Granulating device, method for producing granulated and sintered raw material, and method for producing sintered ore

By setting a nozzle in the granulation device to tilt out steam, the sintered raw materials are efficiently heated, which solves the problem of low steam use efficiency, improves the productivity of sintered ore and reduces manufacturing costs.

CN118946674APending Publication Date: 2024-11-12JFE STEEL CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380033553.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when steam is blown into the sintered raw material and heated granulation, additional steam is required, which leads to an increase in the manufacturing cost of sintered ore and low steam utilization efficiency.

Method used

A granulation device is designed, using a cylindrical drum and steam pipe to spray steam to the accumulation surface of the sintered raw materials through multiple nozzles. The steam spraying direction of the nozzle is set inclined to ensure that the steam heats the sintered raw materials efficiently and reduces steam consumption.

Benefits of technology

The heating efficiency of the sintered raw materials is improved, the aerability of the loading layer is enhanced, the productivity of the sintered ore is improved, and the increase in manufacturing costs is suppressed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946674A_ABST
    Figure CN118946674A_ABST
Patent Text Reader

Abstract

Provided are: a granulation device capable of efficiently heating a sintering raw material by blowing steam into the sintering raw material; a method for producing a granulated sintering raw material; and a method for producing a sintered ore using the method for producing a granulated sintering raw material. A granulation device for granulating a sintering raw material including an iron-containing raw material, a CaO-containing raw material, and a coagulation material, the granulation device comprising: a cylindrical drum which is provided with an input port through which the sintering raw material is input and a discharge port through which the granulated sintering raw material is discharged, and which rotates about a horizontal axis of rotation; the steam piping is only arranged at the front half part between the input port and the middle position between the input port and the discharge port in the drum; and a plurality of nozzles that are connected to the steam piping and that eject steam toward the surface on which the sintering raw material is deposited, the plurality of nozzles being provided at a distance of 500 mm or more from the surface on which the sintering raw material is deposited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a granulating device for granulating a sintering raw material, a method for producing the granulated sintering raw material, and a method for producing a sintered ore. Background Art

[0002] Sintered ore, which is a raw material for blast furnaces, is generally made of iron-containing raw materials such as iron ore powder, recycled powder in ironmaking plants, and underscreen powder of sintered ore, CaO-containing raw materials such as limestone and dolomite, and carbon materials (solid fuels) such as coke powder and anthracite, and is manufactured using a Dwight-Lloyd sintering machine (hereinafter sometimes referred to as a "sintering machine") which is an endlessly movable sintering machine. The sintered raw materials are loaded onto the endlessly movable tray of the sintering machine to form a loading layer. The thickness (height) of the loading layer is about 400 to 800 mm. Afterwards, the carbon material on the surface of the loading layer is ignited by an ignition furnace arranged above the loading layer. The air is sucked downward through a wind box arranged under the tray, so that the carbon material in the loading layer is burned in sequence. The combustion gradually progresses to the lower layer and the front as the tray moves. Through the combustion heat generated at this time, the sintered raw materials burn and melt to form sintered cakes. After that, the obtained sintered cake is crushed in the ore discharging section, cooled in a cooler, and sized into finished sintered ore.

[0003] In the manufacture of sintered ore using the above-mentioned sintering machine, the following technology is known: by preheating and drying the sintering raw material, the proportion of the wet zone of the charging layer is reduced, and the air permeability of the charging layer is improved, thereby improving the productivity of the sintered ore. For example, Patent Document 1 discloses a method for manufacturing granulated sintered raw material in which steam such as water vapor is blown into the granulation of the sintering raw material to heat the sintering raw material. According to Patent Document 1, it is believed that by granulating the sintering raw material while blowing water vapor, the sintering raw material is preheated and dried, the air permeability of the charging layer is improved, and the productivity of the sintered ore can be improved.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2019 / 167888 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In the method disclosed in Patent Document 1, since the sintering raw material is granulated while blowing steam, it is necessary to prepare steam to be blown into the sintering raw material separately. Therefore, there is a problem that the manufacturing cost of the sintered ore increases due to the cost required to prepare the steam. On the other hand, if the sintering raw material can be efficiently heated using steam, the amount of steam used can be reduced, and the increase in the manufacturing cost of the sintered ore can be suppressed. The present invention is completed in view of such problems of the prior art, and its purpose is to provide a granulating device that can blow steam into the sintering raw material to efficiently heat the sintering raw material, a method for manufacturing granulated sintered raw material, and a method for manufacturing sintered ore using the method for manufacturing granulated sintered raw material.

[0009] Means for solving problems

[0010] Means for solving the above-mentioned problems are as follows.

[0011] [1] A granulation device for granulating a sintering raw material including an iron-containing raw material, a CaO-containing raw material and a coagulating material, wherein the device comprises: a cylindrical drum having an inlet for feeding the sintering raw material and an outlet for discharging the granulated sintering raw material, and rotating with a horizontal direction as a rotation axis; a steam pipe provided only in the front half of the drum from the inlet to a middle position between the inlet and the outlet; and a plurality of nozzles connected to the steam pipe for spraying steam toward the accumulation surface of the sintering raw material, wherein the plurality of nozzles are provided at a distance of more than 500 mm from the accumulation surface of the sintering raw material.

[0012] [2] According to the granulation device described in [1], the steam ejection direction of more than half of the multiple nozzles is inclined toward the exhaust port side, and the steam ejection direction of the remaining nozzles is arranged in a manner to eject steam perpendicularly relative to the stacking surface of the sintering raw material.

[0013] [3] According to the granulation device described in [1] or [2], the steam ejection direction of the plurality of nozzles is arranged to be more inclined toward the discharge port as the positions of the nozzles approach the discharge port.

[0014] [4] A method for producing a granulated sintering raw material, comprising using a granulating device to granulate a sintering raw material comprising an iron-containing raw material, a CaO-containing raw material and a coagulating material, wherein the granulating device has a cylindrical drum, the drum being provided with an inlet for feeding the sintering raw material and an outlet for discharging the granulated sintering raw material, and the drum being rotated with a horizontal direction as a rotation axis, and steam is blown into the sintering raw material from a position more than 500 mm away from the accumulation surface of the sintering raw material in the front half of the drum from the inlet to the middle position between the inlet and the outlet, so that the sintering raw material has a temperature more than 10° C. higher than that of the granulated sintering raw material after granulation without blowing the steam.

[0015] [5] The method for producing a granulated sintering raw material according to [4], wherein more than half of the total amount of steam blown into the sintering raw material is blown in an inclined direction toward the discharge port.

[0016] [6] A method for producing a sintered ore, comprising: sintering a granulated sintered raw material granulated by the method for producing a granulated sintered raw material according to [4] or [5] using a sintering machine to produce a sintered ore.

[0017] Effects of the Invention

[0018] By using the granulation device according to the present invention, steam can be blown into the sintering raw material to heat it efficiently, so the steam consumption rate of the steam used in granulation can be reduced. By using the heated granulated sintering raw material, the air permeability of the charging layer is improved and the productivity of the sintered ore is improved. Therefore, by using the granulation device according to the present invention, the productivity of the sintered ore can be improved and the increase in the manufacturing cost of the sintered ore can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram showing an example of the sintered ore production facility 10 including a drum mixer 32 as a granulation device according to the present embodiment.

[0020] Figure 2 This is a graph showing the relationship between the temperature of the sintering raw material at the outlet side of the drum mixer and the air permeability index JPU of the charge layer.

[0021] Figure 3 This is a graph showing the relationship between the temperature of the sintering raw material at the outlet side of the drum mixer and the air permeability index JPU of the charge layer.

[0022] Figure 4 It is a schematic diagram explaining the structure of a drum mixer.

[0023] Figure 5 is a cross-sectional view of a drum mixer showing the locations of multiple nozzles.

[0024] Figure 6 It is a graph showing the results of the steam blowing experiment.

[0025] Figure 7 It is a schematic diagram showing the steam piping.

[0026] Figure 8 It is a graph showing the results of the steam blowing experiment. DETAILED DESCRIPTION

[0027] Hereinafter, the present invention will be described by way of embodiments of the invention. Figure 1 1 is a schematic diagram showing an example of a sintered ore manufacturing facility 10 having a drum mixer 32 as a granulation device according to the present embodiment. The iron-containing raw material 12 stored in the site 11 is transported to the blending tank 22 by the conveyor 14. The iron-containing raw material 12 includes various types of iron ore and dust generated in the ironworks.

[0028] The raw material supply unit 20 is provided with a plurality of mixing tanks 22, 24, 25, 26, and 28. The iron-containing raw material 12 is stored in the mixing tank 22. The CaO-containing raw material 16 including limestone, quicklime, etc. is stored in the mixing tank 24, and the MgO-containing raw material 17 including dolomite, refined nickel slag, etc. is stored in the mixing tank 25. The coagulation material 18 including coke powder and anthracite crushed to a particle size of 1 mm or less using a rod mill is stored in the mixing tank 26. The return ore (sintered ore underscreen powder) with a particle size of 5 mm or less that has become a sintered ore is stored in the mixing tank 28. A predetermined amount of each raw material is taken out from the mixing tanks 22 to 28 of the raw material supply unit 20, and they are mixed to become a sintered raw material. The sintered raw material is transported to the drum mixer 32 by the conveyor 30. The MgO-containing raw material 17 is an arbitrary mixed raw material, which may be mixed with the sintered raw material or not.

[0029] The drum mixer 32 is a granulating device that granulates while blowing steam to the sintering raw material. The drum mixer 32 includes a cylindrical drum 33 that rotates with the horizontal direction as the rotation axis, a steam pipe 36, and a plurality of nozzles 37 connected to the steam pipe 36 and spraying water vapor 38 to the accumulation surface of the sintering raw material. It should be noted that water vapor is an example of steam.

[0030] The cylindrical drum 33 is provided with an inlet 34 provided at one end face side of the drum 33 and into which the sintering raw material is introduced, and an outlet 35 provided at the other end face side of the drum 33 and from which the granulated sintering raw material (hereinafter referred to as quasi-particles) after granulation is discharged. The steam pipe 36 is provided in the drum 33, which is the front half of the area from the inlet 34 to the middle position between the inlet 34 and the outlet 35. A plurality of nozzles 37 are provided at a position which is 500 mm or more in the vertical direction from the accumulation surface of the sintering raw material, and water vapor is blown toward the accumulation surface of the sintering raw material from this position.

[0031] In this way, quasiparticles are produced by granulating the sintering raw material while blowing water vapor, so that quasiparticles are granulated into quasiparticles with an average particle size of about 3.0 mm at a temperature 10°C higher than that of the quasiparticles granulated without blowing water vapor. The quasiparticles are transported to the sintering machine 40 by the conveyor 39. In the present embodiment, the average particle size of the quasiparticles is the arithmetic average particle size, which is defined by Σ(Vi×di) (where Vi is the existence ratio of particles in the i-th particle size range, and di is the representative particle size of the i-th particle size range). In addition, the drum mixer 32 is an example of a granulating device for granulating the sintering raw material.

[0032] The sintering machine 40 is, for example, a Dwight-Lloyd type sintering machine of the downward suction type. The sintering machine 40 includes a sintering raw material supply device 42, an endlessly movable tray trolley 44, an ignition furnace 46, and a wind box 48. The sintering raw material is loaded into the tray trolley 44 from the sintering raw material supply device 42 to form a loading layer of the sintering raw material. The loading layer is ignited by the ignition furnace 46. Air is sucked through the wind box 48, thereby causing the condensed material 18 to burn in the loading layer while causing the combustion and melting zone in the loading layer to move downwardly in the loading layer. Thus, the loading layer is sintered to form a sintered cake. In this embodiment, a gas fuel supply device 47 may also be provided. The gas fuel supplied from the gas fuel supply device 47 is any combustible gas selected from blast furnace gas, coke oven gas, blast furnace and coke oven mixed gas, converter gas, city gas, natural gas, methane gas, ethane gas, propane gas, shale gas, and mixed gases thereof.

[0033] The sintered cake is crushed by the crusher 50 to become a sintered ore. The sintered ore crushed by the crusher 50 is cooled by the cooler 52. The sintered ore cooled by the cooler 52 is screened by a screening device 54 having a plurality of sieves, and is screened into a finished sintered ore 56 with a particle size exceeding 5 mm and a return ore 58 with a particle size of 5 mm or less. The finished sintered ore 56 is used as a blast furnace raw material. On the other hand, the return ore 58 is transported to the matching trough 28 of the raw material supply unit 20 by the conveyor 60. In this embodiment, the particle size of the finished sintered ore 56 and the particle size of the return ore 58 mean the particle size screened by the sieve, for example, the particle size exceeding 5 mm is screened into the particle size on the sieve using a sieve with a mesh of 5 mm, and the particle size below 5 mm is screened into the particle size under the sieve using a sieve with a mesh of 5 mm. The values ​​of the particle sizes of the finished sintered ore 56 and the return ore 58 are just examples and are not limited to the values.

[0034] Thus, in the production of sintered ore using the sintered ore production facility 10, steam is blown into the sintered raw material to granulate and heat the sintered raw material by the drum mixer 32. This improves the air permeability of the sintered raw material charging layer and improves the productivity of the sintered raw material. Figure 2It is a graph showing the relationship between the temperature of the quasiparticles at the exit of the drum mixer and the air permeability index JPU of the charging layer. Figure 2 The horizontal axis of is the temperature (° C.) of the quasiparticles discharged from the drum mixer 32 . The temperature of the quasiparticles is the average temperature of the quasiparticles discharged from the drum mixer 32 .

[0035] The temperature of the sintering raw material before being put into the drum mixer 32 is 35.0°C. The sintering raw material includes a CaO-containing raw material. Since CaO generates heat when reacting with water to generate Ca(OH)2, the temperature of the sintering raw material rises from 35.0°C to about 42.5°C even without blowing in water vapor. Figure 2 The plotted point with the horizontal axis at 42.5° C. is a granulation example in which the sintering raw material was granulated without blowing water vapor into the sintering raw material, and the other plotted points are granulation examples in which water vapor was blown into the sintering raw material to granulate and the sintering raw material was heated.

[0036] Figure 2 The vertical axis of is the air permeability index JPU of the loading layer. JPU is an air permeability index measured by sucking air downwards into the loading layer formed by loading the quasiparticles into the tray in a cold state. The air permeability index JPU is calculated using the following formula (1).

[0037] JPU=V / [S×(ΔP / h) 0.6 ]···(1)

[0038] In the above formula (1), V is the air volume (m 3 / min), S is the effective area of ​​the sintering machine (m 2 ), h is the loading layer height (mm), ΔP is the pressure loss (mmH2O).

[0039] If the air permeability of the packing layer is high, the air permeability index JPU becomes larger, and if the air permeability is low, the air permeability index JPU becomes smaller. Figure 2 As shown, by blowing water vapor into the sintered raw material to raise the temperature of the quasiparticles to more than 42.5°C, the air permeability of the loading layer is improved. In addition, the air permeability of the loading layer formed by the quasiparticles of 56.0°C, whose temperature is raised by more than 10°C from 42.5°C, is significantly higher than that of the loading layer formed by the quasiparticles of 47.0°C. From this result, it can be seen that it is preferred to blow water vapor into the sintered raw material to granulate, so that the quasiparticles have a temperature more than 10°C higher than that of the quasiparticles after granulation without blowing water vapor, thereby forming quasiparticles that form a highly air-permeable loading layer.

[0040] Figure 3 This is a graph showing the relationship between the temperature of quasi-particles at the outlet of a drum mixer and the productivity of sintered ore. Figure 3 The horizontal axis of is the temperature (° C.) of the quasiparticles discharged from the drum mixer 32 . Figure 3 The vertical axis is the productivity of sintered ore (t / (hr×m 2 )).like Figure 3 As shown in FIG. 1 , the productivity of sintered ore when sintered ore is produced using quasiparticles at 56.0°C, which is 10°C higher than 43.5°C, is significantly higher than the productivity of sintered ore when sintered ore is produced using quasiparticles at 47.0°C. Figure 2 The results show that by blowing water vapor into the sintering raw material to perform granulation, quasiparticles having a temperature 10°C or higher than that of quasiparticles after granulation without blowing water vapor are formed, and the quasiparticles are used to produce sintered ore, which can achieve an improvement in the productivity of the sintered ore.

[0041] Next, the structure of the drum mixer 32 that can efficiently increase the temperature of the quasi-particles discharged from the drum mixer 32 by blowing water vapor into the sintering raw material is described. Since the drum 33 rotates with the horizontal direction as the rotation axis, the stacking position of the sintering raw material in the drum 33 is inclined relative to the vertically downward direction of the rotation direction of the drum 33. A plurality of nozzles 37 are arranged at a position that is more than 500 mm away from the stacking surface of the sintering raw material in the vertical direction. In this way, by arranging a plurality of nozzles 37 at a position that is more than 500 mm away from the stacking surface of the sintering raw material in the vertical direction, the temperature of the quasi-particles can be efficiently increased. The rotation axis in the drum mixer 32 can be approximately horizontal. In addition, in order to efficiently discharge the quasi-particles, the rotation axis can also be tilted in a manner that the discharge port 35 is located below the input port 34 in the vertical direction.

[0042] Figure 4 It is a schematic diagram for explaining the structure of the drum mixer 32. Figure 4 (a) is a schematic cross-sectional view of the drum mixer 32. Figure 4 (b) is a schematic diagram of the steam pipe 36. It should be noted that Figure 4 In (b) of FIG. 1 , the plurality of nozzles 37 are shown with arrows indicating the ejection direction of the water vapor ejected from each nozzle.

[0043] like Figure 4As shown, in the drum mixer 32 involved in this embodiment, the steam pipe 36 is provided at a position from the inlet 34 of the drum 33 to the front half between the inlet 34 and the outlet 35, which is 5000 mm away from the inlet 34. In addition, 15 nozzles 37 are provided at intervals of 350 mm in the steam pipe 36. The 1st to 7th nozzles from the inlet 34 side of the plurality of nozzles 37 are provided in a manner to eject water vapor perpendicularly to the accumulation surface of the sintering raw material. The 8th to 14th nozzles from the inlet 34 side are provided in a manner to face the outlet 35 side, and are inclined at 30° to the outlet 35 side relative to the vertical line relative to the accumulation surface of the sintering raw material. The nozzle closest to the outlet 35 side is provided in a manner to be inclined at 45° to the outlet 35 side relative to the vertical line relative to the accumulation surface of the sintering raw material. That is, more than half of the plurality of nozzles 37 are inclined to eject steam toward the discharge port 35, and the remaining nozzles are disposed to eject steam perpendicularly to the deposition surface of the sintering raw material.

[0044] Figure 5 1 is a cross-sectional view of a drum mixer showing the positions of multiple nozzles. In order to confirm the effect of the nozzle installation positions, a steam pipe was installed so that the distances of the nozzles from the deposited surface of the sintering raw material 62 in the vertical direction were 100 mm, 300 mm, 500 mm, 1500 mm, and 2500 mm, respectively. Figure 4 The drum mixer shown in FIG. 1 was used to carry out a steam blowing experiment.

[0045] Figure 6 It is a graph showing the results of the steam blowing experiment. Figure 6 The horizontal axis is the position in the drum mixer (m), and the vertical axis is the temperature of the sintering raw material (℃). Figure 6 In the figure, the temperature of the sintering raw material is the average temperature of the sintering raw material at each position in the drum mixer shown on the horizontal axis. Regarding the conditions of this experiment (steam blowing experiment), in all experimental examples (1 to 5), the steam blowing amount was 7.5 t / h, the steam temperature was 170°C (steam piping pressure: 0.7 MPa), and the raw material (sintering raw material) input amount was 730 t / h.

[0046] like Figure 6As shown, in the drum mixers of Experimental Examples 1 and 2, where the vertical distance from the stacking surface of the sintering raw material is less than 500 mm, the temperature near the inlet becomes high, but the temperature gradually decreases thereafter, and the temperature of the quasiparticles discharged from these drum mixers is low. On the other hand, in the drum mixers of Experimental Examples 3, 4, and 5, where the vertical distance from the stacking surface of the sintering raw material is more than 500 mm, the temperature near the inlet is low, but the subsequent temperature drop is suppressed, and the temperature of the quasiparticles discharged from these drum mixers is higher than that of Experimental Examples 1 and 2. From these results, it is confirmed that by arranging a plurality of nozzles at a position more than 500 mm away from the stacking surface of the sintering raw material in the vertical direction and blowing water vapor into the sintering raw material from the nozzles, the temperature of the quasiparticles discharged from the drum mixer is increased compared with the case where a plurality of nozzles are arranged at a position less than 500 mm away from the stacking surface of the sintering raw material in the vertical direction. Thus, in the drum mixer involved in this embodiment, since the temperature of the quasiparticles can be efficiently increased by blowing in steam, it can be known that if the amount of steam blown in is the same, the temperature of the quasiparticles discharged from the drum mixer can be further increased, and if the temperature of the quasiparticles discharged from the drum mixer is the same, the amount of steam blown in can be reduced.

[0047] On the other hand, the moisture content of the quasi-particles discharged from the drum mixer is also important. If the moisture content of the quasi-particles discharged from the drum mixer is less than the target moisture content (6.5 mass %), the granulation of the sintering raw material will not proceed, and the particle size of the quasi-particles after granulation will become smaller. If the particle size of the quasi-particles becomes smaller, the air permeability of the loading layer formed by the quasi-particles with a small particle size will deteriorate and the productivity of the sintered ore will decrease.

[0048] Figure 7 is a schematic diagram showing steam piping. Figure 7 In FIG. 1 , the plurality of nozzles are also shown with arrows indicating the ejection direction of the water vapor ejected from each nozzle. Figure 7 (a) shows the steam pipe of Experimental Example 11 in which a plurality of nozzles are provided so that the ejection direction of the ejected water vapor is vertically downward. Figure 7 (b) is the steam piping of Experimental Example 12 in which the ejection direction of water vapor ejected from the 1st to 7th nozzles from the inlet side among the multiple nozzles is arranged to be vertically downward, the ejection direction of water vapor ejected from the 8th to 14th nozzles from the inlet side is arranged to be inclined 30° toward the discharge outlet side relative to the vertical downward, and the ejection direction of water vapor ejected from the nozzle closest to the discharge outlet side is arranged to be inclined 45° toward the discharge outlet side relative to the vertical downward. Figure 7(c) is a steam pipe of Experimental Example 13 in which the ejection direction of water vapor ejected from the 1st to 7th nozzles from the input port side among the plurality of nozzles is set to be inclined 30° toward the discharge port side relative to vertical downward, the ejection direction of water vapor ejected from the 8th to 14th nozzles from the input port side is set to be inclined 45° toward the discharge port side relative to vertical downward, and the ejection direction of water vapor ejected from the nozzle closest to the discharge port side is set to be inclined 60° toward the discharge port side relative to vertical downward. A water vapor blowing experiment was conducted using a drum mixer in which these steam pipes were set so that water vapor was blown from a position 1500 mm away in the vertical direction from the stacking surface of the sintering raw material.

[0049] Figure 8 It is a graph showing the results of the steam blowing experiment. Figure 8 The horizontal axis represents the position (m) in the drum mixer, and the vertical axis represents the moisture content (mass %) of the sintering raw material, which shows the average moisture content of the sintering raw material at each position in the drum mixer shown on the horizontal axis.

[0050] like Figure 8 As shown, the moisture content of the quasi-particles after granulation by the drum mixer provided with the steam pipe of Experimental Examples 12 and 13 is greater than the moisture content of the quasi-particles after granulation by the drum mixer provided with the steam pipe of Experimental Example 11. From these results, it can be seen that: preferably, as the position of the nozzle approaches the discharge port, the ejection direction of the ejected water vapor is set more inclined toward the discharge port side. In addition, since the moisture content of the quasi-particles in Experimental Example 13 is greater than that in Experimental Example 12, it can be seen that: preferably, the steam ejection direction of more than half of the nozzles among the multiple nozzles is set inclined toward the discharge port, and more preferably, all of the multiple nozzles are set inclined so that the steam ejection direction of the nozzle is toward the discharge port side. It should be noted that since the steam blowing amount from each nozzle is the same, it can be said that: preferably, the ejection direction of more than half of the total water vapor blowing amount is inclined toward the discharge port side to blow the water vapor into the sintering raw material, and more preferably, the ejection direction of all the water vapor is inclined toward the discharge port side to blow the water vapor into the sintering raw material.

[0051] As described above, the drum mixer 32 as the granulation device involved in the present embodiment can blow steam into the sintering raw material to heat it efficiently. Therefore, if the amount of steam used is the same, the quasi-particles can be heated to a higher temperature, and if the temperature of the outlet side is the same, the quasi-particles can be heated with less steam. In this way, by using the granulation device involved in the present embodiment, the sintering raw material can be heated to a specified temperature while reducing the amount of steam used in the production of sintered ore, thereby achieving an improvement in the productivity of the sintered ore and a suppression of the increase in the production cost of the sintered ore.

[0052] Description of Reference Numerals

[0053] 10 Sintered ore manufacturing equipment

[0054] 11 Venues

[0055] 12 Iron-containing raw materials

[0056] 14 Conveyor

[0057] 16 Raw materials containing CaO

[0058] 17 Raw materials containing MgO

[0059] 18 Condensation material

[0060] 20 Raw material supply department

[0061] 22 Mating groove

[0062] 24 Matching groove

[0063] 26 Matching groove

[0064] 28 Mating groove

[0065] 30 Conveyor

[0066] 32 Drum Mixer

[0067] 33 Roller

[0068] 34 Input port

[0069] 35 Exhaust

[0070] 36 Steam piping

[0071] 37 Nozzle

[0072] 38 Water vapor

[0073] 39 Conveyor

[0074] 40 Sintering Machine

[0075] 42 Sintering raw material supply device

[0076] 44 Pallet Trolley

[0077] 46 Ignition furnace

[0078] 48 Bellows

[0079] 50 Crusher

[0080] 52 Cooling machine

[0081] 54 Screening device

[0082] 56 Finished sintered ore

[0083] 58 Return to Mine

[0084] 60 Conveyor

[0085] 62 Sintering raw materials.

Claims

1. A granulation device for granulating a sintered raw material comprising an iron-containing raw material, a CaO-containing raw material and a condensing material, wherein: have: The cylindrical drum is provided with an inlet for the sintering raw material to be put in and an outlet for the granulated sintering raw material to be discharged, and rotates with the horizontal direction as the rotation axis; The steam pipe is provided only in the front half of the drum from the inlet to the middle position between the inlet and the outlet; and A plurality of nozzles are connected to the steam pipe to spray steam toward the accumulation surface of the sintering raw material. The plurality of nozzles are provided at a distance of 500 mm or more from the deposition surface of the sintering raw material.

2. The granulation device according to claim 1, More than half of the plurality of nozzles are inclined to eject steam toward the discharge port, and the remaining nozzles are disposed to eject steam perpendicularly to the deposition surface of the sintering raw material.

3. The granulation device according to claim 1 or 2, The steam ejection directions of the plurality of nozzles are arranged to be more inclined toward the discharge port as the positions of the nozzles are closer to the discharge port.

4. A method for producing a granulated sintering raw material, comprising granulating a sintering raw material comprising an iron-containing raw material, a CaO-containing raw material and a coagulating material using a granulating device, wherein: The granulation device has a cylindrical drum, which is provided with an inlet for the sintering raw material to be put in and an outlet for the granulated sintering raw material to be discharged, and rotates with the horizontal direction as the rotation axis. Steam is blown into the sintered raw material from a position more than 500 mm away from the accumulation surface of the sintered raw material in the front half of the drum from the inlet to the middle position between the inlet and the outlet, thereby forming a granulated sintered raw material with a temperature more than 10° C. higher than that of the granulated sintered raw material after granulation without blowing the steam.

5. The method for producing a granulated sintering raw material according to claim 4, More than half of the total amount of steam blown into the sintering raw material is blown in an inclined manner so as to be ejected in a direction toward the discharge port.

6. A method for producing sintered ore, The granulated sintered raw material granulated by the method for producing a granulated sintered raw material according to claim 4 or 5 is sintered in a sintering machine to produce a sintered ore.

Citation Information

Patent Citations

  • Method for manufacturing granular sintered raw material

    WO2019167888A1