Chloroprene polymer composition, chloroprene polymer latex, and dip-molded article
By adjusting the molecular weight and adding specific components in the chloroprene-based polymer, the problem of deterioration of softness of chloroprene-based polymer after long-term storage is solved, and excellent tensile strength and softness are achieved. Suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202380030193.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-02-02
- Publication Date
- 2024-11-12
AI Technical Summary
The existing chloroprene-based polymers have poor flexibility after long-term storage, making it difficult to take into account both the tensile strength and the softness of the fracture.
A peak with a weight average molecular weight of 5,000 to 80,000 was detected in the chloroprene-based polymer composition, and an impregnated molded product for testing was prepared under specific conditions, including zinc oxide, p-cresol and dicyclopentadiene. The sodium salts of the butylation reaction product, 2-mercaptobenzimidazole and β-naphthalenesulfonate formalin condensate were adjusted, and the solid content concentration of the composition was molded and heated and dried by impregnation and solidification.
An impregnated molded product with excellent tensile strength and flexibility in fracture has been obtained. It is still very flexible after long-term storage. It is suitable for industrial/home gloves, medical gloves, balloons, catheters or boots and other products.
Smart Images

Figure BDA0005058733630000021 
Figure BDA0005058733630000341 
Figure BDA0005058733630000491
Abstract
Description
Technical Field
[0001] The present invention relates to a chloroprene polymer composition, a chloroprene polymer latex and a dip-molded article. Background Art
[0002] Chloroprene-based polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, rubber boots, and the like.
[0003] Various technologies have been proposed regarding chloroprene polymer latex for dip-molded products and dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex for dip-molded products, which contains 100 parts by mass of a modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, and has a pH of 7 to 14. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, wherein chloroprene and 2,3-dichloro-1,3-butadiene are copolymerized, and in the 13C-solid NMR spectrum of the polychloroprene, the peak area (A) of 126.2 to 127.6 ppm, the peak area (B) of 122.0 to 126.2 ppm, and the peak area (C) of 129.9 to 130.3 ppm are in the ranges shown by the following general formula (I). Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains a high molecular weight polymer and a low molecular weight polymer, and can achieve both excellent softness and mechanical properties in a vulcanized rubber prepared by dip molding. Patent Document 4 describes a chloroprene polymer latex, which has excellent flexibility and exhibits mechanical properties even under mild vulcanization conditions by copolymerizing chloroprene monomers with isoprene monomers as raw materials of isoprene rubber. Patent Document 5 describes an isoprene / chloroprene polymer dip-molded product, which exhibits excellent flexibility even without containing a diphenylguanidine reagent as a vulcanization accelerator by mixing isoprene polymer latex and chloroprene polymer latex. Patent Document 6 describes a dip-molded product, which exhibits excellent mechanical properties by mixing nitrile-butadiene polymer (NBR) latex and isoprene polymer latex with chloroprene polymer latex as a base.
[0004] [Number 1]
[0005]
[0006] [Prior art documents]
[0007] [Patent Document]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 2014-114342
[0009] [Patent Document 2] International Publication No. 2019 / 009038
[0010] [Patent Document 3] Japanese Patent Application Publication No. 2019-143002
[0011] [Patent Document 4] International Publication No. 2021-132460
[0012] [Patent Document 5] Japanese Patent Publication No. 2017-508840
[0013] [Patent Document 6] Japanese Patent Application Publication No. 2020-189963 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] Chloroprene polymer compositions containing chloroprene polymers have been widely used in applications such as gloves, balloons, boots, and catheters. In addition, in particular for medical rubber gloves, there is a tendency to seek chloroprene polymer compositions that can provide dip-molded products that have excellent flexibility, similar to that of dip-molded products obtained using natural rubber and polyisoprene, and have excellent tensile strength at break. However, dip-molded products obtained using chloroprene polymer compositions containing conventional chloroprene polymers may have poor flexibility after long-term storage, and it is difficult to achieve both tensile strength at break and flexibility after long-term storage.
[0016] The present invention has been made in view of such circumstances, and an object of the present invention is to provide a chloroprene polymer composition which has excellent tensile strength at break and flexibility and can provide a dip-molded product having excellent flexibility after long-term storage.
[0017] Solutions for solving problems
[0018] According to the present invention, there is provided a chloroprene polymer composition comprising a chloroprene polymer,
[0019] When the tetrahydrofuran-soluble component of the chloroprene polymer composition is measured by gel permeation chromatography, a peak having a weight average molecular weight of 5,000 to 80,000 is detected.
[0020] The toluene swelling degree of the test dip-molded product of the chloroprene polymer composition is 12.0 or less,
[0021] The test dip-molded product is obtained by molding the test dip-molded body-forming composition by an immersion coagulation method and then heating and drying the molded product at 140° C. for 60 minutes.
[0022] The test dip molded body forming composition contains 2 parts by mass of zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene, 1.0 parts by mass of 2-mercaptobenzimidazole, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, wherein the amount of the water is adjusted so that the solid content concentration of the test dip molded body forming composition becomes 30% by mass.
[0023] The above-mentioned toluene swelling degree is represented by formula (1).
[0024] Formula (1): Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r)
[0025] In formula (1),
[0026] W1 represents the mass of the aforementioned test dip-molded product before immersing the aforementioned test dip-molded product in toluene,
[0027] W2 represents the mass of the aforementioned test dip-molded product after immersing the aforementioned test dip-molded product in toluene,
[0028] P1 represents the specific gravity of the rubber component of the chloroprene polymer composition,
[0029] P2 represents the specific gravity of toluene,
[0030] r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip-molded product.
[0031] Formula (1): Toluene swelling degree (mass %) = (TB-TA) / TA×100
[0032] In formula (1),
[0033] TA represents the mass of the aforementioned test dip-molded product before immersing the aforementioned test dip-molded product in toluene,
[0034] TB represents the mass of the test dip-molded product after immersing the test dip-molded product in toluene.
[0035] As a result of intensive studies, the present inventors have found that by detecting a peak having a weight average molecular weight of 5,000 to 80,000 in a chloroprene polymer composition containing a chloroprene polymer and by making the toluene swelling degree of a test dip-molded article produced under specific conditions within a specific numerical range, a chloroprene polymer composition can be obtained which has excellent tensile strength at break and flexibility and has excellent flexibility after long-term storage, thereby completing the present invention.
[0036] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.
[0037] [1] A chloroprene polymer composition comprising a chloroprene polymer, wherein a peak having a weight average molecular weight of 5,000 to 80,000 is detected when a tetrahydrofuran-soluble component of the chloroprene polymer composition is measured by gel permeation chromatography, and a toluene swelling degree of a test dip-molded article of the chloroprene polymer composition is 12.0% by mass or less, wherein the test dip-molded article is obtained by molding the test dip-molded article by an immersion coagulation method and performing a heat drying treatment at 140°C for 60 minutes. The test dip molded body forming composition obtained by heating for 10 minutes contains 2 parts by mass of zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene, 1.0 parts by mass of 2-mercaptobenzimidazole, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, relative to 100 parts by mass of the solid content of the chloroprene polymer composition. The amount of the water is adjusted so that the solid content concentration of the test dip molded body forming composition becomes 30% by mass. The toluene swelling degree is represented by the formula (1).
[0038] Formula (1): Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r)
[0039] In formula (1),
[0040] W1 represents the mass of the aforementioned test dip-molded product before immersing the aforementioned test dip-molded product in toluene,
[0041] W2 represents the mass of the aforementioned test dip-molded product after immersing the aforementioned test dip-molded product in toluene,
[0042] P1 represents the specific gravity of the rubber component of the chloroprene polymer composition,
[0043] P2 represents the specific gravity of toluene,
[0044] r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip-molded product.
[0045] [2] The chloroprene polymer composition according to [1], wherein the toluene insoluble content is 50 to 90% by mass.
[0046] [3] The chloroprene polymer composition according to [1] or [2], wherein the chloroprene polymer composition contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, and the chloroprene polymer composition contains 8 to 20% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units.
[0047] [4] A chloroprene polymer composition as described in any one of [1] to [3], wherein the low-temperature hardness change ΔH1 of the test dip-molded article is 30 or less, and the low-temperature hardness change ΔH1 is expressed as HB1-HA1, HA1 represents the Shore hardness measured at 23°C using a type A durometer after the test dip-molded article is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm, and HB1 represents the Shore hardness measured at -10°C using a type A durometer after the test dip-molded article is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and then overlapped to a thickness of 6.00±0.20 mm.
[0048] [5] The chloroprene polymer composition according to any one of [1] to [4], wherein the ratio RB / RA of the total peak area amount RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total peak area amount RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, obtained by gas chromatography analysis of an extract obtained by extracting the test dip-molded product with an ethanol / toluene azeotropic mixture as specified in JIS K 6229, is 0.10 or more and 0.70 or less.
[0049] [6] A chloroprene polymer latex comprising the chloroprene polymer composition according to any one of [1] to [5] and water.
[0050] [7] A dip-molded product, which is a dip-molded product comprising the composition for forming a dip-molded product containing the chloroprene polymer latex as described in [6].
[0051] [8] The dip-molded article according to [7], which is industrial / general household gloves, medical gloves, balloons, catheters or boots.
[0052] [9] For the dip-molded article as described in [7], the low-temperature hardness change ΔH2 is less than 30, and the above-mentioned low-temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 means the Shore hardness measured by using a type A durometer at 23°C after the dip-molded article is heated at 70°C for 30 minutes and overlapped to a thickness of 6.00±0.20 mm. HB2 means the Shore hardness measured by using a type A durometer at -10°C after the dip-molded article is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and overlapped to a thickness of 6.00±0.20 mm.
[0053]
[10] A dip-molded article, which is a dip-molded article of a composition for forming a dip-molded article containing a chloroprene polymer latex, wherein the low-temperature hardness change of the dip-molded article is 30 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 represents the Shore hardness measured at 23°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm, HB2 represents the Shore hardness measured at -10°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours, and then overlapped to a thickness of 6.00±0.20 mm, wherein the dip-molded article is measured according to JIS K The tensile strength at break of 6251 is above 18.0 MPa, and the modulus at 100% elongation is below 0.65 MPa.
[0054] Effects of the Invention
[0055] According to the chloroprene polymer composition containing the chloroprene polymer of the present invention, a dip-molded product having excellent tensile strength at break and flexibility and excellent flexibility after long-term storage can be obtained. In addition, the obtained dip-molded product can be used as various products and parts requiring excellent tensile strength at break and flexibility after long-term storage by utilizing its characteristics. Specifically, it can be used as industrial / general household gloves, medical gloves, balloons, catheters, or boots. DETAILED DESCRIPTION
[0056] Hereinafter, the embodiments of the present invention will be described in detail by way of example. The present invention is not limited by these descriptions. The characteristic features of the embodiments of the present invention shown below can be combined with each other. In addition, the invention is established independently for each characteristic feature.
[0057] 1. Chloroprene polymer composition
[0058] The chloroprene polymer composition of the present invention contains a chloroprene polymer. In addition, when the tetrahydrofuran soluble component of the chloroprene polymer composition of the present invention is measured by gel permeation chromatography, a peak with a weight average molecular weight of 5,000 to 80,000 is detected. In addition, the toluene swelling degree of the test dip molded product of the chloroprene polymer composition is 12.0 or less.
[0059] The chloroprene polymer composition of the present invention contains at least one chloroprene polymer. The chloroprene polymer of the present invention is a polymer containing a monomer unit derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene).
[0060] The chloroprene polymer composition of one embodiment of the present invention may also contain a diene polymer A and a chloroprene polymer B. In the present invention, the diene polymer A refers to a polymer containing a diene monomer unit derived from a diene monomer. As described later, the diene polymer A of one embodiment of the present invention preferably contains a monomer unit derived from chloroprene. That is, the chloroprene polymer composition of one embodiment of the present invention may also contain a chloroprene polymer A and a chloroprene polymer B. The diene polymer A and the chloroprene polymer B are described later.
[0061] The chloroprene polymer composition of the present invention has a peak with a weight average molecular weight of 5,000 to 80,000 when the tetrahydrofuran soluble component of the chloroprene polymer composition is measured by gel permeation chromatography. More specifically, the chloroprene polymer composition of the present invention has a peak with a weight average molecular weight of 5,000 to 80,000 in the molecular weight distribution obtained by measuring by gel permeation chromatography a sample obtained by mixing the chloroprene polymer composition with a large amount of methanol to precipitate, filtering and drying the obtained polymer and dissolving it in tetrahydrofuran.
[0062] In addition, in the chloroprene polymer composition according to one embodiment of the present invention, in a molecular weight distribution obtained by dissolving a polymer obtained by mixing the chloroprene polymer composition with a large amount of methanol to precipitate, filtering and drying the obtained polymer in tetrahydrofuran and subjecting the obtained sample to gel permeation chromatography, it is preferred that a peak with a weight average molecular weight of 5,000 to 80,000 and a peak with a weight average molecular weight of 200,000 to 1,500,000 are detected, more preferably a peak with a weight average molecular weight of 5,000 to 50,000 and a peak with a weight average molecular weight of 300,000 to 1,500,000 are detected, and further preferably a peak with a weight average molecular weight of 8,000 to 30,000 and a peak with a weight average molecular weight of 500,000 to 1,500,000 are detected. The chloroprene polymer composition of one embodiment of the present invention preferably contains a diene polymer A having a weight average molecular weight of 5,000 to 80,000 and a chloroprene polymer B having a weight average molecular weight of 200,000 to 1,500,000, or a chloroprene polymer B having a weight average molecular weight of 5,000 to 80,000 and a diene polymer A having a weight average molecular weight of 200,000 to 1,500,000, and more preferably contains a diene polymer A having a weight average molecular weight of 5,000 to 50,000 and a chloroprene polymer B having a weight average molecular weight of 300,000 to 1,500,000. The present invention preferably contains a chloroprene polymer B having a weight average molecular weight of 5,000 to 50,000, or a chloroprene polymer B having a weight average molecular weight of 5,000 to 50,000 and a diene polymer A having a weight average molecular weight of 300,000 to 1,500,000, and more preferably contains a diene polymer A having a weight average molecular weight of 8,000 to 30,000 and a chloroprene polymer B having a weight average molecular weight of 500,000 to 1,500,000, or a chloroprene polymer B having a weight average molecular weight of 8,000 to 30,000 and a diene polymer A having a weight average molecular weight of 500,000 to 1,500,000.
[0063] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 5 to 40% by mass of a polymer having a weight average molecular weight of 5,000 to 80,000, based on 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight average molecular weight of 5,000 to 80,000 may be, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass, or may be within a range between any two of the values exemplified herein.
[0064] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 60 to 95% by mass of a polymer having a weight average molecular weight of 200,000 to 1,500,000, based on 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight average molecular weight of 200,000 to 1,500,000 is, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass, and may be within the range between any two of the values exemplified herein.
[0065] The weight average molecular weight can be obtained, for example, by mixing a chloroprene polymer composition with a large amount of methanol to precipitate it, filtering, and drying the chloroprene polymer composition, and dissolving the obtained chloroprene polymer composition in tetrahydrofuran and analyzing the sample obtained. The measurement conditions of GPC can be described in the examples. The weight average molecular weight can be controlled by adjusting the manufacturing conditions, specifically, by adjusting the polymerization formula of the diene polymer A and the chloroprene polymer B contained in the chloroprene polymer composition, the formula of the type and amount of the chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc.
[0066] The chloroprene polymer composition of one embodiment of the present invention preferably has a toluene insoluble content of 50 to 90% by mass, more preferably 60 to 85% by mass. Examples of the toluene insoluble content include 50, 55, 60, 65, 70, 75, 80, 85, and 90%, and may be within a range between any two of the values exemplified herein.
[0067] The toluene insoluble matter can be determined by immersing a chloroprene polymer composition obtained by freeze-drying a latex containing the chloroprene polymer composition in toluene for 16 hours, wherein the freeze-dried chloroprene polymer composition is designated as Ag and the gel component (insoluble matter) separated from the mixture dissolved in toluene is designated as Bg. Specifically, the toluene insoluble matter can be determined by the method described in the Examples.
[0068] Toluene insoluble matter (gel component) = B / A x 100 (%)
[0069] The toluene insoluble matter can be controlled by adjusting the production conditions of the chloroprene polymer composition, such as the polymerization formula of the polymer (e.g., diene polymer A, chloroprene polymer B) contained in the chloroprene polymer composition, the formula such as the type and amount of the chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc., and adjusting the type and amount of the polymer (e.g., diene polymer A, chloroprene polymer B).
[0070] The chloroprene polymer composition of one embodiment of the present invention preferably contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The chloroprene polymer composition preferably contains 8 to 20% by mass of 2,3-dichloro-1,3-butadiene monomer units, more preferably 10 to 17% by mass, relative to 100% by mass of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units. The content of the 2,3-dichloro-1,3-butadiene monomer units is, for example, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20% by mass, and may be within the range between any two of the values exemplified herein.
[0071] The chloroprene polymer composition of one embodiment of the present invention may contain 70 to 100% by mass of chloroprene monomer units when the chloroprene polymer composition is 100% by mass. The content of the chloroprene monomer units may be, for example, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within the range between any two of the values exemplified herein.
[0072] The chloroprene polymer composition of one embodiment of the present invention may contain 0 to 30% by mass of other monomer units other than the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit when the chloroprene polymer composition is set to 100% by mass. The content of other monomer units is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, or may be within the range between any two of the values exemplified herein. The chloroprene polymer of one embodiment of the present invention may also be composed of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units.
[0073] When the chloroprene polymer composition is a mixture of two or more different chloroprene polymers, the content of each monomer unit refers to the total of each monomer unit in all chloroprene polymers contained in the chloroprene polymer composition.
[0074] The content of 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer composition can be measured by using a pyrolysis gas chromatography-mass spectrometer to measure a test piece of the chloroprene polymer composition obtained by freeze-drying a latex containing the chloroprene polymer composition, and then the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene is obtained and calculated using a calibration curve with the 2,3-dichloro-1,3-butadiene content. Specifically, the measurement can be performed using the method of the Examples.
[0075] The content of 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer composition can be controlled by adjusting the production conditions of the polymer contained in the chloroprene polymer composition, such as the type and amount of raw materials, and the amount of polymer (e.g., diene polymer A, chloroprene polymer B) blended.
[0076] The toluene swelling degree of the test dip-molded product of the chloroprene polymer composition of the present invention is 12.0 or less, preferably 10.0 or less. The toluene swelling degree is represented by formula (1).
[0077] Formula (1): Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r)
[0078] In formula (1), W1 represents the mass of the test dip molded article before immersing the test dip molded article in toluene, W2 represents the mass of the test dip molded article after immersing the test dip molded article in toluene, P1 represents the specific gravity of the rubber component of the chloroprene polymer composition, P2 represents the specific gravity of toluene, and r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip molded article. Here, the rubber component of the chloroprene polymer composition refers to the chloroprene polymer component in the latex containing the chloroprene polymer composition, which can be obtained by mixing the latex containing the chloroprene polymer composition with methanol to precipitate, filtering, and drying.
[0079] Furthermore, the specific gravity of the rubber component of the chloroprene polymer composition and the specific gravity of toluene may be values measured at 20° C., and P2 may be 0.867. P1 may be the specific gravity of the rubber component of the chloroprene polymer composition measured at 20° C., and P1 may be 1.23.
[0080] The toluene swelling degree of the test dip molded product of the chloroprene polymer composition is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, or 12.0, and may be within the range between any two of the values exemplified here.
[0081] The toluene swelling degree of the test dip-molded product of the chloroprene polymer composition is considered to be related to the crosslinking degree of the chloroprene polymer composition, and it is presumed that the higher the crosslinking degree, the lower the swelling degree. The chloroprene polymer composition of the present invention can obtain a dip-molded product having excellent tensile strength at break and flexibility, and excellent flexibility after long-term storage by detecting a peak with a weight average molecular weight of 5,000 to 80,000 and making the toluene swelling degree of the test dip-molded product produced under specific conditions 12.0 or less.
[0082] The toluene swelling degree can be measured by the method described in the Examples. The toluene swelling degree can be adjusted by appropriately selecting a method for producing the chloroprene polymer composition. For example, a chloroprene polymer composition having a toluene swelling degree of 12.0 or less can be obtained by a production method including a polymerization step of polymerizing the chloroprene polymer B in the presence of a diene polymer A, as described later.
[0083] The chloroprene polymer composition of one embodiment of the present invention preferably has a low-temperature hardness change ΔH1 of 30 or less, more preferably 20 or less, of a test dip-molded article prepared from a test dip-molded article forming composition. The low-temperature hardness change ΔH1 is expressed as HB1-HA1. The low-temperature hardness change ΔH1 can be calculated by storing the test dip-molded article at -10°C for 168 hours and subtracting the hardness before low-temperature storage from the hardness after low-temperature storage. Specifically, HA1 represents the Shore hardness measured at 23°C using a type A hardness meter after heating the test dip-molded article at 70°C for 30 minutes (before storing at -10°C for 168 hours), overlapping the test dip-molded article to a thickness of 6.00±0.20 mm. In addition, HB1 represents the Shore hardness measured at -10°C using a type A hardness meter after the test dip-molded product was heated at 70°C for 30 minutes (before being stored at -10°C for 168 hours), and after the test dip-molded product was stored at -10°C for 168 hours, the test dip-molded product was overlapped to a thickness of 6.00±0.20 mm.
[0084] The low temperature hardness change ΔH1 is, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30, and may be within the range between any two of the values exemplified here.
[0085] The low-temperature hardness change ΔH1 can be measured by the method described in the Examples. In addition, the purpose of the heating treatment under the conditions of 70°C and 30 minutes is to melt the crystal structure contained in the test dip-molded product before being stored at -10°C for 168 hours. It is believed that the crystal structure will melt by performing the heating treatment under the conditions of 70°C and 30 minutes. The low-temperature hardness change ΔH1 can be controlled by adjusting the production conditions of the chloroprene polymer composition.
[0086] The chloroprene polymer composition of one embodiment of the present invention preferably has a ratio RB / RA of the total amount of peak areas RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount of peak areas RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, obtained by gas chromatography analysis of an extract obtained by extracting a test dip molded article prepared from the test dip molded article forming composition using an ethanol / toluene azeotropic mixture specified in JIS K 6229, of 0.10 to 0.70, more preferably 0.15 to 0.50. RB / RA is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, and may be within the range between any two of the values exemplified herein.
[0087] RB / RA can be determined by analyzing the extract obtained by extracting the test impregnated molded product with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229 and treating it with hydrochloric acid, and calculating the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount of peak area of rosin acid, neorosin acid, palustric acid, levopimaric acid and their salts to the total amount of peak area of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, and specifically, can be determined by the method described in the Examples. RB / RA can be controlled by adjusting the type and amount of the emulsifier (particularly rosin acid and its salt) used in the emulsion polymerization of the polymer contained in the chloroprene polymer composition.
[0088] The chloroprene polymer composition of one embodiment of the present invention preferably has a tensile strength at break of 18.0 MPa or more, more preferably 19.0 MPa or more, and further preferably 20.0 MPa or more, as measured in accordance with JIS K6251, of a test dip molded article prepared from the test dip molded article forming composition. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within the range between any two of the values exemplified herein.
[0089] The chloroprene polymer composition of one embodiment of the present invention preferably has a test dip molded article prepared from the test dip molded article composition having a modulus of 0.65 MPa or less, more preferably 0.60 MPa or less, at 100% elongation measured in accordance with JIS K6251. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, and may be within the range between any two of the values exemplified herein.
[0090] The chloroprene polymer composition of one embodiment of the present invention preferably has a modulus of 0.80 MPa or less, more preferably 0.7 MPa or less, at 100% elongation measured in accordance with JIS K 6251 after a dip molded article of a composition for forming a dip molded article containing the chloroprene polymer composition, particularly a test dip molded article prepared from the composition for forming a test dip molded article, is stored at 23° C. for 6 months. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, or 0.80 MPa, and may be within the range between any two of the values exemplified herein.
[0091] The tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months of the dip molded article containing the chloroprene polymer composition can be controlled by adjusting the weight average molecular weight of the diene polymer A and the chloroprene polymer B contained in the dip molded article, the type and content of the monomer units contained, the polymerization conditions of each polymer, the blending ratio, etc. In addition, the tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months can be measured as described in the Examples.
[0092] The test dip-molded article can be obtained by molding the test dip-molded article composition by the dip coagulation method and heating and drying at 140°C for 60 minutes. Here, the test dip-molded article composition contains 2 parts by mass of zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene, 1.0 parts by mass of 2-mercaptobenzimidazole, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, and the amount of water can be adjusted so that the solid content concentration of the test dip-molded article composition becomes 30% by mass. Specifically, it can be prepared by the method described in the examples.
[0093] 2. Method for producing chloroprene polymer composition
[0094] The method for producing the chloroprene polymer composition of the present invention is not particularly limited, and the chloroprene polymer composition can be obtained, for example, by the following method.
[0095] The method for producing a chloroprene polymer composition according to one embodiment of the present invention may include a polymerization step of polymerizing a chloroprene polymer B in the presence of a diene polymer A. In addition, as described above, the chloroprene polymer composition of the present invention contains a diene polymer A and a chloroprene polymer B, and the diene polymer A and the chloroprene polymer B may have different weight average molecular weights.
[0096] Hereinafter, first, the diene polymer A and the chloroprene polymer B according to one embodiment of the present invention will be described.
[0097] 2.1 Diene polymer A
[0098] In the present invention, the diene polymer A refers to a polymer containing a diene monomer unit derived from a diene monomer. The diene polymer A may contain a monomer unit derived from a monomer other than the diene monomer, etc., within the range not impairing the purpose of the present invention.
[0099] The diene polymer A of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from diene monomers, preferably 70 to 100% by mass, when the diene polymer A is 100% by mass. The content of the monomer units derived from diene monomers is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100% by mass, and may be within the range between any two of the values exemplified herein.
[0100] The diene monomer may be a conjugated diene monomer having 4 to 6 carbon atoms, and specific examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. The diene polymer A preferably contains a chloroprene monomer unit.
[0101] The diene polymer A according to one embodiment of the present invention preferably contains at least one selected from natural rubber, isoprene polymers, butadiene polymers, styrene-butadiene polymers, chloroprene polymers, and acrylonitrile-butadiene polymers.
[0102] The diene polymer A of one embodiment of the present invention preferably contains a monomer unit derived from chloroprene, and more preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The diene polymer A of one embodiment of the present invention may not contain sulfur, and the diene polymer A of one embodiment of the present invention may also be a polymer having no -SS- structure derived from sulfur in the main chain.
[0103] The diene polymer A of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, when the diene polymer A is 100% by mass. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within the range between any two of the values exemplified herein.
[0104] The diene polymer A of one embodiment of the present invention may contain 0 to 30% by mass of a monomer unit derived from 2,3-dichloro-1,3-butadiene, based on 100% by mass of the diene polymer A. The content of the monomer unit derived from 2,3-dichloro-1,3-butadiene may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within the range between any two of the values exemplified herein.
[0105] The diene polymer A of the present invention may have a weight average molecular weight different from that of the chloroprene polymer B. The difference between the weight average molecular weight of the diene polymer A of one embodiment of the present invention and the weight average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, and more preferably 400,000 or more. The difference between the weight average molecular weight of the diene polymer A and the weight average molecular weight of the chloroprene polymer B described below is, for example, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, and may also be within the range between any two of the values exemplified herein.
[0106] For example, the weight average molecular weight of the diene polymer A may be smaller than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 5,000 to 80,000. The weight average molecular weight of the diene polymer A is, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, or 80,000, and may be within the range between any two of the values exemplified here.
[0107] In addition, as another example, the weight average molecular weight of the diene polymer A may be greater than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 200,000 to 1,500,000. The weight average molecular weight of the diene polymer A is, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, and may be within the range between any two of the values exemplified herein.
[0108] The weight average molecular weight of diene polymer A can be obtained by using gel permeation chromatography (GPC) to mix a polymerization solution (such as latex) containing diene polymer A with a large amount of methanol to precipitate it, filtering, drying and dissolving the diene polymer A in tetrahydrofuran to obtain a sample for analysis. The determination conditions of GPC can be as described in the examples. The weight average molecular weight of diene polymer A can be controlled by adjusting the polymerization formula in the polymerization of diene polymer A, the type and amount of chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc., and can be especially controlled by adjusting the type and amount of chain transfer agent.
[0109] 2.2 Method for producing diene polymer A
[0110] The method for producing the diene polymer A of the present invention is not particularly limited. As an example, the method for producing the diene polymer A according to one embodiment of the present invention may include a diene polymer A polymerization step of polymerizing a raw material monomer containing a diene monomer to obtain a diene polymer.
[0111] In the polymerization step, the raw material monomers include one or more diene monomers and may also include other monomers copolymerizable with the diene monomers. Examples of diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. Examples of other monomers copolymerizable with the diene monomers include styrene, methacrylic acid, acrylonitrile, sulfur, and the like.
[0112] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained diene polymer A is within the above numerical range. As an example, when the diene polymer A contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, and contains 0 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene, the amount of 2,3-dichloro-1,3-butadiene added is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.
[0113] When producing the diene polymer A, the raw material monomers are polymerized by polymerization methods such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization termination solution, and a relatively high polymerization rate.
[0114] In the polymerization step of the diene polymer A, the raw material monomers can be put into a polymerization container together with necessary reagents such as a polymerization initiator, a chain transfer agent, and a solvent for polymerization. As an example, when the diene polymer A is polymerized by emulsion polymerization, the raw material monomers can be put into a reaction tank together with a chain transfer agent, water, an alkali (for example, a metal hydroxide such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc. for polymerization.
[0115] The polymerization initiator is not particularly limited, and a known polymerization initiator commonly used in the polymerization of diene polymers can be used. Examples of the polymerization initiator include organic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide.
[0116] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in the polymerization of diene polymers such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.
[0117] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the diene polymer A obtained can be adjusted.
[0118] As an example, in order to obtain a diene polymer A having a weight average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may be within the range between any two of the values exemplified here.
[0119] In addition, as an example, in order to obtain a diene polymer A having a weight average molecular weight of 200,000 or more, preferably a weight average molecular weight of 500,000 to 1,500,000, the amount of the chain transfer agent added is preferably 0 mass parts or more and less than 0.40 mass parts relative to 100 mass parts of the monomer. The amount of the chain transfer agent added is more preferably 0.02 to 0.05 mass parts, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, 0.30 mass parts, less than 0.40 mass parts, and may also be within the range between any two values exemplified herein. In particular, when it is desired to obtain a diene polymer A having a weight average molecular weight of 200,000 or more, a chain transfer agent may not be used.
[0120] During emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the emulsion polymerization begins, and also includes a case where the composition is changed by adding each component later or adding each component in batches. If the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is 13.5 or less, an excessive increase in viscosity during polymerization can be suppressed, and the polymerization reaction can be controlled more stably.
[0121] In the polymerization step, the monomers include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above for the monomer units that may be contained in the chloroprene polymer. In addition, it is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above numerical range.
[0122] The emulsifier preferably contains rosin acid and / or rosin salt. Examples of rosin salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin salt added may be 3.0 to 7.0 parts by mass relative to 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, or may be within the range between any two of the values exemplified herein.
[0123] Abietic acid and / or abietic acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. As the conjugated resin acid component, abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof may be cited. As the non-conjugated resin acid component, dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof may be cited.
[0124] The ratio RB / RA of the total amount of peak area RB of rosin acid, neorosin acid, palustric acid, levopimaric acid and their salts obtained by gas chromatography analysis of the extract obtained by extracting the rosin acid and rosin acid salt used in the emulsion polymerization step with an ethanol / toluene azeotropic mixture specified in JIS K 6229 to the total amount of peak area RA of dehydrorosin acid, pimaric acid, isopimaric acid, dihydrorosin acid and their salts may be 0.10 or more and 0.70 or less. The RB / RA of rosin acid and rosin acid salt is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, or may be within the range between any two of the values exemplified herein. By adjusting the type and amount of rosin acid and / or rosin acid salt, the RB / RA of the test dip molded product of the obtained chloroprene polymer composition can be adjusted.
[0125] The emulsifier may also contain emulsifiers and dispersants other than rosin acid and rosin salts. As emulsifiers and dispersants other than rosin acid and rosin salts, cationic, anionic, and nonionic emulsifiers and dispersants can be used. In one embodiment of the present invention, as the emulsifier used in the emulsion polymerization step, rosin acid and / or rosin salts, and anionic emulsifiers and dispersants may be included. As anionic emulsifiers and dispersants, from the viewpoint of stabilizing the chloroprene polymer latex when the pH adjuster is added, it is preferred to use sulfate-based and sulfonate-based anionic emulsifiers and dispersants in combination. Specifically, alkyl sulfonates, alkyl aryl sulfates, condensates of sodium β-naphthalenesulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonate having a carbon number of 8 to 20 can be cited. The amount of anionic emulsifiers and dispersants added can be 0.05 to 5 parts by mass relative to 100 parts by mass of the raw material monomer. The amount of the anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass per 100 parts by mass of the raw monomers, or may be within the range between any two of the values exemplified here.
[0126] The polymerization temperature is preferably within a range of 5 to 55° C. It is more preferred that the polymerization temperature is 5° C. or higher because the emulsion does not freeze, and that the polymerization temperature is 55° C. or lower because the diene monomer does not evaporate or boil.
[0127] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that stops the polymerization reaction, or by stopping the addition of a polymerization initiator to adjust the polymerization conversion rate.
[0128] As polymerization terminators, for example, there are diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. A polymerization terminator may not be used in the polymerization step of the diene polymer A of one embodiment of the present invention. After the polymerization is completed, unreacted monomers can be removed by conventional methods such as reduced pressure distillation.
[0129] Furthermore, to the composition (e.g., latex) containing the diene polymer A obtained by the production method of one embodiment of the present invention, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be arbitrarily added after polymerization within a range that does not impair the effects of the present invention.
[0130] In the polymerization step of the diene polymer A, the polymerization may be started after all the raw material monomers and reagents used in the polymerization step are added to the polymerization container before the start of the polymerization, or at least a portion of the raw material monomers and / or reagents used in the polymerization step may be added to the polymerization container before the start of the polymerization and the remaining portion may be added after the start of the polymerization.
[0131] Before the start of polymerization, at least a portion of the raw material monomers and reagents are added to the polymerization container. When the remaining raw material monomers and / or reagents are added after the start of polymerization, the remaining raw material monomers and / or reagents can be added once or in multiple times, or can be added continuously at a certain flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in portions after the start of polymerization. As an example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of chloroprene can be added in portions after the start of polymerization.
[0132] As an example, the batch addition of the remaining raw material monomers and / or reagents can be started when the polymerization rate of the raw material monomers added before the start of polymerization reaches 50 to 95%. The polymerization rate at the start of the batch addition can be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95%, or can be within the range between any two of the values exemplified here.
[0133] When at least a portion of the raw material monomers is added after the start of polymerization, 50 parts by mass or less of 100 parts by mass of all the raw material monomers used in the polymerization step may be added after the start of polymerization. In this case, the amount of the raw material monomer added after the start of polymerization may be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within the range between any two of the values exemplified herein. As an example, the batch addition of the raw material monomers, such as chloroprene, may be performed continuously within 30 to 300 minutes.
[0134] 2.3 Chloroprene polymer B
[0135] The chloroprene polymer B of one embodiment of the present invention contains at least a chloroprene monomer unit, and may also be a copolymer of chloroprene and other monomers copolymerizable with chloroprene. As other monomers, 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, etc. may be listed, and other monomers may also be used in combination of two or more of them. The chloroprene polymer B of one embodiment of the present invention preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The chloroprene polymer B of one embodiment of the present invention may not contain sulfur, and the chloroprene polymer B of one embodiment of the present invention may also be a polymer having no -SS- structure derived from sulfur in the main chain.
[0136] The chloroprene polymer B of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, when the chloroprene polymer B is 100% by mass. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within the range between any two of the values exemplified herein.
[0137] The chloroprene polymer B of one embodiment of the present invention may contain 0 to 30% by mass of a monomer unit derived from 2,3-dichloro-1,3-butadiene, based on 100% by mass of the chloroprene polymer B. The content of the monomer unit derived from 2,3-dichloro-1,3-butadiene may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the values exemplified herein.
[0138] The chloroprene polymer B of the present invention may have a different weight average molecular weight from the diene polymer A. As described above, the difference between the weight average molecular weight of the diene polymer A of one embodiment of the present invention and the weight average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more.
[0139] As an example, the weight average molecular weight of chloroprene polymer B may be greater than that of diene polymer A. The weight average molecular weight of chloroprene polymer B may be 200,000 to 1,500,000. The weight average molecular weight of chloroprene polymer B may be, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, or may be within the range between any two of the values exemplified herein.
[0140] In addition, as another example, the weight average molecular weight of the chloroprene polymer B may be smaller than the molecular weight of the diene polymer A. The weight average molecular weight of the chloroprene polymer B may be 5,000 to 80,000. The weight average molecular weight of the chloroprene polymer B is, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, The amount may be within a range between any two of the values exemplified herein.
[0141] The weight average molecular weight of chloroprene polymer B can be obtained by using gel permeation chromatography (GPC) to analyze a sample obtained by dissolving chloroprene polymer B in tetrahydrofuran, such as a polymerization solution containing chloroprene polymer B, for example, a chloroprene polymer composition (latex) and a large amount of methanol to precipitate it, filtering and drying it. The measurement conditions of GPC can be described in the examples. The weight average molecular weight of chloroprene polymer B can be controlled by adjusting the polymerization formula, the type and amount of chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. in the polymerization of chloroprene polymer B, and can be controlled by adjusting the type and amount of chain transfer agent.
[0142] 2.4 Method for producing chloroprene polymer B
[0143] The method for producing a chloroprene-based polymer composition according to one embodiment of the present invention may include a polymerization step of polymerizing the chloroprene-based polymer B in the presence of the diene-based polymer A.
[0144] According to one embodiment of the present invention, by polymerizing a chloroprene polymer B in the presence of a diene polymer A, a chloroprene polymer composition can be obtained which can obtain a dip molded product having a low modulus at 100% elongation, excellent tensile strength at break, and a low modulus at 100% elongation after storage at 23°C for 6 months.
[0145] The mechanism by which a chloroprene polymer composition having a low modulus at 100% elongation, a more excellent tensile strength at break, and a dip-molded article having a low modulus at 100% elongation after storage at 23°C for 6 months can be obtained by polymerizing the chloroprene polymer B in the presence of the diene polymer A is not yet clear, but it is presumed that the chloroprene polymer composition obtained by polymerizing the chloroprene polymer B in the presence of the diene polymer A has the diene polymer A and the chloroprene polymer B highly uniformly mixed in the chloroprene polymer composition, as compared with a chloroprene polymer composition obtained by polymerizing the diene polymer A and the chloroprene polymer B separately and mixing them after polymerization, and therefore the obtained chloroprene polymer composition and the obtained dip-molded article have excellent physical properties.
[0146] The diene polymer A can be added to the polymerization solution in any form, for example, the polymerization solution after the polymerization of the diene polymer A can be directly used. As an example, when the diene polymer A is polymerized by emulsion polymerization, the latex containing the diene polymer A can be added to the polymerization solution of the chloroprene polymer B. In addition, for example, the diene polymer A can be precipitated from the polymerization solution after the polymerization of the diene polymer A, and the precipitated diene polymer A can be added to the polymerization solution of the chloroprene polymer B. As an example, when the diene polymer A is polymerized by emulsion polymerization, methanol can be used to precipitate the diene polymer A from the latex containing the diene polymer A and add it to the polymerization solution of the chloroprene polymer B, and the diene polymer A obtained by freeze-drying the latex containing the diene polymer A can be added to the polymerization solution of the chloroprene polymer B.
[0147] In the polymerization step of polymerizing the chloroprene polymer B, when the amount of the chloroprene monomer (or raw material monomer) added is 100 parts by mass, the amount of the diene polymer A added may be 5.0 to 60.0 parts by mass or 40.0 to 95.0 parts by mass.
[0148] In one embodiment of the present invention, when the weight average molecular weight of the diene polymer A is less than the weight average molecular weight of the chloroprene polymer B, for example, when the weight average molecular weight of the diene polymer A is 5,000 to 80,000, the amount of the diene polymer A added may be 5.0 to 60.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) added. When the molecular weight of the diene polymer A is greater than the molecular weight of the chloroprene polymer B, for example, when the weight average molecular weight of the diene polymer A is 200,000 to 1,500,000, the amount of the diene polymer A added may be 40.0 to 95.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) added.
[0149] When the weight average molecular weight of diene polymer A is less than the weight average molecular weight of chloroprene polymer B, the amount of diene polymer A added is, for example, 5.0, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 50.0, 60.0 parts by mass relative to 100 parts by mass of chloroprene monomer (or raw material monomer), or it may be in the range between any two numerical values exemplified herein. When the molecular weight of diene polymer A is greater than the molecular weight of chloroprene polymer B, the amount of diene polymer A added is, for example, 40.0, 50.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, 95.0 parts by mass relative to 100 parts by mass of chloroprene monomer (or raw material monomer), or it may be in the range between any two numerical values exemplified herein.
[0150] In the polymerization step, the raw material monomers include chloroprene and may include other monomers copolymerizable with chloroprene. Examples of other monomers include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, styrene, methacrylic acid, acrylonitrile, sulfur, and the like.
[0151] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer B falls within the above-mentioned numerical range.
[0152] When producing the chloroprene polymer B, the raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization-completed solution, and a relatively high polymerization rate.
[0153] In the polymerization step of the chloroprene polymer B, the raw material monomers can be put into a polymerization container together with necessary reagents such as a polymerization initiator, a chain transfer agent, and a solvent to carry out polymerization. As an example, when the chloroprene polymer B is polymerized by emulsion polymerization, the raw material monomers can be put into a reaction tank together with a chain transfer agent, water, an alkali (for example, a metal hydroxide such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc. to carry out polymerization.
[0154] The polymerization initiator is not particularly limited, and a known polymerization initiator commonly used in the polymerization of chloroprene-based polymers can be used. Examples of the polymerization initiator include organic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide.
[0155] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in the polymerization of chloroprene such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.
[0156] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the chloroprene polymer B obtained can be adjusted.
[0157] As an example, in order to obtain a chloroprene polymer B having a weight average molecular weight of 200,000 or more, preferably a weight average molecular weight of 500,000 to 1,500,000, the amount of the chain transfer agent added is preferably 0 to less than 0.40 parts by mass relative to 100 parts by mass of the monomer. The amount of the chain transfer agent added is more preferably 0 to 0.05 parts by mass, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, 0.30 parts by mass, less than 0.40 parts by mass, and may also be within the range between any two of the values exemplified herein. In addition, when it is particularly desired to obtain a chloroprene polymer B having a weight average molecular weight of 200,000 or more, the chain transfer agent may not be used.
[0158] In addition, as an example, in order to obtain a chloroprene polymer B having a weight average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may be within the range between any two of the values exemplified here.
[0159] By adjusting the weight average molecular weights of the diene polymer A and the chloroprene polymer B within the above numerical range, and adjusting the amount of the diene polymer A added relative to 100 parts by mass of the chloroprene monomer added within the above numerical range, a chloroprene polymer composition can be prepared that can provide a dip-molded article having a lower modulus at 100% elongation and a more excellent tensile strength at break.
[0160] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of the emulsion polymerization, and also includes the case where the composition is changed by adding each component later or adding each component in batches. If the pH of the aqueous emulsion at the start of the emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is 13.5 or less, the excessive increase in viscosity during the polymerization can be suppressed, and the polymerization reaction can be controlled more stably.
[0161] In the polymerization step, the monomers include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above for the monomer units that may be contained in the chloroprene polymer. In addition, it is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above numerical range.
[0162] The emulsifier preferably contains rosin acid and / or rosin salt. Examples of rosin salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin salt added may be 3.0 to 7.0 parts by mass relative to 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, or may be within the range between any two of the values exemplified herein.
[0163] Abietic acid and / or abietic acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. As the conjugated resin acid component, abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof may be cited. As the non-conjugated resin acid component, dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof may be cited.
[0164] The ratio RB / RA of the total amount of peak area RB of rosin acid, neorosin acid, palustric acid, levopimaric acid and their salts obtained by gas chromatography analysis of the extract obtained by extracting the rosin acid and rosin acid salt used in the emulsion polymerization step with an ethanol / toluene azeotropic mixture specified in JIS K 6229 to the total amount of peak area RA of dehydrorosin acid, pimaric acid, isopimaric acid, dihydrorosin acid and their salts may be 0.10 or more and 0.70 or less. The RB / RA of rosin acid and rosin acid salt is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, or may be within the range between any two of the values exemplified herein. By adjusting the type and amount of rosin acid and / or rosin acid salt, the RB / RA of the test dip molded product of the obtained chloroprene polymer composition can be adjusted.
[0165] The emulsifier may also contain emulsifiers and dispersants other than rosin acid and rosin salts. As emulsifiers and dispersants other than rosin acid and rosin salts, cationic, anionic, and nonionic emulsifiers and dispersants can be used. In one embodiment of the present invention, as the emulsifier used in the emulsion polymerization step, rosin acid and / or rosin salts, and anionic emulsifiers and dispersants may be included. As anionic emulsifiers and dispersants, from the viewpoint of stabilizing the chloroprene polymer latex when the pH adjuster is added, it is preferred to use sulfate-based and sulfonate-based anionic emulsifiers and dispersants in combination. Specifically, alkyl sulfonates, alkyl aryl sulfates, condensates of sodium β-naphthalenesulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonate having a carbon number of 8 to 20 can be cited. The amount of anionic emulsifiers and dispersants added can be 0.05 to 5 parts by mass relative to 100 parts by mass of the raw material monomer. The amount of the anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass per 100 parts by mass of the raw monomers, or may be within the range between any two of the values exemplified here.
[0166] The polymerization temperature is preferably in the range of 5 to 55° C. It is more preferred that the polymerization temperature is 5° C. or higher because the emulsion does not freeze, and that the polymerization temperature is 55° C. or lower because the chloroprene monomer does not evaporate or boil.
[0167] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that stops the polymerization reaction.
[0168] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the polymerization, unreacted monomers can be removed by a conventional method such as reduced pressure distillation.
[0169] In addition, to the chloroprene polymer composition (e.g., latex) containing the diene polymer A and the chloroprene polymer B obtained by the production method of one embodiment of the present invention, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be arbitrarily added after polymerization within a range that does not impair the effects of the present invention.
[0170] In the polymerization step of the chloroprene-based polymer B, the polymerization may be started after all the raw material monomers and reagents used in the polymerization step are added to the polymerization container before the start of the polymerization, or at least a portion of the raw material monomers and / or reagents used in the polymerization step may be added to the polymerization container before the start of the polymerization, and the remaining portion may be added after the start of the polymerization.
[0171] Before the start of polymerization, at least a portion of the raw material monomers and reagents are added to the polymerization container. When the remaining raw material monomers and / or reagents are added after the start of polymerization, the remaining raw material monomers and / or reagents can be added once or in multiple times, or can be added continuously at a certain flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers and / or reagents can be added in batches after the start of polymerization. As an example, a portion of the polymerization initiator can be added in batches after the start of polymerization.
[0172] 3. Chloroprene polymer latex
[0173] The chloroprene polymer latex of one embodiment of the present invention may contain a chloroprene polymer composition and water. A latex containing a chloroprene polymer composition containing a diene polymer A and a chloroprene polymer B obtained by polymerizing a chloroprene polymer B may be referred to as a chloroprene polymer latex. When the polymer (e.g., diene polymer A and / or chloroprene polymer B) contained in the chloroprene polymer composition of the present invention is obtained by emulsion polymerization, the chloroprene polymer latex may further contain a raw material used in the emulsion polymerization step such as an emulsifier.
[0174] 4. Dip-molded articles (dip-molded articles coated with films)
[0175] The dip-molded product according to one embodiment of the present invention may be a dip-molded product of a composition for forming a dip-molded product containing a chloroprene-based polymer latex.
[0176] The dip-molded article of one embodiment of the present invention is obtained by using the above-mentioned chloroprene polymer composition. The dip-molded article can be obtained by dip-molding the composition for forming a dip-molded article described later alone or mixed with other compositions for forming a dip-molded article. The dip-molded article of the present invention can be a dip-molded article obtained by heat-drying the dip-molded article obtained by dip-molding the composition for forming a dip-molded article by dip coagulation method at 140°C for 1 hour. The dip-molded article of the present invention has high tensile strength at break, low modulus at 100% elongation, and low modulus at 100% elongation after long-term storage. The dip-molded article of one embodiment of the present invention can be suitably used as industrial / general household gloves, medical gloves, balloons, catheters and boots.
[0177] The dip molded article of the present invention may contain the components contained in the above-mentioned dip molded article forming composition. In addition, the dip molded article may contain diene polymer A and chloroprene polymer B as base polymers, and when the dip molded article is set to 100% by mass, it may contain more than 70% by mass of diene polymer A and chloroprene polymer B, preferably more than 80% by mass, and more preferably more than 90% by mass. When the dip molded article is set to 100% by mass, the content of diene polymer A and chloroprene polymer B in the dip molded article is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, 100% by mass, and may also be within the range between any two values exemplified herein.
[0178] The dip-molded article containing the chloroprene polymer of the present invention has high tensile strength at break, low modulus at 100% elongation, and low modulus at 100% elongation after long-term storage, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. In addition, the dip-molded article of one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, or other vulcanization accelerator.
[0179] 4.1 Characteristics of Dip-molded Products
[0180] The dip molded product of one embodiment of the present invention preferably has a peak with a weight average molecular weight of 5,000 to 80,000 detected in the molecular weight distribution obtained by gel permeation chromatography of the soluble component obtained by dissolving the dip molded product in tetrahydrofuran, preferably has a peak with a weight average molecular weight of 5,000 to 80,000 and a peak with a weight average molecular weight of 200,000 to 1,500,000 detected, more preferably has a peak with a weight average molecular weight of 5,000 to 50,000 and a peak with a weight average molecular weight of 300,000 to 1,500,000 detected, and further preferably has a peak with a weight average molecular weight of 8,000 to 30,000 and a peak with a weight average molecular weight of 500,000 to 1,500,000 detected. The weight average molecular weight and blending ratio of the low molecular weight component and the high molecular weight component may be as described above.
[0181] The dip molded article according to one embodiment of the present invention preferably has a toluene swelling degree of 12.0 or less, more preferably 10.0 or less. The toluene swelling degree is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, or 12.0, or may be within the range between any two of the values exemplified herein.
[0182] The dip molded article of one embodiment of the present invention preferably has a low temperature hardness change ΔH2 of 30 or less, more preferably 20 or less. The low temperature hardness change ΔH2 is, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, and may be within the range between any two of the values exemplified here. The hardness change ΔH2 is expressed as HB2-HA2. HA2 indicates the Shore hardness measured at 23°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm. HB2 indicates the Shore hardness measured at -10°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and then overlapped to a thickness of 6.00±0.20 mm.
[0183] The dip molded article according to one embodiment of the present invention preferably has a ratio RB / RA of the total amount of peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount of peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, obtained by gas chromatography analysis of an extract obtained by extraction with an ethanol / toluene azeotropic mixture specified in JIS K 6229, of 0.10 to 0.70, more preferably 0.15 to 0.50. RB / RA is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, and may be within the range between any two of the values exemplified herein.
[0184] The dip molded article according to one embodiment of the present invention preferably has a tensile strength at break measured according to JIS K 6251 of 18.0 MPa or more, more preferably 19.0 MPa or more, and further preferably 20.0 MPa or more. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within the range between any two of the values exemplified herein.
[0185] The dip molded article of one embodiment of the present invention preferably has a modulus of 0.65 MPa or less, more preferably 0.60 MPa or less at 100% elongation measured according to JIS K 6251. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, and may be within the range between any two of the values exemplified herein.
[0186] The dip molded article according to one embodiment of the present invention preferably has a modulus of 0.80 MPa or less, more preferably 0.70 MPa or less, at 100% elongation measured according to JIS K 6251 after storage at 23° C. for 6 months. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, or 1.00 MPa, and may be within the range between any two of the values exemplified herein.
[0187] The weight average molecular weight, toluene swelling degree, low temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months of the dip-molded product are determined by the same method as described in the item of the chloroprene polymer composition.
[0188] The dip-molded article of one embodiment of the present invention may be an dip-molded article having a low-temperature hardness change of 30 or less, and a tensile strength at break measured according to JIS K6251 of 18.0 MPa or more. The dip-molded article of one embodiment of the present invention may be an dip-molded article having a low-temperature hardness change of 30 or less, a tensile strength at break measured according to JIS K 6251 of 18.0 MPa or more, and a modulus at 100% elongation of 0.65 MPa or less. In addition, the dip-molded article of one embodiment of the present invention may satisfy any two or more, three or more, four or more, five or more, six or more requirements of the weight average molecular weight of the dip-molded article, the degree of swelling in toluene, the low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months, or all of the above requirements.
[0189] The dip molded article of one embodiment of the present invention contains a chloroprene polymer composition and may further contain an antioxidant and a metal oxide. In addition, the dip molded article may contain a vulcanizing agent, a vulcanization accelerator and an anti-aging agent. The manufacturing method of the dip molded article may be described in the examples.
[0190] In addition, the weight average molecular weight, toluene swelling degree, low temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 100% elongation, and modulus at 100% elongation after storage at 23°C for 6 months of the dip-molded product can be controlled by adjusting the production method of the chloroprene polymer composition, for example, adjusting the type and amount of raw materials formulated when polymerizing the diene polymer A and the chloroprene polymer, the type and amount of the reagents used, and the polymerization conditions.
[0191] 4.2 Shape of the Dip-molded Product
[0192] The thickness of the dip-molded article (e.g., minimum thickness) may be 0.01 to 0.50 mm. The thickness of the dip-molded article may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, or may be within the range between any two of the values exemplified herein. The thickness of the dip-molded article may be adjusted by the time the molding die is immersed in the composition for forming the dip-molded article, the solid content concentration of the composition for forming the dip-molded article, and the like. When the thickness of the dip-molded article is to be reduced, the immersion time may be shortened or the solid content concentration of the composition for forming the dip-molded article may be reduced.
[0193] The dip molded article may also contain sulfur or a vulcanization accelerator. However, even if the dip molded article does not contain sulfur and a vulcanization accelerator, it may have mechanical properties equivalent to or better than those of a vulcanized dip molded article obtained from a composition for forming a dip molded article containing a conventional chloroprene polymer. Therefore, the chloroprene polymer composition of the present invention is suitable for use as a raw material for the dip molded article (dipping molded article) of the chloroprene polymer of the present embodiment.
[0194] 5. Method for producing dip-molded article
[0195] The method for producing a dip-molded article according to one embodiment of the present invention may include:
[0196] a dip molding step of dip molding a composition for forming a dip molded body containing the above-described chloroprene polymer composition to obtain a dip molded body; and
[0197] The drying step is to heat and dry the impregnation molded body to obtain an impregnation molded article.
[0198] 5.1 Composition for forming an impregnated molded body
[0199] The composition for forming a dip molded body according to one embodiment of the present invention contains the chloroprene polymer composition described above. The composition for forming a dip molded body according to one embodiment of the present invention may contain a metal oxide, an antioxidant, and other necessary reagents in addition to the chloroprene polymer composition. The composition for forming a dip molded body according to one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, etc.
[0200] 5.1.1 Metal oxides
[0201] The composition for forming an impregnation molded body according to one embodiment of the present invention may contain a metal oxide.
[0202] The metal oxide is not particularly limited, and zinc oxide, lead oxide, lead tetraoxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, titanium oxide, etc. can be cited. The metal oxide preferably contains zinc oxide. Zinc oxide is generally considered to function as a supplement for the dechlorination of chloroprene polymers. In addition, these metal oxides can be used alone or in combination of two or more.
[0203] The amount of the metal oxide added is preferably 0.5 to 15.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming the dip molded body. If the amount of the metal oxide added is 0.5 parts by mass or more, an improvement in the tensile strength at break can be expected due to the crosslinking effect between the polymers. If the amount of the metal oxide added is 15.0 parts by mass or less, a dip molded product with excellent flexibility can be obtained. In addition, from the viewpoint of the physical balance between the flexibility and tensile strength at break of the obtained dip molded product, the amount of the metal oxide added is more preferably 0.5 to 5.0 parts by mass.
[0204] 5.1.2 Antioxidants
[0205] The composition for forming a dip molded article according to one embodiment of the present invention may also contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine antioxidants, heat-resistant antioxidants (aging) agents, ozone-resistant antioxidants, etc. can be used. When the obtained dip molded article is used for medical gloves, a phenolic antioxidant can be used from the viewpoint of color tone, texture, and sanitation of the dip molded article. In particular, hindered phenolic antioxidants have a strong effect as described above. As hindered phenol antioxidants, for example, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylene(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-tert-butylhydroquinone, and 2,5'-di-tert-amylhydroquinone can be cited. Among them, butylated reaction products of p-cresol and dicyclopentadiene are generally preferred from the viewpoint of being dispersible in aqueous materials. In addition, these compounds may be used alone or in combination of two or more.
[0206] The amount of the antioxidant added is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip molded body. The amount of the antioxidant added is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, or it may be within the range between any two of the values exemplified herein. If the amount of the antioxidant added is 0.5 parts by mass or more, the effect of suppressing the change in color tone of the dip molded product can be obtained. If the amount of the antioxidant added is 10.0 parts by mass or less, the stability of the composition for forming a dip molded product can be ensured. In addition, from the viewpoint of the balance of the physical properties of the softness and tensile strength at break of the obtained dip molded product, the amount of the antioxidant added is more preferably 0.5 to 5.0 parts by mass.
[0207] 5.1.3 Vulcanizing agents and vulcanization accelerators
[0208] The composition for forming a dip molded body according to one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. In addition, the composition for forming a dip molded body according to one embodiment of the present invention may also be free of sulfur and the above-mentioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based and other vulcanization accelerators. That is, the composition for forming a dip molded body includes a composition containing a vulcanizing agent but not containing a vulcanization accelerator, a composition containing no vulcanizing agent but containing a vulcanization accelerator, a composition containing a vulcanizing agent and a vulcanization accelerator, and a composition containing no vulcanizing agent and a vulcanization accelerator. Whether to prepare a vulcanizing agent and a vulcanization accelerator can be determined according to the expected dip molded product.
[0209] Examples of the vulcanizing agent include sulfur, but are not limited thereto. The amount of the vulcanizing agent added may be 0 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming the dip molded body. The amount of the vulcanizing agent added may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, or may be within the range between any two of the values exemplified herein.
[0210] Vulcanization accelerator refers to a reagent added during the vulcanization of raw rubber to increase the vulcanization rate by reacting with the vulcanizing agent, shorten the vulcanization time, lower the vulcanization temperature, reduce the vulcanizing agent, and improve the physical properties of the vulcanized rubber. It usually refers to a reagent that promotes sulfur vulcanization reaction.
[0211] Examples of the vulcanization accelerator include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, and thiazole-based accelerators, and these may be used alone or in combination of two or more as needed.
[0212] Examples of the thiuram-based vulcanization accelerator include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and bis(pentamethylene)thiuram tetrasulfide.
[0213] Examples of the dithiocarbamate-based vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, iron (III) dimethyldithiocarbamate, tellurium diethyldithiocarbamate, and the like. Zinc dibutyldithiocarbamate is particularly preferably used.
[0214] Examples of the thiourea-based vulcanization accelerator include ethylenethiourea, N,N′-diethylthiourea, trimethylthiourea, and N,N′-diphenylthiourea.
[0215] Examples of the guanidine-based vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salt of dicatechol borate.
[0216] Examples of the xanthate-based vulcanization accelerator include butyl zinc xanthate and isopropyl zinc xanthate.
[0217] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, and 2-(4′-morpholinodithio)benzothiazole.
[0218] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip molded body. The amount of the vulcanization accelerator added may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or may be within the range between any two of the values exemplified herein.
[0219] 5.1.4 Other reagents (aromatic heterocyclic compounds)
[0220] The composition for forming a dip molded article according to one embodiment of the present invention may contain an aromatic heterocyclic compound in the chloroprene polymer.
[0221] The aromatic heterocyclic compound contained in the dip-molded article forming composition for obtaining the dip-molded article of one embodiment of the present invention can be represented by chemical formula (1) and has a benzimidazole structure. In addition, the compound having this structure is sometimes mainly used as a secondary antioxidant in the preparation of the rubber composition.
[0222] [Chemistry 1]
[0223]
[0224] In the chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a group having a thiol group and a hydrogen atom. In addition, X may be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, and zinc is preferred.
[0225] In the chemical formula (1), R1 to R4 each represent a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. R1 to R4 may be the same or different. In addition, the aromatic heterocyclic compound may be used alone or in combination of two or more.
[0226] As aromatic heterocyclic compounds, for example, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxyl-2-mercaptobenzimidazole, or zinc salts of 2-mercaptobenzimidazole can be cited. Among them, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.
[0227] The amount of the aromatic heterocyclic compound added is preferably 0.2 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming the dip molded body. The amount of the aromatic heterocyclic compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, or it may be in the range between any two of the values exemplified herein. If the amount added is 0.2 parts by mass or more, the dip molded product obtained using the composition exhibits very high fracture strength. If the amount added is 10.0 parts by mass or less, the stability of the composition for forming the dip molded body can be ensured. In addition, from the viewpoint of the physical balance of the softness and fracture strength of the obtained dip molded product, the amount added is more preferably 0.3 to 5.0 parts by mass.
[0228] The method for producing a composition for forming an impregnated molded article according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene-based polymer composition, a metal oxide, an antioxidant, and other necessary reagents.
[0229] In the mixing step, an aqueous dispersion containing the metal oxide, the antioxidant, and other necessary reagents may be prepared in advance, and then the chloroprene polymer composition and the aqueous dispersion may be mixed.
[0230] The mixing step can be performed using a known mixing device such as a ball mill.
[0231] 5.2 Dipping molding steps
[0232] The method for producing a dip-molded article according to one embodiment of the present invention may include a dip-molding step of dip-molding a composition for forming a dip-molded article containing a chloroprene polymer composition obtained by the method for producing a chloroprene polymer composition described above to obtain a dip-molded article.
[0233] As the method of dip molding of one embodiment of the present invention, for example, dip coagulation method, simple dip method, thermosensitive dip method, electrodeposition method etc. can be cited. From the viewpoint of easy manufacture and easy acquisition of a certain thickness of dip molded body, dip coagulation method can be used. Specifically, the ceramic forming mold coated with calcium system coagulation liquid is immersed in the dip molded body forming composition, and the dip molded body forming composition is solidified. Then, it is dried after removing water-soluble impurities by leaching, and then formed into dip molded film (rubber coating) by heating and vulcanization, and then the dip molded film is demoulded. Thus, a film-like dip molded body can be obtained.
[0234] 5.3 Drying step
[0235] The method for producing a dip-molded article according to one embodiment of the present invention may include a drying step of heating and drying the dip-molded body to obtain the dip-molded article.
[0236] The heating and drying temperature can be appropriately set according to the composition of the chloroprene polymer composition, and can be 120 to 180° C. The heating temperature is preferably 120 to 150° C. The heating temperature is, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220° C., and can also be within the range between any two values exemplified herein. The heating time can be appropriately set according to the composition of the chloroprene polymer composition, the shape of the unvulcanized molded body, etc., and can be 10 to 300 minutes. The heating time is, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 minutes, and may be within the range between any two of the values exemplified herein. As an example, the dip molded article of one embodiment of the present invention may be obtained by heat drying at 140° C. for 1 hour.
[0237] [Example]
[0238] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0239] <Preparation of Chloroprene-Based Polymer A>
[0240] (Synthesis Example A-1)
[0241] In a polymerization tank with an internal volume of 30 L, 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Co., Ltd.), and 0.5 parts by mass of sodium hydrogen sulfite were added. At a polymerization temperature of 35° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator and polymerization was carried out. At the point where the polymerization rate of the added monomer reached 80%, 27 parts by mass of chloroprene (monomer) were continuously added for 100 minutes. When the polymerization rate of the initially added monomers and the continuously added monomers reached 91%, the addition of the potassium persulfate aqueous solution was stopped to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-1 having a solid content concentration of 60% by mass was obtained by concentration operation. In addition, a part of the obtained latex was used to precipitate chloroprene polymer A-1 by the method described later, and was used for analysis and the preparation of chloroprene polymer B in Examples 1, 2 and 8.
[0242] (Precipitation of Chloroprene Polymer A Using Methanol)
[0243] The obtained latex of chloroprene polymer A-1 was mixed with a large amount of methanol to precipitate the rubber component (chloroprene polymer A-1), filtered and dried to obtain a sample of chloroprene polymer A-1. The sample was also used in the preparation of chloroprene polymer B in Examples 1, 2 and 8 described below.
[0244] (Synthesis Example A-2)
[0245] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the amount of n-dodecyl mercaptan in Synthesis Example A-1 was changed to 5.3 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-2 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-2 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B in Example 3.
[0246] (Synthesis Example A-3)
[0247] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the amount of n-dodecyl mercaptan in Synthesis Example A-1 was changed to 2.4 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-3 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-3 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B in Example 4.
[0248] (Synthesis Example A-4)
[0249] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the amount of n-dodecyl mercaptan in Synthesis Example A-1 was changed to 1.5 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-4 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-4 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B in Example 5.
[0250] (Synthesis Example A-5)
[0251] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the chloroprene (monomer) initially added was changed to 70 parts by mass, 2,3-dichloro-1,3-butadiene was changed to 0 parts by mass, and the chloroprene (monomer) continuously added during the polymerization was changed to 30 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-5 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-5 in the same manner as in Synthesis Example A1, and was used to prepare chloroprene polymer B in Example 6.
[0252] (Synthesis Example A-6)
[0253] In a polymerization tank having an internal volume of 30 L, 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite were added. Polymerization was carried out by continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator at a polymerization temperature of 35° C. under a nitrogen gas flow. When the polymerization rate of the added monomer reached 80%, 27 parts by mass of chloroprene (monomer) were continuously added over 100 minutes. When the polymerization rate of the initially added monomers and the continuously added monomers reached 91%, the addition of the potassium persulfate aqueous solution was stopped to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-6 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-6 in the same procedure as in Synthesis Example A1, and was used to prepare chloroprene polymer B in Example 7.
[0254] <Preparation of Chloroprene Polymer B and Chloroprene Polymer Composition>
[0255] (Example 1)
[0256] In a polymerization tank having an internal volume of 30 L, 1.3 parts by mass of chloroprene polymer A-12 prepared and precipitated in Synthesis Example A-1, 85 parts by mass of chloroprene (monomer), 15 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 5.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 2 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization to obtain a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-1 having a solid content concentration of 60% by weight was obtained by concentration.
[0257] 50 ml of the chloroprene-based polymer latex was sampled, and the remaining chloroprene-based polymer latex was used to prepare a dip-molded article for a test.
[0258] The sampled chloroprene polymer latex is mixed with a large amount of methanol to precipitate the rubber component, and the mixture is filtered and dried to obtain a sample of the chloroprene polymer composition. The weight average molecular weight of the chloroprene polymer composition is measured for the obtained sample. In addition, the chloroprene polymer composition obtained by freeze-drying the chloroprene polymer latex is measured for 2,3-dichloro-1,3-butadiene content and toluene insoluble matter. The analysis results are shown in Table 1. In addition, the measurement method is described below. The weight average molecular weight of the chloroprene polymer composition of Example 1 was measured, and the peak from the chloroprene polymer A with a weight average molecular weight of 5,000 to 80,000 and the peak from the chloroprene polymer B with a weight average molecular weight of 200,000 to 1,500,000 were confirmed.
[0259] (Example 2)
[0260] The polymerization was carried out in the same procedure as in Example 1 except that the chloroprene (monomer) in Example 1 was changed to 91 parts by mass and the 2,3-dichloro-1,3-butadiene was changed to 9 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing a chloroprene polymer B-2 with a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight of the chloroprene polymer composition, the content of 2,3-dichloro-1,3-butadiene and the toluene insoluble content were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0261] (Example 3)
[0262] In a polymerization tank with an internal volume of 30 L, 21.3 parts by mass of chloroprene polymer A-2 prepared and precipitated in Synthesis Example A-2, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 5.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 2 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Co., Ltd.), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator to carry out polymerization. At the point where the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization solution. The polymer solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-2 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0263] (Example 4)
[0264] The polymerization was carried out in the same procedure as in Example 3 except that the chloroprene polymer A-2 in Example 3 was changed to chloroprene polymer A-3. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-4 with a solid content concentration of 60% by mass was obtained by concentration operation. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0265] (Example 5)
[0266] The polymerization was carried out in the same procedure as in Example 3 except that the chloroprene polymer A-2 in Example 3 was changed to chloroprene polymer A-4. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-5 with a solid content concentration of 60% by mass was obtained by concentration operation. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0267] (Example 6)
[0268] The polymerization was carried out in the same procedure as in Example 3 except that the chloroprene polymer A-2 in Example 3 was changed to chloroprene polymer A-5. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-6 with a solid content concentration of 60% by mass was obtained by concentration operation. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0269] (Example 7)
[0270] In a polymerization tank having an internal volume of 30 L, 21.3 parts by mass of chloroprene polymer A-6 prepared and precipitated in Synthesis Example A-6, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOLN", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-7 having a solid content concentration of 60% by weight is obtained by concentration. The obtained latex is used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition are measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0271] (Example 8)
[0272] In a polymerization tank having an internal volume of 30 L, 45.8 parts by mass of the chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 120 parts by mass of pure water, 6.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 2.4 parts by mass of potassium hydroxide, 0.6 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.6 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-8 having a solid content concentration of 60% by weight is obtained by concentration. The obtained latex is used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition are measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0273] (Comparative Example 1)
[0274] In a polymerization tank with an internal volume of 30 L, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Co., Ltd.), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator and polymerization was carried out. At the point where the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization solution. The polymer solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing a chloroprene polymer C having a solid content concentration of 60% by mass was obtained by concentration. In addition, the obtained chloroprene polymer composition was used to prepare a test dip-molded article. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1. In addition, a portion of the obtained chloroprene polymer composition was used in Comparative Example 2.
[0275] (Comparative Example 2)
[0276] The polymerization was carried out in the same manner as in Synthesis Example A1. The obtained polymerization solution was distilled under reduced pressure to remove unreacted monomers, and concentrated to obtain a chloroprene polymer composition containing the chloroprene polymer D having a solid content concentration of 60% by mass.
[0277] The chloroprene polymer composition of chloroprene polymer C obtained in Comparative Example 1 and the chloroprene polymer composition of chloroprene polymer D were mixed at a mass ratio of C / D=80 / 20 to obtain a chloroprene polymer composition of chloroprene polymer E. A test dip-molded article was prepared using the obtained chloroprene polymer composition.
[0278] (Comparative Example 3)
[0279] In a polymerization tank with an internal volume of 30 L, 85 parts by mass of chloroprene polymer A-1 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 150 parts by mass of pure water, 8.5 parts by mass of conjugated resin acid-based rosin acid (trade name "HARTALL R-WW", manufactured by Harima Chemicals Co., Ltd.), 3 parts by mass of potassium hydroxide, 0.7 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Co., Ltd.), 0.7 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator to carry out polymerization. At a point when the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization solution. The polymer solution was subjected to reduced pressure distillation to remove unreacted monomers, and a chloroprene polymer composition containing chloroprene polymer B-9 having a solid content concentration of 60% by mass was obtained by concentration. The obtained latex was used to prepare a test dip molding in the same manner as in Example 1. In addition, the weight average molecular weight, 2,3-dichloro-1,3-butadiene content, and toluene insoluble content of the chloroprene polymer composition were measured in the same manner as in Example 1. The analysis results are shown in Table 1.
[0280] The analysis of the chloroprene-based polymer composition was carried out by the following method.
[0281] <Measurement of Weight Average Molecular Weight of Chloroprene Polymer Composition>
[0282] As described above, the weight average molecular weight is measured by gel permeation chromatography (GPC) under the following measurement conditions using a sample obtained by dissolving a polymer obtained by precipitating the chloroprene polymer composition with methanol, filtering and drying it in 20 ml of tetrahydrofuran.
[0283] Device name: HLC-8320 (manufactured by Tosoh Corporation)
[0284] Chromatographic columns: 3 TSKgel GMHHR-H connected in series
[0285] Temperature: 40℃
[0286] Detection: Differential Refractive Index
[0287] Solvent: Tetrahydrofuran
[0288] Calibration curve: Prepared using standard polystyrene (PS).
[0289] <Determination of 2,3-dichloro-1,3-butadiene content in chloroprene polymer composition>
[0290] A chloroprene polymer composition obtained by freeze-drying a latex containing a chloroprene polymer composition was cut into a test piece of 0.05 mg, and measured by a pyrolysis gas chromatography-mass spectrometer to obtain the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. Using a calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the 2,3-dichloro-1,3-butadiene content, the content (mass %) of the 2,3-dichloro-1,3-butadiene monomer unit relative to 100 mass % of the total of the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit was obtained.
[0291] [Pyrolysis gas chromatography mass spectrometry conditions]
[0292] Device name: HP5890-II
[0293] Chromatographic column: DB-5 (Film thickness 1.0μm)
[0294] Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃
[0295] Inlet temperature: 250℃
[0296] Detector temperature: 280°C
[0297] Detector: FID
[0298] <Toluene insoluble content>
[0299] The chloroprene polymer composition obtained by freeze-drying the latex containing the chloroprene polymer composition is cut into 2 mm squares to obtain a test piece. After the test piece is placed in a conical beaker, 80 g of toluene is used to dissolve the test piece for 16 hours. After that, centrifugation is performed and the gel component (insoluble fraction) is separated using a 200-mesh metal mesh. Then, the mass of the dried product is measured after the gel component is dried. When the freeze-dried chloroprene polymer composition is set as Ag and the gel component (insoluble fraction) separated from the mixture dissolved in toluene is set as Bg, the toluene insoluble fraction in the chloroprene polymer composition is calculated by the following formula.
[0300] Toluene insoluble matter (gel component) = B / A x 100 (%)
[0301] The test dip-molded article was prepared by the following method using the above-mentioned latex, i.e., a latex containing a chloroprene-based polymer composition, and the composition was dip-molded to obtain a dip-molded article. The dip-molded article was heat-dried to produce a test dip-molded article and evaluated.
[0302] <Preparation of Dip Molded Product>
[0303] 100 parts by mass of the solid content of each chloroprene polymer composition containing a chloroprene polymer was mixed with an aqueous dispersion, and water was added to adjust the total solid content concentration of the formulation to 30% by mass, thereby preparing a composition for forming a test dip molded body. The aqueous dispersion was prepared by mixing 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1.0 part by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an aromatic heterocyclic compound, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 10.7 parts by mass of water at 20° C. for 16 hours using a ceramic ball mill. The obtained test dip molded body forming composition contained 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 1.0 part by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an aromatic heterocyclic compound, 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and water, based on 100 parts by mass of the solid content of the chloroprene polymer composition.
[0304] A ceramic cylindrical model with an outer diameter of 50 mm (manufactured by Shinko Co., Ltd.) was immersed in a coagulation solution prepared by mixing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate for 1 second and then taken out. After drying for 3 minutes, it was immersed in the composition for forming a test impregnated molded body prepared according to the above procedure for 2 minutes. Then, it was washed with running water at 45°C for 1 minute and dried at 140°C for 1 hour to prepare a test impregnated molded body film.
[0305] (film thickness)
[0306] The thickness (film thickness) of the test dip-molded product film for evaluation of tensile properties was measured at three locations in the center using a test piece thickness meter (manufactured by Kobun Keiki Co., Ltd., trade name: ASKER SDA-12), and the minimum thickness was taken as the thickness of the test dip-molded product. The results are shown in Table 1.
[0307] (Determination of tensile properties)
[0308] Using the test dip-molded film for evaluating tensile properties, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. In addition, the test dip-molded composition of each example and comparative example was stored at 23° C. for 6 months, and the modulus at 100% elongation was measured in accordance with JIS K 6251. The results are shown in Table 1.
[0309] (Toluene swelling degree)
[0310] The test impregnation molded product was cut into 10 mm × 15 mm to obtain a test piece. The mass W1 of the obtained test piece before immersion was measured, and then the test piece was immersed in toluene at 23°C for 20 hours. The test piece after immersion was taken out from the toluene, the toluene on the surface of the film was wiped off, and the mass W2 after immersion was measured. The toluene swelling degree was calculated from the measured mass W1 before immersion and the mass W2 after immersion according to the following formula. The results are shown in Table 1.
[0311] Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r)
[0312] P1: Specific gravity of the rubber component of the chloroprene polymer composition
[0313] P2: specific gravity of toluene
[0314] r: Mass fraction of the rubber component of the chloroprene polymer composition in the dip-molded article
[0315] In addition, calculation was performed with P1 set to 1.23 and P2 set to 0.867. The rubber component of the chloroprene polymer composition refers to the chloroprene polymer in the latex containing the chloroprene polymer composition, which can be obtained by mixing the latex containing the chloroprene polymer composition of the examples and comparative examples with methanol to precipitate, filtering and drying. The specific gravity of the rubber component of the chloroprene polymer composition is calculated by measuring the density of the rubber component of the chloroprene polymer composition obtained by the above method at room temperature (20°C).
[0316] (Change in low temperature hardness)
[0317] The test dip-molded product was stored at -10°C for 168 hours, and the change in low temperature hardness was calculated from the hardness of the test dip-molded product before and after storage according to formula (2).
[0318] Formula (2): ΔH = HB - HA
[0319] In formula (2), HA represents the Shore hardness measured at 23°C using a type A durometer after the test dip-molded product that was previously stored at -10°C for 168 hours was heated at 70°C for 30 minutes, and then the test dip-molded product was overlapped to a thickness of 6.00±0.20 mm. HB represents the Shore hardness measured at -10°C using a type A durometer after the test dip-molded product that was previously stored at -10°C for 168 hours was heated at 70°C for 30 minutes, and then the test dip-molded product was overlapped to a thickness of 6.00±0.20 mm. For example, when the thickness of the test dip-molded product is 0.20 mm, 30 test dip-molded products are overlapped and the hardness is measured.
[0320] (RB / RA, ratio of the total peak area of RB of abietic acid, neoabietic acid, palustric acid, levorotatory pimaric acid and their salts to the total peak area of RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts)
[0321] 3 g of the test impregnation molded product was cut into 2 mm squares to obtain test pieces. The test piece was placed in an eggplant-shaped flask with a condenser, extracted with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229 and treated with hydrochloric acid, and the obtained extract was subjected to gas chromatography measurement under the following conditions. The total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts was determined from the gas chromatography measurement results. In addition, the total amount RB of the peak areas of rosin acid, neorosin acid, palustric acid, levopimaric acid and their salts was determined, and the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of rosin acid, neorosin acid, palustric acid, levopimaric acid and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts in the test impregnated molded product was calculated.
[0322] [Gas chromatography measurement conditions]
[0323] Use column: FFAP (Film thickness 0.3μm)
[0324] Detector: FID
[0325] Column temperature: 200℃ (maintained for 90min) → 250℃ Heating rate: 10℃ / min Inlet temperature: 270℃ Detector temperature: 270℃ Injection volume: 2μL [Table 1]
[0326]
Claims
1. A chloroprene polymer composition comprising a chloroprene polymer, When the tetrahydrofuran-soluble component of the chloroprene polymer composition is measured by gel permeation chromatography, a peak having a weight average molecular weight of 5,000 to 80,000 is detected. The toluene swelling degree of the test dip-molded product of the chloroprene-based polymer composition is 12.0 or less, The test dip-molded article is obtained by molding the test dip-molded article composition by an immersion coagulation method and performing a heat drying treatment at 140° C. for 60 minutes. The test dip molded body forming composition contains 2 parts by mass of zinc oxide, 2 parts by mass of a butylation reaction product of p-cresol and dicyclopentadiene, 1.0 parts by mass of 2-mercaptobenzimidazole, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate, and water, relative to 100 parts by mass of the solid content of the chloroprene polymer composition, wherein the amount of the water is adjusted so that the solid content concentration of the test dip molded body forming composition becomes 30% by mass. The toluene swelling degree is represented by formula (1): Formula (1): Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r) In formula (1), W1 represents the mass of the test dip-molded product before immersing the test dip-molded product in toluene, W2 represents the mass of the test dip-molded product after immersing the test dip-molded product in toluene, P1 represents the specific gravity of the rubber component of the chloroprene polymer composition, P2 represents the specific gravity of toluene, r represents the mass fraction of the rubber component of the chloroprene polymer composition in the test dip-molded product.
2. The chloroprene polymer composition according to claim 1, wherein The toluene insoluble content is 50 to 90% by mass.
3. The chloroprene polymer composition according to claim 1 or 2, wherein The chloroprene polymer composition contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The chloroprene polymer composition contains 8 to 20% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units.
4. The chloroprene polymer composition according to claim 1 or 2, wherein The low temperature hardness change ΔH1 of the test dip-molded article is 30 or less, The low temperature hardness change ΔH1 is expressed as HB1-HA1, HA1 represents the Shore hardness measured at 23°C using a type A durometer after the test dip-molded product is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm. HB1 represents the Shore hardness measured at -10°C using a type A hardness meter after heating the test dip-molded product at 70°C for 30 minutes and storing the test dip-molded product at -10°C for 168 hours, overlapping the test dip-molded product to a thickness of 6.00±0.20 mm.
5. The chloroprene polymer composition according to claim 1 or 2, wherein The ratio RB / RA of the total amount of peak area RB of abietic acid, neoabietic acid, palustric acid, levorotatory pimaric acid and their salts to the total amount of peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, obtained by gas chromatography analysis of an extract obtained by extracting the test impregnated molded product with an ethanol / toluene azeotropic mixture specified in JIS K 6229, is 0.10 or more and 0.70 or less.
6. A chloroprene polymer latex, The invention comprises the chloroprene polymer composition according to claim 1 or 2 and water.
7. A dip-molded article, This is a dip-molded product comprising the composition for forming a dip-molded product according to claim 6, which comprises the chloroprene polymer latex.
8. The dip-molded article according to claim 7, These are industrial / general household gloves, medical gloves, balloons, catheters or boots.
9. The dip-molded article according to claim 7, wherein Low temperature hardness change ΔH2 is less than 30, The low temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 represents the Shore hardness measured at 23°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm. HB2 represents the Shore hardness measured at -10°C using a type A durometer after the dip-molded product is heated at 70°C for 30 minutes and then stored at -10°C for 168 hours and then overlapped to a thickness of 6.00±0.20 mm.
10. A dip-molded product, which is a dip-molded product of a composition for forming a dip-molded product containing a chloroprene polymer latex, The low temperature hardness of the dip-molded article changes to less than 30, The low temperature hardness change ΔH2 is expressed as HB2-HA2, HA2 represents the Shore hardness measured at 23°C using a type A durometer after the dip-molded article is heated at 70°C for 30 minutes and then overlapped to a thickness of 6.00±0.20 mm. HB2 represents the Shore hardness measured at -10°C using a type A durometer after the dip-molded product is heated at 70°C for 30 minutes and stored at -10°C for 168 hours, and then the dip-molded product is overlapped to a thickness of 6.00±0.20 mm. The dip-molded product has a tensile strength at break measured in accordance with JIS K 6251 of 18.0 MPa or more and a modulus at 100% elongation of 0.65 MPa or less.