Method for producing polyester film using recovered polyester resin, and polyester film
By mixing and melting the recovered polyester resin with the polyester resin of aluminum compound and phosphorus compound, the problems of deterioration and molecular weight reduction in the recycling and reuse of polyester resin are solved, and efficient reuse and performance improvement of the polyester film is achieved .
Patent Information
- Application Number
- CN202380030104.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-12
AI Technical Summary
When the conventional polyester resin is recycled and reused, deterioration caused by antimony compound, titanium compound or germanium compound catalyst leads to the coloring and molecular weight of the polyester resin, which affects the strength and reuseability of the film.
By mixing the recovered polyester resin with a polyester resin containing an aluminum compound and a phosphorus compound and melt forming, a polyester film with excellent reuseability, coloring and less strength are produced.
When recycling polyester resin as raw material, the polyester film has less resin deterioration, reduced molecular weight and reduced mechanical strength, and improved the reusability and performance of the polyester film.
Smart Images

Figure BDA0005057758440000151 
Figure BDA0005057758440000161 
Figure BDA0005057758440000171
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a polyester film comprising recycled polyester resin. Background Art
[0002] Polyester resins represented by polyethylene terephthalate (PET) and polyethylene naphthalate (PEN) have excellent transparency, mechanical properties and chemical properties. Based on the properties of various polyester resins, they are widely used in various fields, such as fibers for clothing or industrial resources, various films or sheets for packaging or industrial use, and hollow molded bodies such as bottles or engineering plastics.
[0003] In recent years, hollow molded bodies made of, for example, polyester resins have become indispensable to our lives. On the one hand, the increase in the use of hollow molded bodies has caused various problems such as resource depletion, increase in marine waste, and global warming. As one of the methods to solve this problem, the so-called recycling / recycling system that recycles and reuses used hollow molded bodies such as polyester bottles has attracted attention. In the case of polyester films, various proposals have been made to produce films using recycled polyester resins as raw materials.
[0004] However, polyester resins using widely used antimony compounds, titanium compounds or germanium compounds as polymerization catalysts generally have to be improved because they are degraded and coloring of the polyester resin and a decrease in molecular weight occurs when the used polyester resin is recovered and regenerated. In particular, when used as films, the stretching waste such as the ear parts generated during film production is often reused as a raw material resin, and a polyester having less coloring and molecular weight decrease due to heating and melting is required even for recycled polyester resins.
[0005] As a method for solving the above-mentioned problems, there is known a method of adding a hindered phenol compound in the production of a polyester resin using an antimony compound, a titanium compound or a germanium compound as a polymerization catalyst (see, for example, Patent Documents 1 and 2).
[0006] In the methods described in Patent Documents 1 and 2, the thermal oxidation stability is improved, but further improvement is required from the viewpoint of suppressing the deterioration of physical properties during recovery and recycling.
[0007] On the other hand, the present applicant has discovered a catalyst having excellent thermal stability. Specifically, the applicant has discovered a catalyst composed of an aluminum compound and a phosphorus compound having a hindered phenol structure as described in Patent Documents 3 and 4. However, research on recycling a used polyester resin, particularly a used polyester resin using at least one selected from antimony compounds, titanium compounds, or germanium compounds as a polymerization catalyst, and producing a film has not been conducted. Prior art literature Patent Literature
[0008] [Patent Document 1] International Publication No. 2013 / 154042 [Patent Document 2] International Publication No. 2013 / 154043 [Patent Document 3] International Publication No. 2007 / 032325 [Patent Document 4] Japanese Patent Application Publication No. 2006-169432 Summary of the invention [Problems to be solved by the invention]
[0009] The present invention is made to solve the problems of the related prior art, and its object is to provide a method for producing a polyester resin and a polyester film containing a recycled polyester resin, wherein even if a used polyester resin using at least one selected from antimony compounds, titanium compounds or germanium compounds as a polymerization catalyst is used, when the polyester film is produced, the strength reduction due to coloring and molecular weight reduction is small, and further, the deterioration when the film waste is reused is small.
Methods for solving the problem
[0010] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by adding a polyester resin containing an aluminum compound and a phosphorus compound to a recycled polyester resin containing at least one element selected from antimony, titanium and germanium, and melt-molding, a polyester film with excellent recyclability and little coloration and strength reduction can be produced.
[0011] That is, the present invention is constituted as follows. [Item 1] A method for producing a polyester film, characterized in that it comprises: a step of mixing a recovered polyester resin (A) with a polyester resin (B) containing an aluminum compound and a phosphorus compound, wherein the polyester resin (A) satisfies the following (1) to (3), (1) the polyester resin (A) contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin (A) is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin (A) is 0.5 to 0.8 dl / g.
[0012] [Item 2] The method for producing a polyester film according to item 1, wherein the polyester resin (B) satisfies the following (4) and (5): (4) the content of aluminum element in the polyester resin (B) is 5 to 50 ppm by mass, (5) The phosphorus content in the polyester resin (B) is 5 to 1000 ppm by mass.
[0013] [Item 3] The method for producing a polyester film according to item 1 or 2, comprising the step of melt-mixing the polyester resin (A) and the polyester resin (B) to obtain a polyester resin composition (C).
[0014] [Item 4] The method for producing a polyester film according to any one of Items 1 to 3, further comprising the step of mixing a polyester resin (D).
[0015] [Item 5] A method for producing a polyester film, characterized in that it comprises: a step of mixing a polyester resin composition (C) with a polyester resin (D), wherein the polyester resin composition (C) is a molten mixture of a recycled polyester resin (A) and a polyester resin (B) containing an aluminum compound and a phosphorus compound, The polyester resin (A) satisfies the following (1) to (3), (1) the polyester resin (A) contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin (A) is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin (A) is 0.5 to 0.8 dl / g.
[0016] [Item 6] The method for producing a polyester film according to any one of Items 1 to 5, wherein the intrinsic viscosity retention rate of the polyester resin composition (C) is 89% or more.
[0017] [Item 7] The method for producing a polyester film according to any one of Items 1 to 6, wherein the intrinsic viscosity retention rate of the polyester resin (A) is 92% or less.
[0018] [Item 8] The method for producing a polyester film according to any one of Claims 1 to 7, wherein the intrinsic viscosity retention rate of the polyester resin (B) is 93% or more.
[0019] [Item 9] The method for producing a polyester film according to any one of claims 1 to 8, wherein the intrinsic viscosity retention rate of the polyester resin (E) constituting the polyester film is 89% or more.
[0020] [Item 10] The method for producing a polyester film according to any one of items 1 to 9, wherein the polyester resin (A) is 5 to 95 parts by mass based on 100 parts by mass of the total of the polyester resin (A) and the polyester resin (B).
[0021] [Item 11] The method for producing a polyester film according to any one of items 1 to 10, wherein the polyester resin (D) is 5 to 95 parts by mass based on 100 parts by mass of the total of the polyester resin (A), the polyester resin (B), and the polyester resin (D).
[0022] [Item 12] The method for producing a polyester film according to any one of items 1 to 11, wherein the polyester film is a multilayer polyester film composed of at least two layers, and at least one surface thereof is a layer not containing the polyester resin (A).
[0023] [Item 13] The method for producing a polyester film according to any one of items 1 to 12, wherein the phosphorus compound has a phosphorus element and a phenol structure in the same molecule.
[0024] [Item 14] The method for producing a polyester film according to any one of Items 1 to 13, wherein the polyester resin (A) contains at least an antimony element and a germanium element.
[0025] [Item 15] The method for producing a polyester film according to any one of Items 1 to 14, wherein the polyester resin (A) contains at least isophthalic acid as a copolymerization component.
[0026] [Item 16] The method for producing a polyester film according to Item 4, wherein the polyester resin (D) contains a melt resistivity adjuster.
[0027] [Item 17] A polyester film, characterized in that it is a polyester film composed of a resin (E), wherein the resin (E) comprises a recycled polyester resin (A) and a polyester resin (B) containing an aluminum compound and a phosphorus compound, The polyester resin (A) satisfies the following (1) to (3), (1) the polyester resin (A) contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin (A) is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin (A) is 0.5 to 0.8 dl / g.
[0028] [Item 18] The polyester film according to item 17, characterized in that the polyester resin (B) satisfies the following (4) and (5), (4) the content of aluminum element in the polyester resin (B) is 5 to 50 ppm by mass, (5) The phosphorus content in the polyester resin (B) is 5 to 1000 ppm by mass.
[0029] [Item 19] The polyester film according to Item 17 or 18, wherein the polyester resin (E) further comprises a polyester resin (D).
[0030] [Item 20] The polyester film according to any one of Items 17 to 19, wherein the intrinsic viscosity retention rate of the polyester resin (E) is 89% or more.
[0031] [Item 21] A polyester film characterized in that the polyester resin constituting the film contains at least antimony element, germanium element and aluminum element.
[0032] [Item 22] The polyester film according to Item 21, wherein the polyester resin constituting the film contains isophthalic acid as a copolymerization component. [Effects of the Invention]
[0033] According to the present invention, even when recycled polyester is used as a raw material, a polyester film having little deterioration of the resin, little decrease in molecular weight, coloration, decrease in mechanical strength, etc. can be obtained. DETAILED DESCRIPTION
[0034] In the present invention, the polyester film is produced by mixing the recovered polyester resin (A) with the polyester resin (B) containing an aluminum compound and a phosphorus compound. The obtained polyester film has excellent characteristics such as little decrease in molecular weight, coloration and / or decrease in mechanical strength.
[0035] [Polyester resin (A)] The polyester resin (A) is a used polyester resin recovered in any form, and its shape is not limited, but is preferably a shape that is easily mixed with the polyester resin (B). Examples of the shape include chips, flakes, and powder. Any form of used polyester resin (A) refers to a resin that has been melted once in order to produce a polyester molded product, and examples thereof include containers such as PET bottles and trays collected from the streets, fibers and products, waste products before the product is taken out during manufacturing, products that have not been shipped to the market as Class B products, ears held during film stretching, end materials of slits, and molded products returned due to complaints, etc. These may be single substances from known sources, such as recycled PET bottles or ear parts of films, or mixtures from different sources.
[0036] The polyester resin (A) preferably contains 50 mol% or more of ethylene terephthalate structural units, more preferably 70 mol% or more, further preferably 80 mol% or more, and particularly preferably 90 mol% or more. As the polycarboxylic acid component other than terephthalic acid and the polyol component other than ethylene glycol, the components described in the polyester resin (B) described below can be used.
[0037] Polyester resin (A) is preferably polyethylene terephthalate resin in terms of quality control. In this case, in polyester resin (A), the copolymer component may contain isophthalic acid component, and when the total acid component is set to 100 mol%, the lower limit of the content of isophthalic acid component is preferably 0.02 mol%, more preferably 0.05 mol%, further preferably 0.1 mol%, particularly preferably 0.2 mol%, and most preferably 0.3 mol%. The upper limit is preferably 5.0 mol%, more preferably 4.0 mol%, further preferably 3.0 mol%, particularly preferably 2.5 mol%, and most preferably 2.0%.
[0038] Diethylene glycol is not only contained in the polyester resin as a by-product of ethylene glycol during polyester polymerization, but is also sometimes added during polymerization for the purpose of adjusting crystallization. When the total diol components are 100 mol%, the lower limit of the content of the diethylene glycol component in the polyester resin (A) is preferably 0.5 mol%, more preferably 0.8 mol%, further preferably 1.0 mol%, particularly preferably 1.2 mol%, and most preferably 1.4 mol%. The upper limit is preferably 5.0 mol%, more preferably 4.0 mol%, further preferably 3.5 mol%, and particularly preferably 3.0 mol%.
[0039] When the total acid components are 100 mol% and the total diol components are 100 mol%, the upper limit of the copolymer components other than isophthalic acid and diethylene glycol in the polyester resin (A) is preferably 3.0 mol%, more preferably 2.5 mol%, and even more preferably 2.0 mol%, respectively, in terms of the acid components and diol components.
[0040] When the total amount of the total acid components and the total diol components is 200 mol%, the total amount of the copolymer components of the polyester resin (A) is calculated as the total amount of the acid components and the diol components, and the lower limit is preferably 0.5 mol%, more preferably 1.0 mol%, further preferably 1.5 mol%, and particularly preferably 2.0 mol%. The upper limit is preferably 7.0 mol%, more preferably 6.0 mol%, further preferably 5.0 mol%, and particularly preferably 4 mol%. If the upper limit is greater than the above, the heat resistance and mechanical strength of the obtained polyester film may be reduced. In addition, in order to prevent this, the amount of the recycled polyester resin (A) added may be limited.
[0041] The polyester resin (A) contains at least one element selected from antimony, titanium and germanium, that is, the polyester resin (A) is preferably produced using at least one polymerization catalyst selected from antimony compounds, titanium compounds and germanium compounds in a catalytic amount.
[0042] The total content of antimony, titanium and germanium in the polyester resin (A) is 2 to 500 mass ppm, preferably 5 to 400 mass ppm, more preferably 10 to 300 mass ppm, and further preferably 50 to 250 mass ppm. If it is greater than 500 mass ppm, the intrinsic viscosity retention rate of the polyester resin composition (C) described below may become insufficient. It should be noted that in this specification, mass ppm means 10 -4 quality%.
[0043] The polyester resin (A) may contain a colorant, lubricant particles, an ultraviolet absorber, a melt resistivity adjuster, an antistatic agent, an antioxidant, a heat stabilizer and the like, which will be described later.
[0044] The intrinsic viscosity of the polyester resin (A) is preferably 0.5 to 0.8 dl / g, more preferably 0.55 to 0.75 dl / g, and even more preferably 0.57 to 0.73 dl / g. When the intrinsic viscosity of the polyester resin (A) is less than the above range, the mechanical strength and impact resistance of the polyester film produced using the polyester resin (A) may be insufficient. On the other hand, when the intrinsic viscosity of the polyester resin (A) is greater than the above range, when the polyester resin (A) and the polyester resin (B) are mixed and melted, local shear heat generation becomes large and the resin deteriorates, and it may be difficult to produce a film with increased stress during stretching. In addition, restrictions on the intrinsic viscosity and amount of the mixed polyester resin (B) may increase.
[0045] The intrinsic viscosity retention rate of the polyester resin (A) is preferably 92% or less, more preferably 91% or less, further preferably 90% or less, and particularly preferably 89% or less. When the intrinsic viscosity retention rate of the polyester resin (A) is greater than 92%, the effect of improving recyclability by blending the polyester resin (B) may not be sufficient. The method for determining the intrinsic viscosity retention rate is described below. The intrinsic viscosity retention rate of the polyester resin (A) is preferably 70% or more, more preferably 75% or more, and further preferably 80% or more. If it is less than 70%, even if the polyester resin (B) is added, the sufficient effect may not be obtained, and the amount of the polyester resin (A) used needs to be reduced to a lower level, and the significance of using recycled polyester becomes small.
[0046] When the polyester resin (A) is a PET bottle collected from the street, the amount of CT (cyclic trimer) contained in the polyester resin (A) is preferably 9000 mass ppm or less, more preferably 8000 mass ppm or less, further preferably 7500 mass ppm or less. It is particularly preferably 7000 mass ppm or less. The CT content is preferably 4000 mass ppm or more, more preferably 4500 mass ppm or more, further preferably 5000 mass ppm or more.
[0047] The polyester resin (A) is preferably a polyester resin produced using only a polymerization catalyst selected from at least one of an antimony compound, a titanium compound, and a germanium compound, but may also include a polyester resin produced using a polymerization catalyst composed of an aluminum compound and a phosphorus compound. The polyester resin produced using a polymerization catalyst selected from at least one of an antimony compound, a titanium compound, and a germanium compound in the polyester resin (A) is preferably greater than 50% by mass, preferably 70% by mass or more, and more preferably 80% by mass or more.
[0048] The polyester resin (A) may be a product obtained by melting and pelletizing a recovered molded product, but is preferably a product that is not melted but is pulverized. From the perspective of operability, the pulverized product preferably has a shape in which the distance between the two longest points is preferably 3 to 30 mm, more preferably 5 to 20 mm. It should be noted that this value is an average value obtained by taking 100 g of the pulverized product and selecting 20 large pulverized products and measuring the resultant.
[0049] [Polyester resin (B)] The polyester resin (B) contains an aluminum compound and a phosphorus compound. That is, the polyester resin (B) is preferably produced using a catalytic amount of a polymerization catalyst composed of an aluminum compound and a phosphorus compound.
[0050] The polyester resin (B) is preferably a polymer formed from at least one selected from polycarboxylic acids and ester-forming derivatives thereof and at least one selected from polyhydric alcohols and ester-forming derivatives thereof.
[0051] <Polycarboxylic acid component> The main polycarboxylic acid component constituting the polyester resin (B) is preferably a dicarboxylic acid. "The main polycarboxylic acid component is a dicarboxylic acid" means that, relative to the total polycarboxylic acid component, it contains more than 50 mol% of dicarboxylic acid, preferably contains 70 mol% or more of dicarboxylic acid, more preferably contains 80 mol% or more of dicarboxylic acid, and further preferably contains 90 mol% or more of dicarboxylic acid. It should be noted that when two or more dicarboxylic acids are used, their total is preferably within the above range.
[0052] Examples of the dicarboxylic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, dodecanedicarboxylic acid, tetradecanedicarboxylic acid, hexadecanedicarboxylic acid, 1,3-cyclobutanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2,5-norbornanedicarboxylic acid, dimer acid, and the like, or ester-forming derivatives thereof; fumaric acid, maleic acid, itaconic acid, unsaturated aliphatic dicarboxylic acids or their ester-forming derivatives as exemplified by the following: phthalic acid, isophthalic acid, terephthalic acid, 5-(alkali metal)sulfoisophthalic acid, biphenyl dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, 4,4'-diphenyl sulfone dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, pamoic acid, anthracene dicarboxylic acid, and aromatic dicarboxylic acids or their ester-forming derivatives as exemplified by the following:
[0053] More preferably, the main polycarboxylic acid component is terephthalic acid or its ester-forming derivative, or naphthalene dicarboxylic acid or its ester-forming derivative. Examples of naphthalene dicarboxylic acid or its ester-forming derivative include 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, or their ester-forming derivatives.
[0054] “The main polycarboxylic acid component is terephthalic acid or its ester-forming derivative, or naphthalene dicarboxylic acid or its ester-forming derivative” means that the total amount of terephthalic acid or its ester-forming derivative and naphthalene dicarboxylic acid or its ester-forming derivative is more than 50 mol%, preferably 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more, relative to the total polycarboxylic acid components.
[0055] As the dicarboxylic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid or ester-forming derivatives thereof are particularly preferred. Other dicarboxylic acids may be used as constituent components as necessary.
[0056] As polycarboxylic acids other than these dicarboxylic acids, if in small amounts, polycarboxylic acids of more than 3 valences and carboxylic acids can be used in combination, preferably polycarboxylic acids of 3 to 4 valences. As polycarboxylic acids, for example, ethanetricarboxylic acid, propanetricarboxylic acid, butanetetracarboxylic acid, pyromellitic acid, trimellitic acid, trimesic acid, 3,4,3',4'-biphenyltetracarboxylic acid and their ester-forming derivatives can be cited. With respect to the total polycarboxylic acid component, polycarboxylic acids of more than 3 valences are preferably less than 20 mol%, more preferably less than 10 mol%, and further preferably less than 5 mol%. It should be noted that when using more than 2 kinds of polycarboxylic acids of more than 3 valences, their total is preferably within the above range.
[0057] As carboxylic acid, lactic acid, citric acid, malic acid, tartaric acid, glycolic acid, 3-hydroxybutyric acid, p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, 4-hydroxycyclohexanecarboxylic acid or their ester forming derivatives etc. can be mentioned. Relative to the total polycarboxylic acid component, hydroxycarboxylic acid is preferably 20 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less. It should be noted that, when using two or more hydroxycarboxylic acids, their total is preferably within the above range.
[0058] Examples of the ester-forming derivatives of polycarboxylic acids or hydroxycarboxylic acids include alkyl esters, acid chlorides, and acid anhydrides thereof.
[0059] <Polyol component> The main polyol component constituting the polyester resin (B) is preferably a diol. "The main polyol component is a diol" means that the diol is contained in an amount of more than 50 mol%, preferably 70 mol% or more, more preferably 80 mol% or more, and further preferably 90 mol% or more relative to the total polyol component. It should be noted that when two or more diols are used, their total amount is preferably within the above range.
[0060] Examples of the diol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, diethylene glycol, triethylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 1,10-decanediol, and 1,12-dodecane. Alkylene glycols exemplified by diols such as polyethylene glycol, polytrimethylene ether glycol, polytetramethylene glycol, etc.; aliphatic diols exemplified by hydroquinone, 4,4'-dihydroxybisphenol, 1,4-di(β-hydroxyethoxy)benzene, 1,4-di(β-hydroxyethoxyphenyl)sulfone, di(p-hydroxyphenyl)ether, di(p-hydroxyphenyl)sulfone, di(p-hydroxyphenyl)methane, 1,2-di(p-hydroxyphenyl)ethane, bisphenol A, bisphenol C, 2,5-naphthalene diol, and diols obtained by adding ethylene oxide to these diols.
[0061] Among these diols, alkylene glycol is preferred, and ethylene glycol, 1,3-propylene glycol, 1,4-butanediol or 1,4-cyclohexanedimethanol is more preferred. The alkylene glycol may contain a substituent or an alicyclic structure in the molecular chain, and two or more thereof may be used simultaneously.
[0062] As polyols other than these diols, trivalent or higher polyols may be used in combination if the amount is small, and trivalent to tetravalent polyols are preferred. Examples of trivalent or higher polyols include trimethylolmethane, trimethylolethane, trimethylolpropane, pentaerythritol, glycerol, and hexanetriol.
[0063] The trivalent or higher polyol content is preferably 20 mol% or less, more preferably 10 mol% or less, and even more preferably 5 mol% or less relative to the total polyol component. When two or more trivalent or higher polyols are used, their total content is preferably within the above range.
[0064] In addition, the combined use of cyclic esters is also permitted. Examples of cyclic esters include ε-caprolactone, β-propiolactone, β-methyl-β-propiolactone, δ-valerolactone, glycolide, lactide, and the like. In addition, examples of ester-forming derivatives of polyols include esters of polyols with lower aliphatic carboxylic acids such as acetic acid.
[0065] The cyclic ester is preferably 20 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less relative to the total of the total polycarboxylic acid component and the total polyol component. It should be noted that when two or more cyclic esters are used, their total is preferably within the above range.
[0066] The composition of the polyester resin (B) can be determined based on the composition of the film to be manufactured by considering the composition of the polyester resin (A). For example, when the polyester resin (A) is mainly recycled beverage bottles, since the main constituent unit of the polyester resin (A) is ethylene terephthalate, if a polyethylene terephthalate film is manufactured, the polyester resin (B) is also polyethylene terephthalate. In this case, the polyester resin (B) preferably contains 90 mol% or more of a component derived from ethylene terephthalate monomer, more preferably 95 mol% or more, and even more preferably 97 mol% or more.
[0067] On the other hand, when the film to be produced is a copolymer composition film such as a heat shrinkable film or a film for molding, the polyester resin (B) is preferably a polyester resin other than copolyester or polyethylene terephthalate. For example, ethylene terephthalate / ethylene isophthalate copolymers, ethylene terephthalate / butylene terephthalate copolymers, ethylene terephthalate / 2,2-dimethyltrimethylene terephthalate copolymers (those obtained by adding neopentyl glycol to the diol component), ethylene 2,2'-ethylene oxide (those obtained by adding diethylene glycol to the diol component), ethylene terephthalate / 1,4-cyclohexanedimethanol terephthalate copolymers (those obtained by adding 1,4-cyclohexanedimethanol to the diol component), polyethylene isophthalate, polybutylene terephthalate, poly2,2-dimethyltrimethylene terephthalate, 2,2'-oxydiethylene terephthalate, 1,4-cyclohexanedimethanol terephthalate, and the like, and products obtained by copolymerizing other components therewith.
[0068] The polyester resin (B) is preferably a polymer composed of only one monomer selected from ethylene terephthalate, butylene terephthalate, trimethylene terephthalate, 1,4-cyclohexanedimethylene terephthalate, ethylene naphthalate, butylene naphthalate or trimethylene naphthalate, or a copolymer composed of two or more of the above monomers. The polyester resin (B) is more preferably a copolymer composed of polyethylene terephthalate or at least one of the above monomers other than ethylene terephthalate and ethylene terephthalate, and particularly preferably polyethylene terephthalate.
[0069] <Polymerization Catalyst> As described above, it is preferred to produce the polyester resin (B) using a polymerization catalyst composed of an aluminum compound and a phosphorus compound.
[0070] (Aluminum compounds) The aluminum compound constituting the polymerization catalyst of the polyester resin (B) is not particularly limited as long as it is soluble in a solvent, and a known aluminum compound can be used without limitation. Examples of the aluminum compound include: carboxylates such as aluminum formate, aluminum acetate, basic aluminum acetate, aluminum acrylate, aluminum oxalate, aluminum acrylate, aluminum laurate, aluminum stearate, aluminum benzoate, aluminum trichloroacetate, aluminum lactate, aluminum citrate, aluminum tartrate, and aluminum salicylate; inorganic acid salts such as aluminum chloride, aluminum hydroxide, basic aluminum chloride, aluminum nitrate, aluminum sulfate, aluminum carbonate, aluminum phosphate, and aluminum phosphonate; aluminum alkoxides such as aluminum methoxide, aluminum ethoxide, aluminum n-propoxide, aluminum isopropoxide, aluminum n-butoxide, and aluminum tert-butoxide; chelates such as aluminum acetylacetonate, aluminum ethylacetoacetate, and aluminum (ethylacetoacetoxy) diisopropoxide; organic aluminum compounds such as trimethylaluminum and triethylaluminum, partial hydrolyzates thereof, reaction products of aluminum alkoxides, aluminum chelates, and hydroxycarboxylic acids, aluminum oxide, ultrafine aluminum oxide, aluminum silicate, and composite oxides of aluminum with titanium, silicon, zirconium, alkali metals, alkaline earth metals, and the like. Among these, at least one selected from carboxylates, inorganic acid salts and chelates is preferred, among which at least one selected from aluminum acetate, basic aluminum acetate, aluminum chloride, aluminum hydroxide, basic aluminum chloride and aluminum acetylacetonate is more preferred, further preferred is at least one selected from aluminum acetate, basic aluminum acetate, aluminum chloride, aluminum hydroxide, basic aluminum chloride and aluminum acetylacetonate, particularly preferred is at least one selected from aluminum acetate and basic aluminum acetate, and most preferred is basic aluminum acetate.
[0071] The aluminum compound is preferably an aluminum compound soluble in solvents such as water and glycol. The solvent that can be used in the manufacture of the polyester resin (B) refers to water and alkylene glycols. Based on the alkylene glycols, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, trimethylene glycol, di(trimethylene glycol), tetramethylene glycol, di(tetramethylene glycol), neopentyl glycol, etc. are mentioned. Preferably, it is at least one selected from water, ethylene glycol, trimethylene glycol and tetramethylene glycol, and more preferably water or ethylene glycol.
[0072] The content of aluminum in the polyester resin (B) is preferably 5 to 50 mass ppm, more preferably 7 to 40 mass ppm, further preferably 10 to 30 mass ppm, and particularly preferably 15 to 25 mass ppm. When the aluminum content is less than 5 mass ppm, the polymerization activity may not be fully exerted. On the other hand, when it exceeds 50 mass ppm, the amount of aluminum-based foreign matter may increase.
[0073] In addition, when cost is important, the content of aluminum in the polyester resin (B) is preferably 9 to 20 mass ppm, more preferably 9 to 19 mass ppm, further preferably 10 to 17 mass ppm, and particularly preferably 12 to 17 mass ppm. When the aluminum content is less than 9 mass ppm, the polymerization activity may not be fully exerted. On the other hand, when it is greater than 20 mass ppm, the amount of aluminum-based foreign matter may increase due to the relationship with the content of phosphorus described later, and the cost of the catalyst increases.
[0074] (Phosphorus compounds) The phosphorus compound used as the polymerization catalyst for the polyester resin (B) is not particularly limited, but phosphonic acid compounds and phosphinic acid compounds are preferred because the catalytic activity is enhanced to a greater extent when used. Among them, phosphonic acid compounds are more preferred because the catalytic activity is enhanced to a particularly great extent when used.
[0075] Among the above-mentioned phosphorus compounds, phosphorus compounds having a phosphorus element and a phenol structure in the same molecule are preferred. As long as the phosphorus compound has a phosphorus element and a phenol structure in the same molecule, there is no particular limitation, but when one or more compounds selected from the group consisting of phosphonic acid compounds having a phosphorus element and a phenol structure in the same molecule and phosphinic acid compounds having a phosphorus element and a phenol structure in the same molecule are used, the catalytic activity is improved greatly, so it is preferred; when one or more phosphonic acid compounds having a phosphorus element and a phenol structure in the same molecule are used, the catalytic activity is improved greatly, so it is more preferred.
[0076] In addition, examples of phosphorus compounds having a phosphorus element and a phenol structure in the same molecule include P(=O)R 1 (OR 2 )(OR 3 ) or P(=O)R 1 R 4 (OR 2 ) represented by the compound, etc. 1 R represents a hydrocarbon group having 1 to 50 carbon atoms containing a phenolic moiety, or a hydrocarbon group having 1 to 50 carbon atoms containing a substituent such as a hydroxyl group, a halogen group, an alkoxy group, or an amino group and a phenolic structure. 4 R represents a hydrogen atom, a hydrocarbon group having 1 to 50 carbon atoms, or a hydrocarbon group having 1 to 50 carbon atoms and having a substituent such as a hydroxyl group, a halogen group, an alkoxy group, or an amino group. 2 , R 3 Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 50 carbon atoms, or a hydrocarbon group having 1 to 50 carbon atoms and containing a substituent such as a hydroxyl group or an alkoxy group. The hydrocarbon group may contain a branched structure, an alicyclic structure such as a cyclohexyl group, or an aromatic ring structure such as a phenyl group or a naphthyl group. 2 and R 4The ends of the may be bonded to each other.
[0077] Examples of the phosphorus compound having a phosphorus element and a phenol structure in the same molecule include p-hydroxyphenylphosphonic acid, dimethyl p-hydroxyphenylphosphonate, diethyl p-hydroxyphenylphosphonate, diphenyl p-hydroxyphenylphosphonate, bis(p-hydroxyphenyl)phosphinic acid, methyl bis(p-hydroxyphenyl)phosphinic acid, phenyl bis(p-hydroxyphenyl)phosphinic acid, p-hydroxyphenylphosphinic acid, methyl p-hydroxyphenylphosphinic acid, and phenyl p-hydroxyphenylphosphinic acid.
[0078] As the phosphorus compound having a phosphorus element and a phenol structure in the same molecule, in addition to the above examples, there can be mentioned a phosphorus compound having a phosphorus element and a hindered phenol structure (a phenol structure in which an alkyl group having a tertiary carbon (preferably an alkyl group having a tertiary carbon such as a tert-butyl group, 2,3-dimethyl-2-butyl group, a neopentyl group, etc.) is bonded to one or two ortho positions of a hydroxyl group in the same molecule, etc.), preferably a phosphorus compound having a phosphorus element and a structure of the following (chemical formula A) in the same molecule, and more preferably 3,5-di-tert-butyl-4-hydroxybenzyl dialkyl phosphonate as shown in the following (chemical formula B). It should be noted that as the phosphorus compound used for producing the polyester resin (B), 3,5-di-tert-butyl-4-hydroxybenzyl dialkyl phosphonate as shown in the following (chemical formula B) is preferred, but in addition, a modified form of 3,5-di-tert-butyl-4-hydroxybenzyl dialkyl phosphonate may be contained. The details of the modified form are as follows.
[0079]
Chemical formula 1
[0080] (In (chemical formula A), * represents an atomic bond.)
[0081]
Chemical formula 2
[0082] ((Chemical Formula B) where X 1 , X 2 They are hydrogen and an alkyl group having 1 to 4 carbon atoms.)
[0083] In this specification, a polyester resin in which at least one hindered phenol structure can be detected by a P-NMR measurement method when the solution is dissolved in a hexafluoroisopropanol-based solvent is referred to as "having a hindered phenol structure". That is, the polyester resin (B) is preferably a polyester resin produced using a phosphorus compound having a phosphorus element and a hindered phenol structure in the same molecule as a polymerization catalyst. The method for detecting the hindered phenol structure in the polyester resin (B) (P-NMR measurement method) will be described later.
[0084] In the above (chemical formula B), X 1 , X 2All of them are preferably alkyl groups having 1 to 4 carbon atoms, and more preferably alkyl groups having 1 to 2 carbon atoms. In particular, an ethyl ester having 2 carbon atoms is preferably Irganox 1222 (manufactured by BASF) because it is commercially available and easily available.
[0085] The phosphorus compound is preferably used by heat treatment in a solvent. It should be noted that the details of the heat treatment are described later. As the phosphorus compound, when 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid dialkyl ester as a phosphorus compound shown in the above (chemical formula B) is used, in the above heat treatment, the partial structure of 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid dialkyl ester as a phosphorus compound shown in (chemical formula B) changes. For example, the detachment of the tert-butyl group, the hydrolysis of the ethyl ester group and the hydroxyethyl ester exchange structure (ester exchange structure with ethylene glycol) and other changes occur. Therefore, in the present invention, as a phosphorus compound, a phosphorus compound whose structure changes other than 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid dialkyl ester shown in (chemical formula B) is also included. It should be noted that the detachment of the tert-butyl group occurs significantly at high temperatures in the polymerization process.
[0086] Hereinafter, when 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl ester is used as the phosphorus compound, 9 phosphorus compounds in which a part of 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid diethyl ester undergoes structural changes are shown below. The component amounts of various phosphorus compounds undergoing structural changes in the diol solution can be quantified by the P-NMR measurement method.
[0087]
Chemistry 3
[0088] Therefore, the phosphorus compound in the present invention may contain, in addition to 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid dialkyl ester, modified forms of 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid dialkyl ester as shown in the nine chemical formulas above.
[0089] When Irganox 1222 is used as the phosphorus compound, the polyester resin contains 9 types of phosphorus compound residues as shown in Table 1 below. When at least one of the 9 types of hindered phenol structures shown in Table 1 is detected by the P-NMR measurement method, the polyester resin (B) can be said to be a polyester resin produced using a phosphorus compound having a phosphorus element and a hindered phenol structure in the same molecule as a polymerization catalyst. By using a phosphorus compound having a hindered phenol structure, it is possible to exert sufficient polymerization activity while suppressing an increase in catalyst cost.
[0090]
Table 1
[0091] In the present invention, it is preferred that at least one of the above Chemical Formulas 1, 4 and 7 is contained.
[0092] The phosphorus content in the polyester resin (B) is preferably 5 to 1000 mass ppm, more preferably 10 to 500 mass ppm, further preferably 15 to 200 mass ppm, particularly preferably 20 to 100 mass ppm, and most preferably 30 to 50 mass ppm. When the phosphorus content is less than 5 mass ppm, there is a possibility that the polymerization activity decreases and the amount of aluminum-based foreign matter increases. On the other hand, if it is greater than 1000 mass ppm, there is a concern that the polymerization activity decreases and there is a concern that the amount of phosphorus compound added increases, thereby increasing the catalyst cost.
[0093] In the case of focusing on cost, the phosphorus content in the polyester resin (B) is preferably 13 to 31 mass ppm, more preferably 15 to 29 mass ppm, and further preferably 16 to 28 mass ppm. When the phosphorus content is less than 13 mass ppm, there is a possibility that the polymerization activity decreases and the amount of aluminum-based foreign matter increases. On the other hand, if it is greater than 31 mass ppm, there is a concern that the polymerization activity decreases and there is a concern that the amount of phosphorus compound added increases, thereby increasing the catalyst cost.
[0094] In the polyester resin (B), the molar ratio of phosphorus to aluminum (hereinafter referred to as "residual molar ratio of phosphorus to aluminum" to distinguish it from the "added molar ratio of phosphorus to aluminum" described later) is preferably 1.00 to 5.00, more preferably 1.10 to 4.00, further preferably 1.20 to 3.50, and particularly preferably 1.25 to 3.00. As described above, the aluminum and phosphorus in the polyester resin (B) are derived from the aluminum compound and phosphorus compound used as the polymerization catalyst of the polyester resin (B), respectively. By using these aluminum compounds and phosphorus compounds in combination at a specific ratio, a complex having catalytic activity can be functionally formed in the polymerization system, and sufficient polymerization activity can be exerted. In addition, although the catalyst cost of the resin produced using the polymerization catalyst composed of the aluminum compound and the phosphorus compound becomes higher (the production cost is high) compared with the polyester resin produced using the catalyst such as the antimony catalyst, by using the aluminum compound and the phosphorus compound in combination at a specific ratio, it is possible to suppress the increase in catalyst cost while exerting sufficient polymerization activity. When the residual molar ratio of phosphorus to aluminum is less than 1.00, there is a concern that thermal stability and thermal oxidation stability may decrease, and the amount of aluminum-based foreign matter may increase. On the other hand, when the residual molar ratio of phosphorus to aluminum is greater than 5.00, there is a concern that the catalyst cost may increase because the amount of phosphorus compound added becomes too much. When cost is given priority, the residual molar ratio of phosphorus element to aluminum element is preferably 1.32 to 1.80, more preferably 1.38 to 1.68.
[0095] As the polymerization catalyst used in the manufacture of the polyester resin (B), in addition to the above-mentioned aluminum compounds and phosphorus compounds, other polymerization catalysts such as antimony compounds, germanium compounds, and titanium compounds may also be used in combination within the range that the characteristics, processability, color tone, and other products of the polyester resin (B) will not cause problems. The content of antimony element in the polyester resin (B) is preferably less than 30 mass ppm, the content of germanium element in the polyester resin (B) is preferably less than 10 mass ppm, and the content of titanium element in the polyester resin (B) is preferably less than 3 mass ppm. However, it is preferred not to use the above-mentioned other condensation catalysts as much as possible. It should be noted that trace mixing of other polymerization catalysts due to residual resin in the polyester resin (B) manufacturing device is not excluded.
[0096] The content of aluminum elements corresponding to aluminum-based foreign matters in the polyester resin (B) is preferably 3000 mass ppm or less, more preferably 2800 mass ppm or less, further preferably 2000 mass ppm or less, and further preferably 1500 mass ppm or less. Aluminum-based foreign matters refer to foreign matters caused by aluminum compounds used as polymerization catalysts, which are foreign matters insoluble in the polyester resin (B). When the content of aluminum-based foreign matters exceeds the above value, it becomes a cause of insoluble tiny foreign matters contained in the polyester resin (B), and there is a concern that the quality of the molded body will deteriorate. In addition, it is also related to the problem of increased filter clogging during polyester filtration in the polycondensation process and the molding process. The preferred lower limit of the content of aluminum elements corresponding to aluminum-based foreign matters is preferably 0 mass ppm, and due to technical difficulties, it is preferably around 300 mass ppm. It should be noted that in this specification, the aluminum element amount measured by the measuring method described later in the examples is an indicator for relatively evaluating the aluminum foreign matter amount based on the aluminum element amount, and does not represent the absolute value of the aluminum foreign matter amount contained in the polyester resin.
[0097] The intrinsic viscosity of the polyester resin (B) is preferably 0.50 to 0.90 dl / g, more preferably 0.55 to 0.80 dl / g, and further preferably 0.58 to 0.75 dl / g. When the intrinsic viscosity of the polyester resin (B) is less than the above, there is a concern that a large amount of fine powder (fine) will be generated due to friction between the polyester resin particles and friction between the polyester resin particles and the air transport duct when the polyester resin (B) is transported by air. When the intrinsic viscosity of the polyester resin (B) is greater than the above, there is a possibility that the local shear heat generation during melt mixing of the polyester resin (B) and the recovered polyester resin (A) becomes large, the resin deteriorates, and the stress during stretching becomes high, making the production of the film difficult. The intrinsic viscosity of the polyester resin (B) can be adjusted in accordance with the intrinsic viscosity of the polyester resin (A) so that the intrinsic viscosity of the polyester constituting the film is within an appropriate range. It should be noted that, since there is a concern that economic efficiency may be reduced when a polyester resin (B) having an intrinsic viscosity greater than 0.62 dl / g is produced only by melt polymerization, when a polyester resin (B) greater than 0.62 dl / g is required, it is preferred to polymerize the polyester resin (B) obtained by melt polymerization by a solid phase polymerization method.
[0098] In the solid phase polymerization, the CT content in the polyester resin (B) is preferably 7000 mass ppm or less, more preferably 6000 mass ppm or less, and further preferably 5500 mass ppm or less. In practice, the CT content is preferably 2500 mass ppm or more, and more preferably 3000 mass ppm or more.
[0099] The intrinsic viscosity retention rate of the polyester resin (B) is preferably 93% or more, more preferably 94% or more, and further preferably 95% or more. When the intrinsic viscosity retention rate of the polyester resin (B) is less than 93%, the intrinsic viscosity retention rate of the polyester resin composition (C) becomes low, and there is a concern that the recyclability becomes insufficient. Although the upper limit of the intrinsic viscosity retention rate of the polyester resin (B) is preferably 100%, it is about 99% due to technical difficulties.
[0100] In addition, the manufacturing method of polyester resin (B) is as mentioned later. The longest distance between two points of the polyester resin (B) is 2 to 10 mm, more preferably 3 to 6 mm in the pellets. Examples of the shape of the pellets include spherical, elliptical, barrel-shaped, and cubic shapes.
[0101] The polyester resin (B) may be a resin pelletized after polymerization, or may be a product recovered during the process of molding an article using the polyester resin (B). Examples of the products recovered during the process include products that were not shipped to the market as B-grade products, ears held during film stretching, end materials of slits, and molded articles returned due to complaints, etc. In the case of these products recovered during the process, they are preferably crushed products similar to the polyester resin (A).
[0102] The polyester resin (B) can also be used as a masterbatch (concentrated resin) of additives such as the polyester resin (D) described later.
[0103] [Polyester resin composition (C)] In the present invention, a polyester resin (A) and a polyester resin (B) are mixed to produce a film. A mixture of the polyester resin (A) and the polyester resin (B) is referred to as a polyester resin composition (C). In the production of the film, the polyester resin (A) and the polyester resin (B) can be fed into an extruder through their respective feed ports, or both can be fed into the same feed port, or both can be dry-mixed in advance. From the viewpoint of operability, it is preferred to melt-mix the polyester resin (A) and the polyester resin (B) as the polyester resin composition (C), and use it in the production of the film. It is preferred that the polyester resin (A) and the polyester resin (B) are mixed in a mass ratio of 5:95 to 95:5 to produce the polyester resin composition (C). That is, in the polyester resin composition (C), the polyester resin (A) is preferably 5 to 95 parts by mass relative to a total of 100 parts by mass of the polyester resin (A) and the polyester resin (B). By being within the above range, the coloration of the polyester resin composition (C) and the decrease in molecular weight can be suppressed. It should be noted that the suppression of coloration in this specification means that even if the number of reuses is increased (repeated re-mixing), the decrease in the L value described later and the increase in the b value described later can be suppressed. When the blending ratio of the polyester resin (A) is greater than 95 parts by mass, the intrinsic viscosity retention rate of the polyester resin composition (C) decreases, and the recyclability may become insufficient. On the other hand, when the blending ratio of the polyester resin (A) is less than 5 parts by mass, there is a concern that the economic efficiency is reduced due to the saturation of the coloration suppression effect. It should be noted that since the polyester resin (B) is produced using a polymerization catalyst composed of an aluminum compound and a phosphorus compound, even if the residual molar ratio of phosphorus element to aluminum element is within the above-mentioned specified range, the cost of the catalyst becomes higher (the manufacturing cost becomes higher) compared with the polyester resin produced using a catalyst such as an antimony catalyst. By using the polyester resin (A) and the polyester resin (B) together, it is possible to suppress the manufacturing cost while improving the recyclability. If the blending ratio of the polyester resin (A) is increased, although the manufacturing cost of the polyester resin composition (C) can be reduced, if the number of reuses is increased, the color tone is likely to deteriorate. On the other hand, if the blending ratio of the polyester resin (B) is increased, even if the number of reuses of the polyester resin composition (C) is increased, the deterioration of the color tone can be suppressed, but there is a concern that the manufacturing cost will increase. The mass ratio of the polyester resin (A) to the polyester resin (B) is more preferably 20:80 to 80:20, and more preferably 25:75 to 75:25.
[0104] The polyester resin (A) and the polyester resin (B) can be dry-mixed to produce the polyester resin composition (C). Alternatively, the polyester resin (A) and the polyester resin (B) can be kneaded using a melt extrusion method to produce the polyester resin composition (C). In this case, after the polyester resin (A) and the polyester resin (B) are dry-mixed, they can be melted / kneaded using a general resin mixing device such as a Banbury mixer, a kneader, a single-screw extruder, a twin-screw extruder, a four-screw extruder, a single-screw planetary extruder, etc. to produce the polyester resin composition (C). Among them, preferred are extruders with excellent surface renewal such as twin-screw extruders, quad-screw extruders, and single-screw planetary extruders. In addition, a preferred embodiment is that the extruder has at least one, preferably two, and more preferably three vent ports, and the vent port is connected to a decompression system to suppress the degradation of the polyester resin composition (C). Alternatively, after the polymerization of the polyester resin (B) is completed, the polyester resin (A) may be added to the molten polyester resin (B) before being cooled and pelletized, and kneaded to obtain the polyester resin composition (C).
[0105] The polyester resin composition (C) may be formed into a film in a molten state, but is preferably formed into pellets. The shape of the pellets is the same as that of the polyester resin (B).
[0106] The intrinsic viscosity of the polyester resin composition (C) is preferably 0.50 to 0.90 dl / g, more preferably 0.55 to 0.80 dl / g, and more preferably 0.58 to 0.75 dl / g. When the intrinsic viscosity of the polyester resin composition (C) is less than the above, there is a concern that the mechanical strength and impact resistance of the manufactured polyester film become insufficient. When the intrinsic viscosity of the polyester resin composition (C) is greater than the above, there is a concern that the economic efficiency decreases, the local shear heat generation during melting in an extruder increases, the resin deteriorates, and the stress during stretching increases, making the film production difficult.
[0107] The intrinsic viscosity retention rate of the polyester resin composition (C) is preferably 89% or more, more preferably 90% or more, further preferably 92% or more, particularly preferably 93% or more, and most preferably 94% or more. When the intrinsic viscosity retention rate of the polyester resin composition (C) is less than 89%, the recyclability may become insufficient. The upper limit of the intrinsic viscosity retention rate of the polyester resin composition (C) is preferably 100%, but due to technical difficulties, it is about 99%. In addition, it is preferred that the intrinsic viscosity retention rate of the polyester resin composition (C) is higher than the intrinsic viscosity retention rate of the polyester resin (A). It should be noted that when it is only recorded as "intrinsic viscosity retention rate" in this specification, it refers to the intrinsic viscosity retention rate of the re-mixed product when it is re-mixed only once.
[0108] It is also a preferred embodiment that the CT content in the re-mixed product of the first re-mixing of the polyester resin composition (C) is 6600 mass ppm or less. It is more preferably 6400 mass ppm or less, and further preferably 6000 mass ppm or less. The lower limit is not limited, but due to technical difficulties, it is about 2500 mass ppm, preferably 3000 mass ppm or more. If the CT content is greater than 6600 mass ppm, it may increase the amount of CT precipitation on the film surface, increase the haze, etc., which may become undesirable in terms of use, and the film-making equipment may be contaminated by CT, requiring an increase in the number of cleaning times. In order to make the CT content of the polyester resin composition (C) less than the above, methods such as using a polyester resin (A) with a small CT content, reducing the CT content of the polyester resin (B), and reducing the CT content of the polyester resin composition (C) can be adopted. As a method for reducing the CT content of the polyester resin (B) and the polyester resin composition (C), solid phase polymerization, heating treatment at 190 to 220° C. in a closed container or under an airflow containing ethylene glycol, etc.
[0109] The value (ΔCT) of the CT amount of the remixed product of the polyester resin composition (C) after the 3rd remixing minus the CT amount of the remixed product of the polyester resin composition (C) after the first remixing is preferably 900 mass ppm or less. It is more preferably 700 mass ppm or less, and further preferably 600 mass ppm or less. The lower limit is 0 mass ppm, but it is about 200 mass ppm due to technical difficulties. When ΔCT is greater than 900 mass ppm, as described above, there is a case where the amount of CT precipitation on the film surface increases.
[0110] In addition, the polyester resin composition (C) contains the polyester resin (B) produced using the above-mentioned Irganox 1222 as the phosphorus compound, and when the polyester resin composition (C) is subjected to the P-NMR measurement method, at least one of the nine hindered phenol structures shown in Table 1 can be detected. The same applies to the case where a phosphorus compound other than Irganox 1222 having a phosphorus element and a hindered phenol structure in the same molecule is used as a polymerization catalyst.
[0111] [Polyester resin (D)] One preferred mode when producing a film according to the present invention is to further add a polyester resin (D) to produce a polyester film. The polyester resin (D) may have various compositions depending on the film to be produced. For example, when producing a polyethylene terephthalate film, the total amount of copolymer components other than the terephthalic acid component and the ethylene glycol component in the polyester resin (D) is preferably 10 mol % or less, more preferably 7 mol % or less, and particularly preferably 5 mol % or less. For example, when a polyester-based heat shrinkable film is produced, the polyester resin (A) and the polyester resin (B) preferably contain a component other than copolyester or polyethylene terephthalate, depending on how the polyester resin (A) and the polyester resin (B) form the composition of the final heat shrinkable film. For example, when producing a polyester film containing voids, a polyester obtained by copolymerization of polyethylene glycol and polytetramethylene glycol or the like may be used. The carboxylic acid component and the diol component used for the polyester resin (D) are the same as those exemplified for the polyester resin (B).
[0112] The intrinsic viscosity of the polyester resin (D) varies in an appropriate range depending on the film to be produced, but is preferably 0.50 to 0.90 dl / g, more preferably 0.55 to 0.80 dl / g, and even more preferably 0.58 to 0.75 dl / g. The catalyst used for the polyester resin (D) is the same as those exemplified for the production of the polyester resin (A). The viscosity retention rate of the polyester resin (D) is preferably as high as possible, but the intrinsic viscosity retention rate may be 92% or less, 91% or less, 90% or less, and particularly 89% or less. The viscosity retention rate of the polyester resin (D) can be increased by reducing the amount of the catalyst, deactivating the catalyst, adding an anti-degradation agent such as a heat stabilizer, and the like. The lower limit of the viscosity retention rate of the polyester resin (D) is the same as that of the polyester resin (A).
[0113] In the manufacture of the film, colorants, lubricant particles, ultraviolet absorbers, melt resistivity regulators, antistatic agents, antioxidants, thermal stabilizers, etc. are often added, and the polyester resin (D) can also be a masterbatch (concentrated resin) of these additives. As lubricant particles, non-polar particles such as silicon dioxide, calcium carbonate, talc, kaolin, and organic particles such as cross-linked styrene, cross-linked acrylic resin, and melamine resin can be cited. As a particle size, it is preferably 10nm to 5μm, and more preferably 50nm to 3μm. The particle size can be obtained by the Coulter counter method. As a melt resistivity regulator, a combination of metal compounds such as calcium, magnesium, and potassium and phosphorus compounds can be cited.
[0114] When the polyester resin (D) is used as a masterbatch of a melt resistivity modifier, in order to reduce the melt resistance, it is preferred to combine at least one of a magnesium compound and a calcium compound with a phosphorus compound, and further, an alkali metal compound may be combined as needed. In particular, a combination of a magnesium compound, an alkali metal compound, and a phosphorus compound is preferred. In addition, a combination of a calcium compound and a phosphorus compound is a preferred combination because internal particles serving as a lubricant can be generated by the reaction of calcium and the phosphorus compound.
[0115] As the magnesium compound and the calcium compound, known compounds can be used. For example, lower fatty acid salts such as acetates and alcohol salts such as methoxides can be cited. These can be used alone or in combination of two or more. In particular, magnesium acetate and calcium acetate are preferred.
[0116] The amount of magnesium and calcium is preferably 400 to 2700 ppm by mass relative to the polyester resin (D). The more preferred amount of magnesium and calcium is 450 to 2500 ppm by mass, and even more preferably 450 to 2000 ppm by mass. It should be noted that the above-mentioned amount of magnesium and calcium is the amount of each element when only a magnesium compound or only a calcium compound is used, and the total amount when both are used.
[0117] As the alkali metal of the alkali metal compound, lithium, sodium, and potassium can be cited. In addition, as the alkali metal compound, for example, lower fatty acid salts such as lithium acetate and potassium acetate, and alcohol salts such as potassium methoxide can be cited, and these can be used alone or in combination of two or more. As the alkali metal, potassium is preferred because it has a large effect of reducing the melting resistance. As the alkali metal compound, acetate is preferred, and potassium acetate is more preferred.
[0118] The amount of the alkali metal element is preferably 40 to 270 ppm by mass relative to the polyester resin (D). When the amount of the alkali metal element is less than 40 ppm by mass, a large amount of polyester resin (D) needs to be added in order to improve the film forming properties during film production. When the amount of the alkali metal element is more than 270 ppm by mass, it may lead to a decrease in heat resistance and poor coloring of the film, which is not preferred. The preferred amount of the alkali metal element is 45 to 250 ppm by mass, and the more preferred amount of the alkali metal element is 45 to 200 ppm by mass. When the amount of magnesium metal element, calcium metal element, and alkali metal element is less than the above range, the melt resistance becomes high, and in order to improve the film forming properties during film production, it is sometimes necessary to add a large amount of polyester resin (D). When it exceeds the above range, the amount of insoluble foreign matter generated increases, and the coloring of the film sometimes becomes stronger.
[0119] Examples of phosphorus compounds include phosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, phosphinic acid, and ester compounds thereof. For example, phosphoric acid, trimethyl phosphate, tributyl phosphate, triphenyl phosphate, monomethyl phosphate, dimethyl phosphate, monobutyl phosphate, and dibutyl phosphate; phosphorous acid, trimethyl phosphite, tributyl phosphite, methylphosphonic acid, dimethyl methylphosphonate, dimethyl ethylphosphonate, dimethyl phenylphosphonate, diethyl phenylphosphonate, diphenyl phenylphosphonate, ethyl diethylphosphonoacetate, phosphinic acid, methylphosphinic acid, dimethylphosphinic acid, phenylphosphinic acid, diphenylphosphinic acid, methyl dimethylphosphinic acid, and methyl diphenylphosphinic acid. Among them, triesters of phosphoric acid having an alkyl group having 2 to 4 carbon atoms are preferably used. Specifically, triethyl phosphate, tripropyl phosphate, tributyl phosphate, and the like can be mentioned, and these can be used alone or in combination of two or more. In particular, triethyl phosphate is preferred because it is considered to form a complex having an appropriate degree of interaction with magnesium and calcium ions, and can provide a polyester resin having low melt resistance, less foreign matter, and excellent color tone.
[0120] The amount of phosphorus relative to the polyester resin (D) is preferably 200 to 4000 mass ppm. When the amount of phosphorus is less than 200 mass ppm, the amount of insoluble foreign matter generated increases. The further foreignified magnesium and calcium have a weaker effect on reducing the melt resistance. In addition, it sometimes leads to a decrease in heat resistance and thus a stronger coloring of the film. When the amount of phosphorus is greater than 4000 mass ppm, the melt resistance becomes higher due to the interaction of excessive phosphorus compounds with magnesium and calcium ions, so it is not preferred. The amount of phosphorus is more preferably 300 mass ppm or more, and more preferably 350 ppm or more. In addition, the amount of phosphorus is more preferably 3500 mass ppm or less, more preferably 3000 mass ppm or less, particularly preferably 2500 mass ppm or less, and most preferably 2000 mass ppm or less.
[0121] In the polyester resin (D), when the amount of magnesium element is m (mol%), the amount of alkali metal element is k (mol%), and the amount of phosphorus element is p (mol%) relative to the dicarboxylic acid component, the molar ratio of magnesium element, alkali metal element, and phosphorus element satisfies the following formula, because foreign matter and coloration are reduced and the effect of reducing melt resistance is higher, which is preferred. 1.5≤(m+k / 2) / p≤5 "(m+k / 2) / p" is more preferably 1.8 or more, further preferably 2.0 or more, and particularly preferably 2.3 or more. "(m+k / 2) / p" is more preferably 4 or less, further preferably 3.5 or less. It should be noted that k may be 0.
[0122] In the polyester resin (D), when the amount of calcium element is c (mol%) and the amount of phosphorus element is p (mol%) relative to the dicarboxylic acid component, when the molar ratio of calcium element to phosphorus element satisfies the following formula, foreign matter and coloration are reduced and the effect of reducing melt resistance is higher, so it is preferred. 0.01≤c / p≤5 c / p is 0.05 or more, more preferably 4.0 or less, 0.1 or more, and further preferably 3.0 or less.
[0123] In the production of the polyester resin (D), the magnesium compound, calcium compound, phosphorus compound, and alkali metal compound can be added during the polymerization of the polyester. Since the acid component of the polyester can form a salt with calcium ions, magnesium ions, or alkali metal ions to suppress foreignization and can be uniformly dispersed in the oligomer, it is preferably added during the esterification step or between the end of the esterification step and the start of the polymerization step. In the production of the polyester resin (D), antimony compounds, aluminum compounds, germanium compounds, titanium compounds, etc. can be used as the polymerization catalyst.
[0124] Various types of polyester resins (D) can be used. When the total amount of the polyester resin (A), the polyester resin (B) and the polyester resin (D) is taken as 100 parts by mass, the content of the polyester resin (D) is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, further preferably 70 parts by mass or less, particularly preferably 60 parts by mass or less, and most preferably 50 parts by mass or less. If the content is larger than the above, the economic significance and environmental significance of using the recycled polyester resin will be weakened.
[0125] [Polyester resin composition (E)] The polyester film is prepared by melt-mixing polyester resin (A) and polyester resin (B) or polyester resin composition (C) as raw material polyester resins and, if necessary, polyester resin (D) to form a film according to a predetermined method.
[0126] Thus, the polyester resin constituting the film is referred to as the polyester resin composition (E). In the case of a polyester film composed of multiple layers described below, the polyester resin constituting the layers containing the polyester resin (A) and the polyester resin (B) is referred to as the polyester resin composition (E). When the polyester resin (D) is not used, the polyester resin composition (C) is the polyester resin composition (E). The composition and intrinsic viscosity of the polyester resin composition (E) are the same as those described for the polyester resin (D).
[0127] The amount of antimony element in the polyester resin composition (E) is preferably 10 mass ppm or more, more preferably 15 mass ppm or more, and further preferably 20 mass ppm or more. The amount of antimony element in the polyester resin composition (E) is preferably 250 mass ppm or less, more preferably 200 ppm or less, and further preferably 180 ppm or less. By being within the above range, a film with little deterioration, high transparency, and low haze can be obtained while ensuring economic efficiency.
[0128] The amount of germanium in the polyester resin composition (E) is preferably 0.1 mass ppm or more, more preferably 0.15 mass ppm or more, and further preferably 0.20 mass ppm or more. The amount of germanium in the polyester resin composition (E) is preferably 5 mass ppm or less, more preferably 4 ppm or less, and further preferably 3 ppm or less. By being within the above range, a film with little deterioration can be obtained while ensuring economic efficiency.
[0129] The amount of aluminum element in the polyester resin composition (E) is preferably 1 mass ppm or more, more preferably 3 mass ppm or more, and further preferably 5 mass ppm or more. The amount of aluminum element in the polyester resin composition (E) is preferably 20 mass ppm or less, more preferably 17 ppm or less, and further preferably 15 ppm or less. By being within the above range, a film with little deterioration can be obtained while ensuring economic efficiency.
[0130] The CT content in the polyester resin composition (E) is preferably 6600 mass ppm or less, more preferably 6400 mass ppm or less, and further preferably 6000 mass ppm or less. The CT content in the polyester resin composition (E) is preferably 3000 mass ppm or more, and further preferably 4000 mass ppm or more.
[0131] The ratio of the amount of antimony element to the amount of aluminum element (Sb amount / Al amount) in the polyester resin composition (E) is preferably 1 or more, more preferably 5 or more, further preferably 18 or more, and particularly preferably 10 or more. The Sb amount / Al amount in the polyester resin composition (E) is preferably 200 or less, more preferably 170 or less, further preferably 150 or less, and particularly preferably 130 or less. By setting it within the above range, a film with little deterioration, high transparency, and low haze can be obtained while ensuring economic efficiency.
[0132] In order to stably adhere the molten resin to the cooling roll using static electricity during the film production process, the melt resistance of the polyester composition (E) is preferably 0.05×10 8 ~10×10 8 Ω·cm. The melting resistance is more preferably 0.1×10 8 On the other hand, 5×10 8Below, more preferably 1×10 8 As follows. The melt resistance can be adjusted by the amount and composition of the polyester composition (D) used as a masterbatch of a melt resistivity regulator. For example, if the polyester resin (A) is derived from a PET bottle, it usually does not contain a melt resistivity regulator, and the amount of the polyester resin (D) can be increased. If the polyester resin (A) is derived from a film recycling material and contains a melt resistivity regulator, the amount of the polyester resin (D) can be reduced. In addition, the polyester resin (A) sometimes contains a phosphorus compound as a catalyst aid and stabilizer. When the phosphorus compound has a function as a melt resistivity regulator, the amount of the phosphorus compound in the polyester resin (D) can be reduced.
[0133] Specifically, the amount of magnesium element in the polyester composition (E) is preferably adjusted to 15 to 150 mass ppm, more preferably 20 to 120 mass ppm. Furthermore, the amount of alkali metal elements is preferably 1.5 to 15 mass ppm, more preferably adjusted to 2 to 12 mass ppm. In this case, the calcium compound may not be contained. In addition, when a calcium compound is contained, the amount of calcium element is preferably 15 to 350 mass ppm, more preferably 20 to 300 mass ppm, and the upper limit may be arbitrarily 250 mass ppm, 200 mass ppm, or 150 mass ppm. In this case, a magnesium compound may be contained. It should be noted that this value is a value excluding lubricant particles derived from calcium carbonate and the like.
[0134] The amount of phosphorus in the polyester composition (E) includes phosphorus derived from the polyester resin (A) and the polyester resin (B), but since these phosphorus may have little effect on adjusting the melting resistance, the preferred amount of phosphorus in the polyester composition (E) is not a fixed value, and is preferably an amount that gives an appropriate melting resistance range in consideration of the amounts of phosphorus contained in the polyester resin (A) and the polyester resin (B). For example, 10 to 400 mass ppm is preferred, 15 to 300 mass ppm is more preferred, and the upper limit can be arbitrarily 250 mass ppm, 200 mass ppm, or 150 mass ppm.
[0135] The intrinsic viscosity retention rate of the polyester resin composition (E) is preferably 89% or more, more preferably 90% or more, further preferably 91% or more, particularly preferably 92%, and most preferably 93% or more. The intrinsic viscosity retention rate of the polyester resin composition (E) is preferably 100%, but is preferably 99% or less, more preferably 98% or less in practice.
[0136] Various properties of the polyester resin composition (E) are the same as those described for the polyester resin composition (C).
[0137] The film may contain various additives other than the polyester resin, depending on its use and required properties. As additives, in addition to the various additives listed in the polyester resin (D), resins such as polyamide, polyimide, polycarbonate, polyurethane, polyether, polyphenylene sulfide, polyphenylene sulfide, polyetherimide, and polyphenylene ether may be added. If it is a porous polyester film, a porous imparting agent such as polystyrene or polyolefin may be added. Relative to the total amount of the polyester resin composition (E) and the resins other than the polyester resin composition (E), the addition amount of the resins other than the polyester is preferably 1 to 30% by mass, more preferably 2 to 20% by mass.
[0138] [Polyester film] The polyester film can be made into a film by extruding it from a die onto a cooling roll after melt kneading by an extruder as long as it is an unstretched film. Alternatively, the film can be made by a calendering method. In the case of a stretched film, the unstretched film obtained above can be stretched in the longitudinal direction or the width direction to obtain a single-screw stretched or twin-screw stretched polyester film.
[0139] The stretching method, for example, can be performed between rollers with a difference in circumferential speed when stretching in the length direction. For stretching in the width direction, for example, the two ends of the film are held by a movable clamp and guided to a tenter, and the film can be stretched by expanding the width of the movable track of the clamp. In the case of sequential twin-screw stretching, it can be performed in any direction first, but it is usually more common to stretch in the length direction first. In addition, a twin-screw stretching machine can be used to stretch in the length direction and the width direction simultaneously or in any order. Stretching can be multi-stage stretching, and when there are multiple stages, the length direction and the width direction can be performed alternately.
[0140] The stretching temperature is preferably in the range of glass transition temperature (Tg) of the polyester resin composition (E) + 5 to Tg + 70°C, more preferably in the range of Tg + 10 to Tg + 60°C. The stretching ratio is 10 times or less, further 8 times or less, and particularly preferably 6 times or less in at least one direction. In order to impart strong orientation, the stretching ratio is preferably 2 times or more, more preferably 2.5 times or more, and particularly preferably 2.8 times or more. Even twin-screw stretching can make a film with strong single-screw properties, and the stretching ratio in the direction perpendicular to the main stretching direction can be below the above.
[0141] The stretched polyester film is preferably heat-set at a temperature below the crystalline melting point (mp) of the polyester resin composition (E). The heat-setting temperature is preferably mp-10°C or less, more preferably mp-20°C or less. The lower limit of the heat-setting temperature is related to the composition of the polyester resin composition (E) and the heat resistance to be imparted to the film, but is generally preferably 100°C or more, more preferably 130°C or more. For example, when the polyester resin composition (E) is a polyethylene terephthalate film, the heat-setting temperature is preferably 170 to 250°C, more preferably 180 to 240°C.
[0142] Heat setting is preferably performed while maintaining the stretching ratio, but in order to reduce the thermal shrinkage of the polyester film, a relaxation process of shrinking the polyester film by about 1 to 5% from the stretched state may be applied between heat setting and cooling. The relaxation process is preferably performed at 100°C to the heat setting temperature - 5°C, more preferably 120°C to the heat setting temperature - 10°C. The relaxation rate is preferably 1.5 to 4%.
[0143] The polyester film may be a single layer or a multilayer. In the case of a multilayer, at least one layer needs to be a polyester resin composition (E). It is also possible that a plurality of layers or all layers are a polyester resin composition (E), in which case the composition ratios of the polyester resin (A), the polyester resin (B), and the polyester resin (D) may be different based on the different layers. Furthermore, in the case of a multilayer structure, it is preferably a structure of three or more layers, with the middle layer being a layer of the polyester resin composition (E) and the outermost layer being a recycled polyester resin A. In particular, it is preferably a structure not containing the polyester resin A recycled from the street market. In the case of multiple layers, the thickness of the polyester resin composition (E) layer is preferably 30% or more of the total film thickness, more preferably 50% or more, further preferably 60% or more, particularly preferably 70% or more. If it is less than the above, the significance of using the recycled polyester (A) becomes small.
[0144] The thickness of the polyester film is preferably 1 to 2000 μm, more preferably 2 to 1000 μm. It can be set to an appropriate range according to the application. For example, as a representative thickness, it is 20 to 150 μm in optical applications, 10 to 100 μm in transfer and release films, 5 to 50 μm in general packaging films, and 200 to 1000 μm for thick objects such as trays.
[0145] <Surface treatment of polyester film> The polyester film is preferably subjected to a surface treatment in order to improve adhesion with adhesives, coating materials, inks, etc. Examples of the surface treatment include corona treatment, plasma treatment, and flame treatment.
[0146] The polyester film may be provided with an easy-adhesion layer. As the resin used in the easy-adhesive layer, polyester resin, polyurethane resin, polycarbonate resin, acrylic resin, etc. can be used, preferably polyester resin, polyester polyurethane resin, polycarbonate polyurethane resin, acrylic resin. The easy-adhesive layer is preferably cross-linked. As a cross-linking agent, isocyanate compounds, melamine compounds, epoxy resins, oxazoline compounds, etc. can be cited. In addition, adding water-soluble resins such as polyvinyl alcohol is a useful means for improving the adhesion with a polarizer.
[0147] The easy-adhesion layer can be formed by applying these resins and, if necessary, adding a crosslinking agent, particles, etc. as a water-based coating on a polyester film and drying the coating. Examples of the particles include those used in the above-mentioned polyester film. The easy-adhesive layer can be set off-line on the film after stretching, but is preferably set online in the film-making process. When set online, it can be arbitrarily before longitudinal stretching or transverse stretching, but it is preferably applied just before transverse stretching, and preheated, heated, and heat-treated by a tenter to dry and crosslink. It should be noted that when the online coating is performed just before longitudinal stretching by a roller, it is preferably guided to the stretching roller after being dried by a vertical dryer after coating. The coating amount of the adhesive layer is preferably 0.01 to 1.0 g / m 2 , more preferably 0.03 to 0.5 g / m 2 .
[0148] The polyester film produced by the present invention can be used for various purposes without limitation. For example, the polyester film can be used for substrate films of prisms and lens sheets, hard coating films, electrode substrate films of touch panels, anti-scattering films, anti-reflection films, polarizer protective films, polarizing plate protective films, surface protective films of display devices and circuits, etc., release films of ceramic green sheets, etc., release films of polarizing plates, transfer films, in-mold transfer films, in-mold forming films, barrier films with aluminum or inorganic oxides vapor-deposited, solar cell backsheets, circuit substrate films, flat cable substrate films, magnetic recording medium substrate films, ink ribbons, image receiving films, labels, tags, cards, films for packaging bags, heat shrinkable films, trays, cover tapes, etc. Additives can be added to the membrane according to respective uses, and the membrane can be processed after it has functions.
[0149] [Method for producing polyester resin (B)] Next, the method for producing the polyester resin (B) will be described. As the method for producing the polyester resin (B), a method having known steps can be used except that a polyester polymerization catalyst composed of an aluminum compound and a phosphorus compound is used as a catalyst, but it is preferred to add a polymerization catalyst so as to satisfy the following (4) and (5), and it is further preferred to add a polymerization catalyst so as to satisfy the following (6) in addition to the following (4) and (5). It should be noted that the preferred numerical ranges for the following (4) to (6) are as described above. (4) The content of aluminum in the polyester resin (B) is 5 to 50 ppm by mass, (5) The phosphorus content in the polyester resin (B) is 5 to 1000 ppm by mass, (6) The residual molar ratio of phosphorus element to aluminum element in the polyester resin (B) is 1.00 or more and 5.00 or less.
[0150] The method for producing the polyester resin (B) preferably comprises a first step of synthesizing a polyester or an oligomer thereof as a polycondensate (low-cost condensate) as an intermediate, and a second step of further polycondensing the intermediate.
[0151] In addition, it is preferred that a solution S containing an aluminum compound and a solution T containing a phosphorus compound are added to the intermediate after the first step and before the second step to satisfy the following (7) to (9). Since the polycarboxylic acids and their ester-forming derivatives, hydroxycarboxylic acids and their ester-forming derivatives which may be added in a small amount, and cyclic esters which may be added in a small amount used to produce the polyester resin (B) are not distilled out of the reaction system to the outside of the system during the polymerization, almost 100% of the amount initially added to the system as a catalyst remains in the polyester resin (B) produced by the polymerization, and the mass of the "produced polyester resin" can be calculated based on these added amounts. (7) the amount of aluminum element added is 5 to 50 ppm by mass (more preferably 7 to 40 ppm by mass, further preferably 10 to 30 ppm by mass, and particularly preferably 15 to 25 ppm by mass) relative to the produced polyester resin (B), (8) The amount of phosphorus added is 5 to 1500 ppm by mass (more preferably 10 to 500 ppm by mass, further preferably 20 to 200 ppm by mass, and particularly preferably 30 to 100 ppm by mass) relative to the produced polyester resin (B). (9) The molar ratio of the amount of phosphorus added in (8) to the amount of aluminum added in (7) (hereinafter referred to as "the molar ratio of phosphorus added to aluminum") is 1.00 or more and 7.00 or less (more preferably 1.50 to 6.00, and even more preferably 2.00 to 5.00).
[0152] The method for producing the polyester or its oligomer which is the low-cost polycondensate (oligomer) synthesized in the first step is not particularly limited.
[0153] The method for producing the polyester resin (B) can be carried out by a method having a currently known process, in addition to paying attention to the point that a polyester polymerization catalyst composed of an aluminum compound and a phosphorus compound is used as a catalyst and the amount of the polyester polymerization catalyst added. For example, when producing polyethylene terephthalate, it can be produced by the following method: a direct esterification method in which terephthalic acid and ethylene glycol and other copolymer components as required are directly reacted, water is distilled off and esterification is carried out, and then polycondensation is carried out under normal pressure or reduced pressure; or an ester exchange method in which dimethyl terephthalate and ethylene glycol and other copolymer components as required are reacted, methanol is distilled off and ester exchange is carried out, and then polycondensation is carried out under normal pressure or reduced pressure. Further, solid phase polymerization can be carried out to increase the limiting viscosity as needed. It should be noted that the amount (mass) of the generated polyester resin (B) can be calculated based on the amount (mass) of the polycarboxylic acid including dicarboxylic acid and the like used as a raw material.
[0154] In any of these embodiments, the esterification reaction or transesterification reaction may be performed in one step or in multiple steps.
[0155] In addition, the polyester resin produced by the melt polymerization method can be additionally polymerized by the solid phase polymerization method. The solid phase polymerization reaction can be carried out using a continuous apparatus in the same manner as the melt polycondensation reaction.
[0156] In the case of a continuous polycondensation apparatus (polymerization method of three stages including an initial stage, an intermediate stage, and a late stage) composed of three or more reactors, the first stage is regarded as the initial stage, the final stage is regarded as the late stage, and the stage from the second stage to before the final stage is regarded as the intermediate stage. The reaction conditions of the polymerization reaction in the intermediate stage are preferably conditions between the reaction conditions in the initial stage and the reaction conditions in the final stage. It is preferred to smoothly distribute the degree of increase in the limiting viscosity reached in each of these polymerization reaction steps.
[0157] (Solid Phase Polymerization) In order to increase the intrinsic viscosity, the polyester resin produced by the melt polymerization method may be subjected to solid phase polymerization. The solid phase polymerization may be a batch polymerization method or a continuous polymerization method, but the solid phase polymerization is preferably carried out in a continuous apparatus like the melt polymerization.
[0158] In order to reduce the CT content of the polyester resin (B), it is preferred to subject the polyester resin produced by the melt polymerization method to additional polymerization by the solid phase polymerization method. The solid phase polymerization is carried out by making the polyester obtained in the second step (melt polymerization) into a powdery form. The powdery form refers to polyester in the form of chips, pellets, flakes, or powder, preferably chips or pellets.
[0159] The solid phase polymerization is carried out by heating the polyester in powder form at a temperature below the melting point of the polyester under an inert gas flow or under reduced pressure. The solid phase polymerization process may be carried out in one step or in multiple steps.
[0160] The powdery polyester supplied to the solid phase polymerization step may be heated to a temperature lower than the temperature at which the solid phase polymerization is previously performed to perform preliminary crystallization, and then supplied to the solid phase polymerization step.
[0161] Such a pre-crystallization process can be carried out by heating the powdered polyester in a dry state, usually at a temperature of 120 to 200°C, preferably at 130 to 180°C, for 1 minute to 4 hours, or by heating the powdered polyester in an atmosphere of water vapor, an atmosphere of an inert gas containing water vapor, or an atmosphere of air containing water vapor, usually at a temperature of 120 to 200°C for more than 1 minute.
[0162] As described above, the melt-polymerized polyester is, for example, fragmented and then transported to a storage silo or a solid phase polymerization step through a transport pipe. If such fragment transportation is performed by a low-density transport method using air forcing, for example, a large impact force is generated due to the collision between the surface of the melt-polymerized polyester fragments and the pipe, resulting in a large amount of particles and film-like substances. Such particles and film-like substances have the effect of promoting the crystallization of the polyester, and when they exist in large quantities, the transparency of the obtained molded body becomes very poor. Therefore, adding such a step of removing particles and film-like substances is one of the preferred embodiments.
[0163] The above-mentioned method for removing particles and film-like substances is not limited. For example, the following treatment methods can be cited: in the intermediate process between the solid-phase polymerization process and the post-process set after the solid-phase polymerization process, a vibrating screen process and an air flow classification process using air flow, a gravity classification process, etc. are respectively set.
[0164] When the aluminum compound and the phosphorus compound are used as catalysts, they are preferably added in the form of a slurry or a solution, more preferably a solution dissolved in a solvent such as water or a glycol, further preferably a solution dissolved in water and / or a glycol, and most preferably a solution dissolved in ethylene glycol.
[0165] It is preferred that the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved are added at any stage before the start of the polymerization reaction in the production process of the polyester resin (B) so that the content (residual amount) in the polyester resin (B) satisfies the ranges of (4) to (6) above.
[0166] By adding the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved so that the content (residual amount) in the polyester resin (B) satisfies the above (4) to (6), a complex having catalytic activity is functionally formed in the polymerization system, and sufficient polymerization activity can be exerted. In addition, the generation of aluminum-based foreign matter can also be suppressed.
[0167] It should be noted that, even if the polymerization of the polyester resin is carried out under reduced pressure, almost 100% of the aluminum atoms in the aluminum compound that functions as a catalyst initially added to the system will remain in the polyester resin (B) produced by the polymerization. That is, since the amount of the aluminum compound hardly changes before and after the polymerization, if the amount of aluminum atoms added to the intermediate is 5 to 50 mass ppm, the content of aluminum atoms in the polyester resin (B) will also be 5 to 50 mass ppm.
[0168] In addition, when the phosphorus compound functions as a catalyst together with the aluminum compound, a part (about 10 to 40%) of the amount initially added to the system as a catalyst is removed to the outside of the system when the polymerization of the polyester resin is placed under a reduced pressure environment, but this removal ratio varies depending on the added molar ratio of phosphorus atoms to aluminum atoms, the alkalinity and acidity of the solution in which the aluminum compound is dissolved and the solution in which the phosphorus compound is dissolved, the method of adding the aluminum-containing solution and the phosphorus-containing solution (single-liquefaction addition, separate addition), etc. Therefore, the amount of the phosphorus compound added to the polyester resin (B) as the final product is preferably appropriately set so as to satisfy the above (5).
[0169] It is preferred to add the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved at the same time, or to mix the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved in advance in a ratio to be added to the intermediate to prepare a mixed solution, and then add the liquefied mixed solution to the intermediate. As a method of liquefaction in advance, there can be cited a method of mixing the respective solutions in a tank, and a method of converging and mixing in the middle of a pipeline where a catalyst is added.
[0170] It should be noted that when adding to the reaction container, it is preferred to increase the stirring of the reaction container. When adding in a pipe between reaction containers, it is preferred to provide an inline mixer or the like so that the added catalyst solution can be quickly and uniformly mixed.
[0171] When the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved are added separately, excessive foreign matter caused by the aluminum compound is likely to occur, the temperature of the crystallization during heating becomes lower, the temperature of the crystallization during cooling becomes higher, and sometimes sufficient catalyst activity cannot be obtained. By adding the aluminum compound and the phosphorus compound simultaneously, a complex of the aluminum compound and the phosphorus compound that brings polymerization activity can be generated quickly and without waste, while when they are added separately, the complex of the aluminum compound and the phosphorus compound is not generated sufficiently, and there is a concern that the aluminum compound that cannot form a complex with the phosphorus compound will precipitate as foreign matter.
[0172] In addition, the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved are preferably added before the start of the polymerization reaction and after the esterification reaction or the transesterification reaction is completed, and more preferably, the solution S in which the aluminum compound is dissolved and the solution T in which the phosphorus compound is dissolved are added to the intermediate after the first step and before the second step. If they are added before the esterification reaction or the transesterification reaction is completed, the amount of aluminum-based foreign matter may increase.
[0173] When the polyester resin (B) is composed of at least one selected from polycarboxylic acids and their ester-forming derivatives and at least one selected from polyols and their ester-forming derivatives, the solution S in which the aluminum compound is dissolved is preferably a diol solution in which the aluminum compound is dissolved, and the solution T in which the phosphorus compound is dissolved is preferably a diol solution in which the phosphorus compound is dissolved.
[0174] <Heat treatment of phosphorus compounds> The phosphorus compound used in the production of the polyester resin (B) is preferably a phosphorus compound that has been heat-treated in a solvent. The solvent used is not limited as long as it is at least one selected from the group consisting of water and alkyl glycols. As the alkyl glycol, a solvent that dissolves the phosphorus compound is preferably used, and a diol that is a component of the polyester resin (B) such as ethylene glycol is more preferably used. The heat treatment in the solvent is preferably performed after the phosphorus compound is dissolved, even if it is not completely dissolved.
[0175] Regarding the conditions for the heat treatment, the heat treatment temperature is preferably 170 to 196° C., more preferably 175 to 185° C., and even more preferably 175 to 180° C. The heat treatment time is preferably 30 to 240 minutes, and more preferably 50 to 210 minutes.
[0176] The concentration of the phosphorus compound during the heat treatment is preferably 3 to 10% by mass.
[0177] The heat treatment can make the acidity of the phosphorus compound contained in the diol solution constant, and by using it together with the aluminum compound, the polymerization activity can be improved while reducing the amount of aluminum-based foreign matter generated by the polymerization catalyst, and the amount of phosphorus compound distilled off in the polymerization process can be suppressed, thereby improving economic efficiency. Therefore, the heat treatment is preferably performed. [Example]
[0178] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples. It should be noted that the evaluation methods used in the examples and comparative examples are as follows.
[0179] [Evaluation Method] (1) Intrinsic viscosity (IV) About 3 g of the sample was freeze-ground and dried at 140°C for 15 minutes, and 0.20 g was weighed and stirred at 100°C for 60 minutes in 20 ml of a mixed solvent of 1,1,2,2-tetrachloroethane and p-chlorophenol at a mass ratio of 1:3 to completely dissolve the sample. The sample was then cooled to room temperature and filtered through a glass filter. The dripping time of the sample and the solvent was measured using an Ubbelohde viscometer (manufactured by Lihe Co., Ltd.) adjusted to 30°C, and the intrinsic viscosity [η] was calculated according to the following formula. ηSp=(τ-τ0)τ0 Here, [η]: Intrinsic viscosity (dl / g) ηSp: Specific viscosity (-) K': Huggins' constant (= 0.33) C: concentration (=1g / dl) τ: Sample dripping time (sec) τ0: Solvent dripping time (sec)
[0180] (2) Content of specified metal elements in polyester resin The polyester resin described below was weighed in a platinum crucible, carbonized in an electric furnace, and then ashed at 550°C for 8 hours using a muffle furnace. The ashed sample was dissolved in 1.2M hydrochloric acid to prepare a sample solution. The sample solution prepared was measured under the following conditions, and the concentrations of antimony, germanium, and titanium in the polyester resin were determined by high-frequency inductively coupled plasma emission spectrometry. Device: CIROS-120 manufactured by SPECTRO Plasma power: 1400W Plasma gas: 13.0L / min Auxiliary gas: 2.0L / min Atomizer: Cross Atomizer Spray chamber: Cyclone chamber Measurement wavelength: 167.078nm
[0181] (3) Phosphorus content in polyester resin polyester film After wet decomposition of the polyester resin using sulfuric acid, nitric acid, and perchloric acid, it was neutralized using aqueous ammonia. After adding ammonium molybdate and hydrazine sulfate to the prepared solution, an ultraviolet-visible spectrophotometer (manufactured by Shimadzu Corporation, UV-1700) was used to measure the absorbance at a wavelength of 830 nm. The concentration of phosphorus in the polyester resin was determined from a pre-prepared standard curve.
[0182] (4) Amount of aluminum foreign matter in polyester resin 30g of polyester resin and 250mL of a mixed solution of p-chlorophenol / tetrachloroethane (3 / 1: mass ratio) were added to a 500mL conical flask with a stirrer, and heated and dissolved at 100-105°C for 1.5 hours using a hot stirrer. For the solution, a polytetrafluoroethylene membrane filter with a diameter of 47mm / pore size of 1.0μm (PTFE membrane filter manufactured by Advantec, product name: T100A047A) was used to filter and separate foreign matter. The effective filter diameter was set to 37.5mm. After the filtration was completed, 50mL of chloroform was used for cleaning, and then the filter was dried.
[0183] A scanning fluorescent X-ray analyzer (manufactured by RIGAKU, ZSX100e, Rh tube ball 4.0kW) was used to quantify the amount of aluminum on the filter surface of the membrane filter. The quantification was performed on the portion with a diameter of 30 mm in the center of the membrane filter. It should be noted that the aluminum content of the standard curve of the fluorescent X-ray analysis was obtained by using a known polyethylene terephthalate resin, and the apparent aluminum content was expressed in ppm. The determination was carried out by using pentaerythritol as a spectroscopic crystal at an X-ray output power of 50kV-70mA, using a PC (proportional counter) as a detector, and measuring the Al-Kα ray intensity under the conditions of PHA (pulse height analyzer) 100-300. The aluminum content in the polyethylene terephthalate resin used for the standard curve was quantified by high-frequency inductively coupled plasma emission spectrometry.
[0184] (5) Confirmation of the presence of hindered phenol structures or their decomposition residues in the sample 420 mg of the sample was dissolved in 2.7 mL of a mixed solvent of hexafluoroisopropanol and deuterated benzene mixed at a ratio of 1:1 (mass ratio), and 10 μL of a 25% phosphoric acid deuterated acetone solution was added and centrifuged. Then, 100 to 150 mg of trifluoroacetic acid was added to the supernatant, and P-NMR measurement was immediately performed under the following conditions. Apparatus: Fourier transform nuclear magnetic resonance apparatus (manufactured by BRUKER, AVANCE 500) 31P resonance frequency: 202.456MHz Locking solvent: deuterated benzene Detection pulse deflection angle: 65° Data reading time: 1.5 seconds Delay time: 0.5 seconds Proton decoupling: Complete decoupling Measuring temperature: 25~35℃ Scan times: about 20,000 to 30,000 times The peak wavelengths of the residues of the chemical formula numbers shown in Table 1 are as follows. When these peak wavelengths are detected, it is determined that the sample has a hindered phenol structure. Chemical formula 1: 34.5ppm, Chemical formula 4: 30.5ppm, Chemical formula 7: 53.6ppm, Chemical formula 2: 33.8ppm, Chemical formula 5: 30.1ppm, Chemical formula 8: 53.0ppm, Chemical formula 3: 31.9ppm, Chemical formula 6: 28.7ppm, Chemical formula 9: 51.3ppm.
[0185] (6) Quantification of cyclic trimers The sample is frozen and crushed or fragmented, and 100 mg of the sample is accurately weighed. It is dissolved in 3 mL of a hexafluoroisopropanol / chloroform mixture (volume ratio = 2 / 3), and 20 mL of chloroform is further added for dilution. 10 mL of methanol is added to it to precipitate the polymer and then filtered. The filtrate is evaporated to dryness and 10 mL of dimethylformamide is used to make the volume constant. Next, the amount of cyclic trimer in the polyester resin or in the hollow molded body is quantified using the following high performance liquid chromatography. Repeat the above operation 5 times, and the average value is taken as the CT content. Device: L-7000 (manufactured by Hitachi, Ltd.) Chromatographic column: μ-Bondasphere C18 5μ100 angstroms 3.9 mm×15 cm (manufactured by Waters) Solvent: Eluent A: 2% acetic acid / water (v / v) Eluent B: acetonitrile Gradient B%: 10→100% (0→55 min) Flow rate: 0.8 mL / min Temperature: 30℃ Detector: UV-259nm
[0186] (7) Intrinsic viscosity retention rate of the sample The sample was dried at 140°C in a vacuum dryer for 16 hours to produce a dry polyester with a moisture content of less than 150 ppm. As for the sample, in the case of a film, the film was cut into pieces of about 1 cm square as pellets, and the pellets of the resin pellets were directly used as samples. Using the dry polyester, the re-mixed product was re-mixed once in a twin-screw extruder under the following conditions, and the intrinsic viscosity of the re-mixed product was measured, and the intrinsic viscosity retention rate was calculated using the following formula. In addition, using the above-mentioned dry polyester resin, the re-mixed product was re-mixed three times in a twin-screw extruder under the following conditions, and the intrinsic viscosity of the re-mixed product was measured, and the intrinsic viscosity retention rate was calculated using the following formula. It should be noted that the method for measuring the intrinsic viscosity is consistent with that described in (1) above. Twin-screw extruder: KZW15TW-45 / 60MG-NH (-2200) manufactured by TECHNOVEL Set temperature: 260℃ (actual temperature 268~270℃) Screw speed: 200rpm Discharge volume 1.7~2.0kg / h Intrinsic viscosity retention rate (%) = 100 × intrinsic viscosity of re-mixed product / intrinsic viscosity of sample The water content of 0.6 g of the sample was measured by a coulometric titration method using a Karl Fischer moisture meter (CA-200, manufactured by Mitsubishi Chemical Corporation Analytech) at 230° C. for 5 minutes and a nitrogen gas flow of 250 mL / min.
[0187] (8) Composition analysis of polyester resin 20 mg of the polyester resin was dissolved in 0.6 mL of a mixed solvent of deuterated hexafluoroisopropanol and deuterated chloroform in a ratio of 1:9 (volume ratio) and centrifuged, and the supernatant was extracted and subjected to H-NMR measurement under the following conditions. Apparatus: Fourier transform nuclear magnetic resonance apparatus (made by BRUKER, AVANCE NEO 600) 1 H resonance frequency: 600.13MHz Lock solvent: deuterated chloroform Deflection angle: 30° Data reading time: 4 seconds Delay time: 1 second Measurement temperature: 30℃ Scan times: 128 times
[0188] Hereinafter, the preparation of the aluminum-containing ethylene glycol solution and the phosphorus-containing ethylene glycol solution will be described.
[0189] <Preparation of Aluminum-Containing Ethylene Glycol Solution s> An equal amount (volume ratio) of ethylene glycol is added to a preparation tank relative to a 20 g / L aqueous solution of basic aluminum acetate. After stirring for several hours at room temperature (23°C), the solution is stirred for several hours at 50-90°C under reduced pressure (3 kPa) while distilling water from the system to prepare an aluminum-containing ethylene glycol solution s containing 20 g / L of aluminum compound.
[0190] <Preparation of phosphorus-containing ethylene glycol solution t> As a phosphorus compound, Irganox 1222 (manufactured by BASF) was added to a preparation tank together with ethylene glycol, and heat-treated at 175° C. for 150 minutes while stirring under nitrogen substitution to prepare a phosphorus-containing ethylene glycol solution t containing 50 g / L of the phosphorus compound.
[0191] 〔Manufacture of polyester resin〕 <Polyester resin (B1)> In a 10L stainless steel autoclave equipped with a stirrer, a polyester oligomer having an esterification rate of about 95% composed of high-purity terephthalic acid and ethylene glycol and high-purity terephthalic acid, which had been prepared in advance, was placed and an esterification reaction was carried out at 260°C to obtain an oligomer mixture. The concentration of the acid terminal group of the obtained oligomer mixture was 750eq / ton, and the ratio of the hydroxyl terminal (OH%) was 59 mol%. To the obtained oligomer mixture, a liquefied mixed solution of the aluminum-containing ethylene glycol solution s and the phosphorus-containing ethylene glycol solution t prepared according to the above method was added and mixed. The mixed solution was prepared so that the aluminum element and the phosphorus element concentrations were 21 mass ppm and 58 mass ppm, respectively, relative to the mass of the oligomer mixture. The molar ratio of phosphorus element added relative to aluminum element was 2.41. It should be noted that the amount of polyester resin generated can be calculated based on the amount of terephthalic acid added. In this embodiment, the mixed solution was added so that the aluminum element and the phosphorus element concentrations were 21 mass ppm and 58 mass ppm, respectively, relative to the mass of the polyester resin generated. After that, the system temperature was raised to 280°C over 1 hour, and the system pressure was slowly reduced to 0.15 kPa during this period. Under this condition, a polycondensation reaction was carried out to obtain a polyester resin with an IV of 0.60 dl / g. After that, the obtained polyester resin was extruded into a strand shape and cut into a pellet shape of 2.5×3×4 mm, and then solid-phase polymerization was carried out for 7 hours at 230°C under reduced pressure using a batch-type solid-phase polymerization device to obtain a polyester resin (B1) with an intrinsic viscosity of 0.75 dl / g and a CT content of 4700 mass ppm. The residual amount of aluminum element in the polyester resin (B1) was 21 mass ppm, the residual amount of phosphorus element was 45 mass ppm, and the residual molar ratio of phosphorus element to aluminum element was 1.87. The content of aluminum element equivalent to aluminum-based foreign matter in the polyester resin (B1) was 710 mass ppm, and the L value of the polyester resin (B-1) was 58.7, which confirmed that the polyester resin (B1) had a hindered phenol structure. DEG was 1.5 mol%. The intrinsic viscosity retention rate at the first re-kneading was 98%, and that at the third re-kneading was 88%.
[0192] Polyester resin (B2) A polyester resin (B2) having an intrinsic viscosity of 0.75 dl / g and a CT content of 4700 mass ppm was obtained by the same method as the polyester resin (B1), except that the addition amounts of aluminum and phosphorus were different. The residual amount of aluminum in the polyester resin (B2) was 16 mass ppm, the residual amount of phosphorus was 26 mass ppm, and the residual molar ratio of phosphorus to aluminum was 1.42. The content of aluminum equivalent to aluminum-based foreign matter in the polyester resin (B2) was 2000 mass ppm, and the L value of the polyester resin (B2) was 58.5, which confirmed that the polyester resin (B2) had a hindered phenol structure. The intrinsic viscosity retention rate at the first re-mixing was 97%, and that at the third re-mixing was 87%.
[0193] Polyester resin (B3) A polyester resin (B3) having an intrinsic viscosity of 0.75 dl / g and a CT content of 4700 mass ppm was obtained by the same method as the polyester resin (B1), except that the addition amounts of aluminum and phosphorus were different. The residual amount of aluminum in the polyester resin (B3) was 10 mass ppm, the residual amount of phosphorus was 16 mass ppm, and the residual molar ratio of phosphorus to aluminum was 1.39. The content of aluminum equivalent to aluminum-based foreign matter in the polyester resin (B3) was 2300 mass ppm, the L value of the polyester resin (B3) was 56.6, and it was confirmed that the polyester resin (B3) had a hindered phenol structure. The intrinsic viscosity retention rate at the first re-mixing was 96%, and that at the third re-mixing was 86%.
[0194] Polyester resin (B4) The polyester resin (B1) and silica particles having an average particle size of 2.5 μm were charged into a twin-screw extruder and kneaded at 285° C. to prepare pellets of a masterbatch having a silica particle content of 10,000 ppm.
[0195] Polyester resin (D1) Polyethylene terephthalate pellets using antimony trioxide as a catalyst (antimony content: 230 mass ppm, phosphorus content: 50 mass ppm, intrinsic viscosity: 0.75 dl / g)
[0196] Polyester resin (D2) The polyester resin (D1) and silica particles having an average particle size of 2.5 μm were charged into a twin-screw extruder and kneaded at 285° C. to prepare pellets of a masterbatch having a silica particle content of 6000 ppm.
[0197] Polyester resin (D3) To an oligomer prepared from terephthalic acid and ethylene glycol according to a conventional method, basic aluminum acetate, magnesium acetate dihydrate, potassium acetate, and triethyl phosphate were added so that the aluminum element was 60 ppm, the magnesium element was 1000 ppm, the potassium element was 100 ppm, and the phosphorus element was 500 ppm, respectively, relative to the polyester resin after production, and the temperature of the system was raised to 280° C. over 1 hour. During this period, the pressure of the system was gradually reduced to 0.15 kPa, and a polycondensation reaction was carried out for 80 minutes under this condition to obtain pellets of a polyester resin (D3). The intrinsic viscosity of the polyester resin (D3) was 0.67 dl / g. In addition, the aluminum element content, the magnesium element content, the potassium element content, and the phosphorus element content of the polyester resin (D3) were determined by the following method.
[0198] Determination of the amount of each element in polyester resin (D3) The polyester resin was heated and melted at 280°C in a stainless steel circular ring with a thickness of 5 mm and an inner diameter of 50 mm to prepare a sample piece, and the element amount was obtained by fluorescent X-ray analysis and expressed in ppm (mass basis). It should be noted that when quantifying, a standard curve obtained by using samples with known element amounts in advance was used.
[0199] 〔Recycled polyester resin〕 <Polyester resin (A1)> As the polyester resin (A1), a recycled polyester resin flake provided by Kyoei Industry Co., Ltd. was used. According to the results of its composition analysis, it was confirmed that the recycled polyester resin flake contained 1.7 mol% of isophthalic acid component, 2.1 mol% of diethylene glycol component, and a CT content of 4900 ppm. The size of the flake was 8.6 mm. The intrinsic viscosity of the recycled polyester resin flake was 0.750 dl / g. In addition, the content of antimony element in the above-mentioned recycled polyester resin flake was 190 mass ppm, and the content of germanium element was 1.6 mass ppm. It should be noted that the content of titanium element is very small when it is less than 1 mass ppm, so the content of titanium element is omitted in Tables 2 and 3. From the content of each element of antimony, germanium, and titanium, it can be confirmed that the above-mentioned recycled polyester resin flake is a recycled polyester resin flake mainly composed of a hollow molded body of a polyester resin manufactured using an antimony catalyst. The IV retention rate of the polyester resin A1 in the first re-kneading was 88%, and the IV retention rate in the third re-kneading was 77%.
[0200] (Examples, Comparative Examples, Reference Examples) Each polyester resin was supplied to a single screw extruder at the blending ratio (parts by mass) shown in Table 2 and melted at 290°C. The molten polymer was filtered through a filter material of a stainless steel sintered body (nominal filtration accuracy 20 μm particles 95% removal), formed into a sheet through an extrusion port, and extruded onto a casting drum with a surface temperature of 30°C, and then cooled and solidified to produce an unstretched film. It should be noted that the polyester resin was supplied in a small amount and mixed in a manner that would not cause segregation and then put into the hopper. This unstretched film was stretched 3.3 times in the longitudinal direction at 95°C using rolls having a peripheral speed difference.
[0201] The single-screw stretched film was then guided to a tenter stretcher, and while the ends of the film were clamped by a clamp, it was guided to a hot air zone at a temperature of 125°C and stretched 3.5 times in the width direction. Subsequently, while maintaining the stretched width in the width direction, a heat setting treatment was performed at a temperature of 220°C for 10 seconds, and a relaxation treatment of 3.0% was further performed. After that, the two ends (ears) of the film cooled to 120°C were cut with a shear knife to obtain a twin-screw stretched PET film with a film thickness of 75 μm. The film was wound on a paper tube.
[0202] Evaluation of membrane recovery and reusability The ear portions of the films produced in Examples and Comparative Examples were cut multiple times, and the cut film pieces were fed into a twin-screw extruder and melt-kneaded at 290° C. to form pellets. The obtained pellets were further melt-kneaded at 290° C. to form pellets. The obtained second pellets were used to prepare a film in the same manner, and the film was wound around a paper tube to prepare a remelted resin film. The side surface of the wound film was observed to observe the difference in color tone. ○: No difference in color tone is perceived. △: The re-melted resin film was slightly yellowish. ×: The re-melted resin film has a distinct yellow tint.
[0203]
Table 2
[0204] Embodiments 12 to 15 The polyester resin for the intermediate layer shown in Table 3 was supplied to extruder 1, and the polyester resin for the surface layer was supplied to extruder 2 and melted at 285° C. A twin-screw stretched PET film was produced except that two types of three-layer die openings were used and the thickness of the surface layer / intermediate layer / surface layer was 1 / 8 / 1. In addition, the evaluation of the recovery and recyclability of the membrane was carried out in the same manner as in Example 1, with the membrane being a single-layer structure.
Table 3
[0205] Embodiments 16 to 17 Recycled flakes of ear parts obtained from another polyester film production line (IV = 0.61 dl / g, Sb content: 140 ppm, lubricant particles are trace amounts) were prepared as polyester resin A2, and polyester resin B5 was prepared by melt polymerization in the same manner as polyester resin B1, and the intrinsic viscosity of the melt polymerization alone was 0.67 dl / g. The polyester resins in Table 4 were used to produce the same film as in Example 1. It should be noted that after longitudinal stretching, the film was coated with an easy-adhesive coating material of the following composition on both sides and then guided to a tenter, thereby producing a twin-screw stretched PET having easy-adhesive layers on both sides.
[0206] (Adjustment of easy-adhesion coating) By carrying out transesterification and polycondensation reactions in a conventional manner, a water-dispersible sulfonic acid metal salt group-containing copolyester resin having the following composition was prepared: as dicarboxylic acid components (relative to the total dicarboxylic acid components), 46 mol% of terephthalic acid, 46 mol% of isophthalic acid and 8 mol% of 5-sodium sulfoisophthalate; as diol components (relative to the total diol components), 50 mol% of ethylene glycol and 50 mol% of neopentyl glycol were prepared. Then, 51.4 parts by mass of water, 38 parts by mass of isopropyl alcohol, 5 parts by mass of n-butyl cellosolve and 0.06 parts by mass of a nonionic surfactant were mixed, and the mixture was heated and stirred until the temperature reached 77° C., and then 5 parts by mass of the water-dispersible sulfonic acid metal salt group-containing copolyester resin was added. After continued stirring until there were no lumps of the resin, the resin aqueous dispersion was cooled to room temperature to obtain a uniform water-dispersible copolyester resin liquid having a solid content concentration of 5.0% by mass. Furthermore, 3 parts by mass of agglomerated silica particles (SYLYSIA 310 manufactured by Fuji Silysia Co., Ltd.) were dispersed in 50 parts by mass of water, and then 0.54 parts by mass of an aqueous dispersion of SYLYSIA 310 was added to 99.46 parts by mass of the above-mentioned water-dispersible copolyester resin liquid, and 20 parts by mass of water was added while stirring to obtain an easily adhesive coating.
[0207]
Table 4
[0208] As shown in Table 2, as the amount of Examples 1 to 6 and the polyester resin B1 decreases, the intrinsic viscosity retention rate tends to decrease, but still has a high intrinsic viscosity retention rate compared with Comparative Examples 1 and 2 and the reference example. According to Examples 7 to 12, even if the polyester resins B2 and B3 with low aluminum and phosphorus contents are used to reduce costs, the intrinsic viscosity retention rate is high. Coloring of the roller end surface after re-filming is not a problem in the examples.
[0209] Examples 12 to 15 in Table 3 are examples using the polyester resin A1 recovered from the intermediate layer. The coloring of the roller end surface after re-filming was not a problem in the examples. Examples 16 and 17 in Table 4 are examples using polyester resins recovered from the film production process. Among these, coloration of the roller end surface after re-filming did not cause a problem in the examples.
[0210] Embodiment 18 Polyester resin (A1), polyester resin (B1), polyester resin (D2), and polyester resin (D3) were supplied to a single-screw extruder at a mixing ratio (parts by mass) of 50:40:5:5, and a twin-screw stretched PET film was obtained in the same manner. It should be noted that the close contact with the casting drum was performed by an electrostatic close contact method using a wire electrode. Even if the casting speed is increased, the close contact with the roller can still be cast stably without entraining air. The intrinsic viscosity retention rate was 94% after the first re-kneading and 84% after the third re-kneading, and no difference in color tone was observed at the end surface of the film using the re-melted resin.
[0211] The cast sheet of the polyester resin composition constituting the film of Example 18 was crushed, and the amounts of each element were measured by the same method as that for the polyester resin (D3). The results showed that the amount of antimony element was 105 mass ppm, the amount of aluminum element was 10 mass ppm, the amount of magnesium element was 50 mass ppm, the amount of potassium element was 5 mass ppm, and the amount of phosphorus element was 53 mass ppm.
[0212] The melting resistance of the polyester resin composition constituting the film of Example 18 measured by the following method was 0.22×10 8 Ω·cm. Determination method of melting resistance Two electrodes (stainless steel needles with a diameter of 0.6 mm) were placed on both ends of the polyester composition melted at 275°C, and sandwiched between two quartz plates with a width of 2 cm to form a uniform layer of the molten polyester composition with a width of 2 cm and a thickness of 0.6 mm. The current (io) was measured when a DC voltage of 120 V was applied, and the current was substituted into the following formula to determine the melting resistance value ρi (Ω·cm). ρi(Ω·cm)=(A / L)×(V / io) [A: electrode area (cm 2 )、L:distance between electrodes (cm), V:voltage (V)] A(cm 2 )=[width of molten polyester composition layer]×[thickness]=2(cm)×0.06(cm), V=120(V). L is measured without including the electrode diameter.
Industrial Applicability
[0213] By mixing a polyester resin (B) containing an aluminum compound and a phosphorus compound with a recycled polyester resin (A) to produce a polyester film, the coloration of the polyester film and the decrease in molecular weight can be suppressed, and a polyester film with excellent recyclability can be obtained. The present invention can contribute to solving various problems such as suppressing the depletion of resources, reducing marine garbage, and suppressing global warming.
Claims
1. A method for producing a polyester film, It is characterized in that include: A step of mixing the recovered polyester resin A with the polyester resin B containing an aluminum compound and a phosphorus compound, The polyester resin A satisfies the following (1) to (3), (1) the polyester resin A contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin A is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin A is 0.5 to 0.8 dl / g.
2. The method for producing a polyester film according to claim 1, It is characterized in that The polyester resin B satisfies the following (4) and (5), (4) The content of aluminum in the polyester resin B is 5 to 50 ppm by mass, (5) The phosphorus content in the polyester resin B is 5 to 1000 ppm by mass.
3. The method for producing a polyester film according to claim 1 or 2, wherein include: A step of melt-mixing the polyester resin A and the polyester resin B to obtain a polyester resin composition C.
4. The method for producing a polyester film according to any one of claims 1 to 3, wherein include: A step of further mixing polyester resin D.
5. A method for producing a polyester film, It is characterized in that The method comprises the steps of mixing a polyester resin composition C with a polyester resin D, wherein the polyester resin composition C is a molten mixture of a recycled polyester resin A and a polyester resin B containing an aluminum compound and a phosphorus compound, The polyester resin A satisfies the following (1) to (3), (1) the polyester resin A contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin A is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin A is 0.5 to 0.8 dl / g.
6. The method for producing a polyester film according to any one of claims 1 to 5, in, The intrinsic viscosity retention rate of the polyester resin composition C is 89% or more.
7. The method for producing a polyester film according to any one of claims 1 to 6, in, The intrinsic viscosity retention rate of the polyester resin A is 92% or less.
8. The method for producing a polyester film according to any one of claims 1 to 7, in, The intrinsic viscosity retention rate of the polyester resin B is 93% or more.
9. The method for producing a polyester film according to any one of claims 1 to 8, in, The intrinsic viscosity retention rate of the polyester resin E constituting the polyester film is 89% or more.
10. The method for producing a polyester film according to any one of claims 1 to 9, in, The polyester resin A is contained in an amount of 5 to 95 parts by mass relative to 100 parts by mass of the total of the polyester resin A and the polyester resin B.
11. The method for producing a polyester film according to any one of claims 1 to 10, in, The polyester resin D is contained in an amount of 5 to 95 parts by mass based on 100 parts by mass of the total of the polyester resin A, the polyester resin B, and the polyester resin D.
12. The method for producing a polyester film according to any one of claims 1 to 11, in, The polyester film is a multilayer polyester film composed of at least two layers, and at least one surface thereof is a layer not containing the polyester resin A.
13. The method for producing a polyester film according to any one of claims 1 to 12, in, The phosphorus compound has a phosphorus element and a phenol structure in the same molecule.
14. The method for producing a polyester film according to any one of claims 1 to 13, in, The polyester resin A contains at least antimony element and germanium element.
15. The method for producing a polyester film according to any one of claims 1 to 14, in, The polyester resin A contains at least isophthalic acid as a copolymerization component.
16. The method for producing a polyester film according to claim 4, in, The polyester resin D contains a melt resistivity adjuster.
17. A polyester film, It is characterized in that The polyester film is composed of a resin E, wherein the resin E comprises a recycled polyester resin A and a polyester resin B containing an aluminum compound and a phosphorus compound. The polyester resin A satisfies the following (1) to (3), (1) the polyester resin A contains at least one element selected from antimony, titanium and germanium, (2) the total content of antimony, titanium and germanium in the polyester resin A is 2 to 500 ppm by mass, (3) The intrinsic viscosity of the polyester resin A is 0.5 to 0.8 dl / g.
18. The polyester film according to claim 17, It is characterized in that The polyester resin B satisfies the following (4) and (5), (4) The content of aluminum in the polyester resin B is 5 to 50 ppm by mass, (5) The phosphorus content in the polyester resin B is 5 to 1000 ppm by mass.
19. The polyester film according to claim 17 or 18, in, The polyester resin E further includes a polyester resin D.
20. The polyester film according to any one of claims 17 to 19, in, The intrinsic viscosity retention rate of the polyester resin E is 89% or more.
21. A polyester film, It is characterized in that The polyester resin constituting the film contains at least antimony element, germanium element and aluminum element.
22. The polyester film according to claim 21, in, The polyester resin constituting the film contains isophthalic acid as a copolymer component.