g of dry powder.

[0186] The obtained powder is used The copolymer was melt-extruded at 370°C using a screw extruder (manufactured by Imoto Seisakusho Co., Ltd.) to obtain pellets. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.

[0187] After degassing the obtained pellets at 200°C in an electric furnace for 8 hours, they were placed in a 500ml portable reactor (TVS1 type, manufactured by Pressure Glass Industry Co., Ltd.) and heated to 200°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced into atmospheric pressure. 0.5 hours after the introduction of F2 gas, the gas was temporarily evacuated and F2 gas was introduced again. After a further 0.5 hours, the gas was evacuated again and F2 gas was introduced again. After that, the above-mentioned F2 gas introduction and evacuation operations were continued once for 1 hour, and the reaction was carried out at a temperature of 200°C for 8 hours. After the reaction was completed, the reactor was fully replaced with N2 gas, the fluorination reaction was terminated, and pellets were obtained. Using the obtained pellets, various physical properties were measured by the above method. The results are shown in Table 3.

[0188] Comparative Example 3

[0189] The amount of methanol added before the start of polymerization was changed to 0.295 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.295 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.938 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. The obtained pellets were used to measure the HFP content and PPVE content by the above method. The results are shown in Table 3.

[0190] The obtained pellets were fluorinated in the same manner as in Comparative Example 1. Using the obtained pellets, various physical properties were measured by the above-mentioned methods. The results are shown in Table 3.

[0191] Comparative Example 4

[0192] 40.25 kg of deionized water and 0.290 kg of methanol were added to an autoclave with a stirrer of 174 L volume, and the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, 40.25 kg of HFP and 0.32 kg of PPVE were added to the autoclave in a vacuum state, and the autoclave was heated to 32.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.928 MPa, and then 0.31 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.928 MPa, and the set pressure was maintained by continuously adding TFE. 0.290 kg of methanol was added 1.5 hours after the start of polymerization. 0.31 kg of DHP was added 2 hours and 4 hours after the start of polymerization to reduce the internal pressure by 0.001 MPa, and 0.24 kg was added 6 hours later to reduce the internal pressure by 0.001 MPa. Thereafter, 0.07 kg of DHP was added every 2 hours until the reaction was completed.

[0193] It should be noted that 0.11 kg of PPVE was added when the continuous additional input amount of TFE reached 8.1 kg, 16.2 kg, and 24.3 kg, respectively. In addition, 0.290 kg of methanol was added to the autoclave when the additional input amount of TFE reached 6.0 kg and 18.1 kg, respectively. Then, the polymerization was terminated when the additional input amount of TFE reached 40.25 kg. After the polymerization was completed, the unreacted TFE and HFP were released to obtain a wet powder. After that, the wet powder was washed with pure water and dried at 150°C for 10 hours to obtain 47.0 kg of dry powder.

[0194] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.

[0195] The obtained pellets were fluorinated in the same manner as in Comparative Example 1. Using the obtained pellets, various physical properties were measured by the above-mentioned methods. The results are shown in Table 3.

[0196] Comparative Example 5

[0197] The amount of methanol added before the start of polymerization was changed to 0.367 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.367 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.930 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. Various physical properties were measured using the pellets obtained by the above-mentioned methods. The results are shown in Table 3.

[0198] Example 1

[0199] 40.25 kg of deionized water and 0.223 kg of methanol were added to an autoclave with a stirrer of a volume of 174 L, and the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, 40.25 kg of HFP was added to the autoclave in a vacuum state, and the autoclave was heated to 30.0 ° C. Next, TFE was added until the internal pressure of the autoclave reached 0.897 MPa, and then 0.63 kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.897 MPa, and the set pressure was maintained by continuously adding TFE. 0.223 kg of methanol was added 1.5 hours after the start of polymerization. 2 hours and 4 hours after the start of polymerization, 0.63 kg of DHP was added and the internal pressure was reduced by 0.001 MPa. 6 hours later, 0.48 kg was added and the internal pressure was reduced by 0.001 MPa. Thereafter, 0.13 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.001 MPa each time.

[0200] In addition, when the additional amount of TFE reached 6.0 kg and 18.1 kg, 0.223 kg of methanol was added to the autoclave, respectively. Then, when the additional amount of TFE reached 40.25 kg, the polymerization was terminated. After the polymerization was completed, unreacted TFE and HFP were released to obtain a wet powder. Thereafter, the wet powder was washed with pure water and dried at 150° C. for 10 hours to obtain 45.9 kg of dry powder.

[0201] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.

[0202] After degassing the obtained pellets at 200°C in an electric furnace for 72 hours, the pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 120°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced into atmospheric pressure. 0.5 hours after the introduction of F2 gas, the gas was temporarily evacuated and F2 gas was introduced again. After a further 0.5 hours, the gas was evacuated again and F2 gas was introduced again. After that, the above-mentioned F2 gas introduction and evacuation operations were continued once for 1 hour, and the reaction was carried out at a temperature of 120°C for 7 hours. After the reaction was completed, the reactor was fully replaced with N2 gas, the fluorination reaction was terminated, and pellets were obtained. Using the obtained pellets, various physical properties were measured by the above method. The results are shown in Table 3.

[0203] Example 2

[0204] The amount of methanol added before the start of polymerization was changed to 0.354 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.354 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.938 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. The HFP content and PPVE content were measured using the obtained pellets by the above-mentioned method. The results are shown in Table 3.

[0205] The obtained pellets were fluorinated in the same manner as in Comparative Example 1. Using the obtained pellets, various physical properties were measured by the above-mentioned methods. The results are shown in Table 3.

[0206] Example 3

[0207] The amount of methanol added before the start of polymerization was changed to 0.347 kg, the amount of methanol added in batches after the start of polymerization was changed to 0.347 kg, and the set pressure inside the autoclave before and after the start of polymerization was changed to 0.928 MPa. Copolymer pellets were obtained in the same manner as in Comparative Example 1. The HFP content and PPVE content were measured using the obtained pellets by the above-mentioned method. The results are shown in Table 3.

[0208] The obtained pellets were fluorinated in the same manner as in Comparative Example 1. Using the obtained pellets, various physical properties were measured by the above-mentioned methods. The results are shown in Table 3.

[0209] Example 4

[0210] 40.25kg of deionized water and 0.216kg of methanol were added to an autoclave with a stirrer of 174L, and the autoclave was fully replaced with vacuum nitrogen. Then, the autoclave was vacuum degassed, 40.25kg of HFP and 0.03kg of PPVE were added to the autoclave in a vacuum state, and the autoclave was heated to 30.0°C. Next, TFE was added until the internal pressure of the autoclave reached 0.891MPa, and then 0.63kg of 8% by mass di(ω-hydroperfluorohexanoyl) peroxide solution (hereinafter referred to as DHP) was added to the autoclave to start polymerization. The internal pressure of the autoclave at the start of polymerization was set to 0.891MPa, and the set pressure was maintained by continuously adding TFE. 0.216kg of methanol was added 1.5 hours after the start of polymerization. 2 hours and 4 hours after the start of polymerization, 0.63 kg of DHP was added and the internal pressure was reduced by 0.001 MPa. 6 hours later, 0.48 kg was added and the internal pressure was reduced by 0.001 MPa. Thereafter, 0.13 kg of DHP was added every 2 hours until the reaction was completed, and the internal pressure was reduced by 0.001 MPa each time.

[0211] It should be noted that PPVE was added with 0.01 kg of TFE when the continuous additional input amount reached 8.1 kg, 16.2 kg, and 24.3 kg. In addition, 0.216 kg of methanol was added to the autoclave when the additional input amount of TFE reached 6.0 kg and 18.1 kg. Then, the polymerization was terminated when the additional input amount of TFE reached 40.25 kg. After the polymerization was completed, the unreacted TFE and HFP were released to obtain a wet powder. After that, the wet powder was washed with pure water and dried at 150°C for 10 hours to obtain 46.1 kg of dry powder.

[0212] The obtained powder was melt-extruded at 370°C using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The HFP content and PPVE content of the obtained pellets were measured by the above-mentioned method. The results are shown in Table 3.

[0213] The obtained pellets were fluorinated in the same manner as in Comparative Example 1. Using the obtained pellets, various physical properties were measured by the above-mentioned methods. The results are shown in Table 3.

[0214] [Table 3]

[0215] Table 3

[0216]

[0217] "Others (pcs / C10)" in Table 3 6The record of "<9" in Table 3 means that the number (total number) of -CF2H groups is less than 9. The record of "<6" in Table 3 means that the number (total number) of the target functional groups is less than 6. The record of "ND" in Table 3 means that the peak for the target functional group cannot be confirmed to a quantitative degree.

[0218] Next, the following properties were evaluated using the obtained pellets. The results are shown in Table 4.

[0219] (Abrasion test)

[0220] Using pellets and a hot press molding machine, a sheet test piece with a thickness of about 0.2 mm was made, and a 10 cm × 10 cm test piece was cut out from it. The made test piece was fixed on the test bench of the Taber wear tester (No. 101 special Taber wear tester, manufactured by Yasuda Seiki Manufacturing Co., Ltd.), and the wear test was carried out using the Taber wear tester under the conditions of a test piece surface temperature of 105°C, a load of 500g, a wear wheel CS-10 (grinded with abrasive paper #240 for 20 turns), and a rotation speed of 60rpm. The weight of the test piece after 1000 turns was measured, and the weight of the test piece was further measured after 3100 turns of the test using the same test piece. The amount of wear was calculated by the following formula.

[0221] Wear loss (mg) = M1-M2

[0222] M1: Weight of test piece after 1000 revolutions (mg)

[0223] M2: Test piece weight after 3100 revolutions (mg)

[0224] (97.5℃ load deflection)

[0225] Using pellets and a hot press molding machine, a sheet test piece with a thickness of about 3.5 mm was made, from which a test piece of 80×10 mm was cut out and heated at 100°C for 20 hours in an electric furnace. In addition to using the obtained test piece, the test was carried out according to the method described in JIS KK 7191-1 using a heat deformation tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) at a test temperature of 30°C to 150°C, a heating rate of 120°C / hour, a bending stress of 1.8MPa, and a flat method. The load deflection rate was calculated by the following formula. The sheet with a small load deflection rate at 97.5°C has excellent rigidity at high temperatures.

[0226] Load deflection (%) = a2 / a1×100

[0227] a1: Thickness of the test piece before the test (mm)

[0228] a2: Deflection at 97.5°C (mm)

[0229] (Evaluation of creep resistance)

[0230] The creep resistance is determined according to the method described in ASTM D395 or JIS K6262:2013. Using pellets and a hot press molding machine, a molded body with an outer diameter of 13 mm and a height of 8 mm is produced. By cutting the obtained molded body, a test piece with an outer diameter of 13 mm and a height of 6 mm is produced. The produced test piece is compressed to a compression deformation rate of 25% at room temperature using a compression device. The compressed test piece is placed in an electric furnace fixed to the compression device and placed at 45°C for 72 hours. The compression device is removed from the electric furnace, cooled to room temperature, and then the test piece is removed. After the recovered test piece is placed at room temperature for 30 minutes, the height of the recovered test piece is measured, and the recovery ratio is calculated by the following formula.

[0231] Recovery ratio (%) = (t2-t1) / t3×100

[0232] t1: Height of spacer (mm)

[0233] t2: Height of the test piece removed from the compression device (mm)

[0234] t3: Compression deformation height (mm)

[0235] In the above test, t1 = 4.5 mm, t3 = 1.5 mm.

[0236] (Tensile strength after 300,000 cycles)

[0237] The tensile strength after 300,000 cycles was measured using a fatigue testing machine MMT-250NV-10 manufactured by Shimadzu Corporation. A sheet with a thickness of about 2.4 mm was made using pellets and a hot press molding machine, and a dumbbell-shaped sample (thickness 2.4 mm, width 5.0 mm, and measuring portion length 22 mm) was made using an ASTM D1708 micro dumbbell. The sample was mounted on a measuring fixture, and the measuring fixture was set in a constant temperature bath at 140°C with the sample mounted. Repeated stretching in a uniaxial direction was performed with a stroke of 0.2 mm and a frequency of 100 Hz, and the tensile strength of each stretch was measured (tensile strength when the stroke is +0.2 mm, unit: N).

[0238] The sheet having high tensile strength after 300,000 cycles maintained high tensile strength even after being loaded 300,000 times, and was excellent in durability against repeated loads (140° C.).

[0239] (Tensile creep test)

[0240] Use Hitachi High-Tech Corporation TMA-7100 to measure tensile creep strain. Use pellets and hot press molding machine to make a sheet with a thickness of about 0.1mm, and make a sample with a width of 2mm and a length of 22mm from the sheet. The sample is installed in the measuring fixture with a distance of 10mm between the fixtures. For the sample, the cross-sectional load becomes 4.69N / mm 2 The sample was loaded in a manner of 105°C and placed at 105°C. The displacement (mm) of the length of the sample was measured from 70 minutes after the start of the test to 975 minutes after the start of the test. The ratio of the displacement (mm) of the length to the initial sample length (10 mm) was calculated (tensile creep strain (%)). The sheet with a small tensile creep strain (%) measured at 105°C and 975 minutes is not easy to elongate even when loaded with a tensile load in a very high temperature environment, and has excellent high temperature tensile creep resistance.

[0241] (Injection moldability)

[0242] ·condition

[0243] The copolymer was injection molded using an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., SE50EV-A), with the barrel temperature set to 385°C, the mold temperature set to 177°C, and the injection speed set to 20 mm / s. As a mold, a mold (100 mm×100 mm×2.0 mmt, film gate, flow length 100 mm from the gate) in which HPM38 was plated with Cr was used. The obtained injection molded body was observed and evaluated according to the following criteria. The presence or absence of turbidity was visually confirmed. The presence or absence of surface roughness was confirmed by contacting the surface of the injection molded body.

[0244] 3: The injection molded body is transparent as a whole and the surface is smooth as a whole;

[0245] 2: White turbidity is observed within 1 cm from the mold gate and the surface is smooth overall;

[0246] 1: Cloudiness was observed within 1 cm from the location of the mold gate, and roughness was confirmed on the surface within 1 cm from the location of the mold gate;

[0247] 0: The copolymer was not filled in the entire mold, and a molded product of a desired shape was not obtained.

[0248] (Hydrogen peroxide immersion test)

[0249] Using pellets and a hot press molding machine, a sheet with a thickness of about 0.2 mm was produced to produce a 15 mm square test piece. 10 test pieces and 15 g of a 3 mass % hydrogen peroxide solution were placed in a 50 mL polypropylene bottle, heated at 95° C. for 20 hours in an electric furnace, and then cooled to room temperature. The test piece was taken out from the hydrogen peroxide solution, and TISAB solution (10) (manufactured by Kanto Chemical Co., Ltd.) was added to the remaining hydrogen peroxide solution. The fluoride ion concentration in the obtained hydrogen peroxide solution was measured using a fluoride ion meter. The fluoride ion concentration per unit sheet weight (eluted fluoride ion concentration) was calculated from the obtained measured value according to the following formula.

[0250] Dissolved fluoride ion concentration (mass ppm) = measured value (ppm) × amount of hydrogen peroxide solution (g) / weight of test piece (g)

[0251] (Ozone exposure test)

[0252] Use pellets and a hot press molding machine to make a sheet with a thickness of 1 mm, and then cut out 10×20 mm as a sample for ozone exposure test. Connect the ozone gas (ozone / oxygen = 10 / 90 volume %) generated by an ozone generator (trade name: SGX-A11MN (modified), manufactured by Sumitomo Seiki Industries, Ltd.) to a PFA container filled with ion exchange water, add water vapor to the ozone gas by bubbling in the ion exchange water, and then expose the sample to the wet ozone gas at 0.7 liters / minute through the PFA tank containing the sample at room temperature. Take out the sample 35 days after the start of exposure, rinse the surface lightly with ion exchange water, and use a transmission optical microscope to observe the portion 5μm to 200μm deep from the sample surface at a magnification of 100 times, and take a picture together with a standard scale to measure the sample surface every 1mm 2 The number of cracks with a length of 10 μm or more was evaluated according to the following criteria.

[0253] ○: The number of cracks is 10 or less;

[0254] ×: The number of cracks exceeded ten.

[0255] (Chemical liquid immersion crack test)

[0256] Using pellets and a hot press molding machine, a molded body with a thickness of about 2 mm was made. Using a rectangular dumbbell of 13.5 mm × 38 mm, the obtained sheet was punched to obtain 3 test pieces. In the center of the long side of each test piece obtained, a 19 mm × 0.45 mm blade was used to cut the incision according to ASTM D1693. Three incision test pieces and 25 g of concentrated hydrochloric acid were placed in a 100 mL polypropylene bottle, and after being immersed in a constant temperature bath at 25 ° C for 20 hours, the incision test piece was taken out. The three obtained incision test pieces were installed in a stress crack test fixture according to ASTM D1693. After heating at 80 ° C for 2 hours in an electric furnace, the incision and its surroundings were visually observed to count the number of cracks. The sheet without cracking has excellent solvent crack resistance.

[0257] ○: The number of cracks is 0;

[0258] ×: The number of cracks is 1 or more.

[0259] (125℃ tensile elongation)

[0260] The pellets and a hot press molding machine were used to obtain a 2.0 mm thick test piece (compression molding). A dumbbell-shaped test piece was cut out from the test piece using an ASTM V-type dumbbell, and the obtained dumbbell-shaped test piece was used to measure the tensile elongation at 125° C. under the conditions of 50 mm / min using Autograph (AG-I300 kN manufactured by Shimadzu Corporation) according to ASTM D638.

[0261] (Wire coating molding)

[0262] use A wire coating molding machine (manufactured by TANABE PLASTIC MACHINERY CO., LTD.) was used to extrusion coat a conductor having a conductor diameter of 0.50 mm with the following coating thickness to obtain a coated wire. The wire coating extrusion molding conditions were as follows.

[0263] a) Core conductor: soft steel wire conductor diameter 0.50mm

[0264] b) Coating thickness: 0.20mm

[0265] c) Diameter of coated wire: 0.90mm

[0266] d) Wire pulling speed: 30m / min

[0267] e) Extrusion conditions:

[0268] · Single screw extruder with barrel diameter = 30mm, L / D = 22

[0269] Die head (inner diameter) / sheet (outer diameter) = 9.0mm / 5.0mm

[0270] The set temperatures of the extruder were: barrel C-1 (320°C), barrel C-2 (350°C), barrel C-3 (370°C), head H (380°C), die head D-1 (380°C), die head D-2 (380°C). The core wire preheating was set to 80°C.

[0271] It was visually confirmed that the covered electric wire was produced without any problem.

[0272] (Film Forming)

[0273] use The film was produced using a T-die using an extruder (manufactured by Imoto Seisakusho). The extrusion molding conditions were as follows.

[0274] a) Winding speed: 1m / min

[0275] b) Roller temperature: 120°C

[0276] c) Film width: 70mm

[0277] d)Thickness: 0.10mm

[0278] e) Extrusion conditions:

[0279] · Single screw extruder with barrel diameter = 14mm, L / D = 20

[0280] Extruder set temperature: barrel C-1 (330°C), barrel C-2 (350°C), barrel C-3 (365°C), T-die head (370°C)

[0281] It was visually confirmed that the film was produced without any problem.

[0282]

Claims

1. A fluorinated copolymer, which is a fluorinated copolymer containing tetrafluoroethylene units, hexafluoropropylene units and fluoro(alkyl vinyl ether) units, wherein: The content of the hexafluoropropylene unit is 11.2% to 13.2% by mass based on the total monomer units. The content of the fluoro(alkyl vinyl ether) unit is 0% by mass to 0.4% by mass based on the total monomer units. The melt flow rate at 372°C is 10.0 g / 10 min to 17.0 g / 10 min, The total number of -CF2H, carbonyl-containing terminal groups, -CF=CF2 and -CH2OH is relative to every 10 6 The number of carbon atoms in the main chain is less than 90.

2. The fluorinated copolymer according to claim 1, wherein The content of the hexafluoropropylene unit is 11.5% by mass to 12.5% ​​by mass based on the total monomer units.

3. The fluorinated copolymer according to claim 1 or 2, wherein The content of the fluoro(alkyl vinyl ether) unit is 0% by mass to 0.1% by mass based on all monomer units.

4. The fluorinated copolymer according to any one of claims 1 to 3, wherein The melt flow rate at 372° C. is 10.5 g / 10 min to 16.5 g / 10 min.

5. The fluorinated copolymer according to any one of claims 1 to 4, wherein The fluoro(alkyl vinyl ether) unit is a perfluoro(propyl vinyl ether) unit. 6 . An injection-molded article comprising the fluorinated copolymer according to claim 1 . 7 . A covered electric wire comprising a covering layer comprising the fluorinated copolymer according to claim 1 .

8. A molded product comprising the fluorinated copolymer according to any one of claims 1 to 5, wherein The molded body is a wafer carrier, a filter cover, a membrane or a wire covering.

Citation Information

Patent Citations

  • Fluorine-containing copolymer and molded article