Granulating device, method for producing granulated and sintered raw material, and method for producing sintered ore
By blowing steam into the rear half of the drum and adding moisture in moderation, the problem of drop in the temperature of the sintered raw materials and the difficulty of heat transfer is solved, the productivity and aeration of the sintered ore are improved, the manufacturing cost is reduced, and high-efficiency granulation and high-quality granulation are achieved. Production of mass sintered ore.
Patent Information
- Application Number
- CN202380033573.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-14
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the temperature drops and heat transfer difficulty in sintering raw materials during granulation, resulting in limited increase in sintering ore productivity and manufacturing costs.
Design a granulation device to blow steam into the sintered raw material in the rear half of the drum, combine the steam pipe and nozzle to achieve efficient heating of the granulated sintered raw material, and add appropriate amount of moisture after granulation to maintain temperature and particle diameter .
The productivity of the sintered ore and the aerability of the loading layer are improved, manufacturing costs are reduced, the high temperature and suitable particle size of the granulated sintered raw materials are ensured, and the quality and efficiency of the sintered ore are improved.
Smart Images

Figure CN118946675A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a granulating device for granulating a sintering raw material, a method for producing the granulated sintering raw material, and a method for producing a sintered ore. Background Art
[0002] Sintered ore, which is a raw material for blast furnaces, is generally made of iron-containing raw materials such as iron ore powder, recycled powder in ironmaking plants, and sintered ore underscreen powder, CaO-containing raw materials such as limestone and dolomite, and carbon materials (solid fuels) such as coke powder and anthracite. It is manufactured using a Dwight-Lloyd sintering machine (hereinafter sometimes referred to as a "sintering machine") which is an endlessly movable sintering machine. The sintered raw materials are loaded onto the endlessly movable tray of the sintering machine to form a loading layer. The thickness (height) of the loading layer is about 400 to 800 mm. After that, the carbon material on the surface of the loading layer is ignited by an ignition furnace arranged above the loading layer. The air is sucked downward through a wind box arranged under the tray, so that the carbon material in the loading layer is burned in sequence. The combustion gradually progresses to the lower layer and the front as the tray moves. Through the combustion heat generated at this time, the sintered raw materials burn and melt to form sintered cakes. After that, the obtained sintered cake is crushed in the ore discharging section, cooled in a cooler, and sized into finished sintered ore.
[0003] In the manufacture of sintered ore using the above-mentioned sintering machine, the following technology is known: by preheating and drying the sintering raw material, the proportion of the wet zone of the charging layer is reduced, and the air permeability of the charging layer is improved, thereby improving the productivity of the sintered ore. For example, Patent Document 1 discloses a method for manufacturing granulated sintered raw material in which steam such as water vapor is blown into the granulation of the sintering raw material to heat the sintering raw material. According to Patent Document 1, it is believed that by granulating the sintering raw material while blowing water vapor, the sintering raw material is preheated and dried, the air permeability of the charging layer is improved, and the productivity of the sintered ore can be improved.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2019 / 167888
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2022-39966 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Although the method disclosed in Patent Document 1 is a method of granulating the sintering raw material while blowing steam, there is no disclosure or suggestion about blowing steam into the downstream area (latter half) where the sintering raw material moves in the drum mixer. Therefore, when the method disclosed in Patent Document 1 is used, the temperature of the granulated sintering raw material will drop before being discharged from the discharge port. In addition, the method disclosed in Patent Document 2 is a method of heating the granulated raw material using a heating device. Therefore, even after passing through the heating device, it is possible that the target temperature cannot be reached due to the difficulty of heat transfer to the inside of the raw material. The present invention is completed in view of the problems of such prior arts, and its purpose is to provide a granulating device that can blow steam into the sintering raw material to efficiently heat the sintering raw material, a method for manufacturing the granulated sintering raw material, and a method for manufacturing sintered ore using the method for manufacturing the granulated sintering raw material.
[0010] Means for solving problems
[0011] Means for solving the above-mentioned problems are as follows.
[0012] [1] A granulation device for granulating a sintering raw material including an iron-containing raw material, a CaO-containing raw material and a coagulating material, wherein the device comprises: a cylindrical drum having an inlet for feeding the sintering raw material and an outlet for discharging the granulated sintering raw material, and rotating with a horizontal axis as a rotation axis; a steam pipe provided only in the drum from a middle position between the inlet and the outlet to the rear half of the outlet; and a plurality of nozzles connected to the steam pipe for spraying steam toward the accumulation surface of the sintering raw material.
[0013] [2] A method for producing a granulated sintering raw material, comprising using a granulating device to granulate a sintering raw material comprising an iron-containing raw material, a CaO-containing raw material and a coagulating material, wherein the granulating device has a cylindrical drum, the drum being provided with an inlet for feeding the sintering raw material and an outlet for discharging the granulated sintering raw material, the drum being rotated with a horizontal axis as a rotation axis, and steam is blown into the sintering raw material only in a portion of the drum from a middle position between the inlet and the outlet to the latter half of the outlet to form the granulated sintering raw material.
[0014] [3] The method for producing a granulated sintering raw material according to [2], wherein when the temperature of the granulated sintering raw material discharged from the granulating device reaches 60° C. or higher, 0.5 mass % or higher and 4.5 mass % or lower of water is further added to the sintering raw material.
[0015] [4] A method for producing a sintered ore, comprising sintering a granulated sintered raw material granulated by the method for producing a granulated sintered raw material according to [2] or [3] using a sintering machine to produce a sintered ore.
[0016] Effects of the Invention
[0017] By using the granulation device according to the present invention, steam can be blown into the sintering raw material to heat it efficiently, so the amount of steam used in granulation can be reduced. By using the heated granulated sintering raw material, the air permeability of the charging layer is improved, and the productivity of the sintered ore is improved. Therefore, by using the granulation device according to the present invention, the productivity of the sintered ore can be improved and the increase in the manufacturing cost of the sintered ore can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram showing an example of the sintered ore production facility 10 including a drum mixer 32 as a granulation device according to the present embodiment.
[0019] Figure 2 This is a graph showing the relationship between the temperature increase of quasi-particles when loading the sintering machine into a tray and the increase rate of the productivity of the sintered ore.
[0020] Figure 3 This is a graph showing the water content of the sintering raw materials in Experimental Examples 1 to 3.
[0021] Figure 4 This is a graph showing the particle size of the quasiparticles in Experimental Examples 1 to 3 and the air permeability index JPU of the encapsulation layer.
[0022] Figure 5 This is a graph showing the productivity of the sintered ore in Experimental Examples 1 to 3. DETAILED DESCRIPTION
[0023] Hereinafter, the present invention will be described by way of embodiments of the invention. Figure 1 1 is a schematic diagram showing an example of a sintered ore manufacturing facility 10 having a drum mixer 32 as a granulation device according to the present embodiment. The iron-containing raw material 12 stored in the site 11 is transported to the blending tank 22 by the conveyor 14. The iron-containing raw material 12 includes various types of iron ore and dust generated in the ironworks.
[0024] The raw material supply unit 20 is provided with a plurality of mixing tanks 22, 24, 25, 26, and 28. The iron-containing raw material 12 is stored in the mixing tank 22. The CaO-containing raw material 16 including limestone, quicklime, etc. is stored in the mixing tank 24, and the MgO-containing raw material 17 including dolomite, refined nickel slag, etc. is stored in the mixing tank 25. The coagulation material 18 including coke powder and anthracite crushed to a particle size of 1 mm or less using a rod mill is stored in the mixing tank 26. The return ore (sintered ore underscreen powder) with a particle size of 5 mm or less that has become a sintered ore is stored in the mixing tank 28. A predetermined amount of each raw material is taken out from the mixing tanks 22 to 28 of the raw material supply unit 20, and they are mixed to become a sintered raw material. The sintered raw material is transported to the drum mixer 32 by the conveyor 30. The MgO-containing raw material 17 is an arbitrary mixed raw material, which may be mixed with the sintered raw material or not.
[0025] The drum mixer 32 is a granulating device that granulates while blowing steam to the sintering raw material. The drum mixer 32 has a cylindrical drum 33 that rotates with the horizontal direction as the rotation axis, a steam pipe 36, and a plurality of nozzles 37 connected to the steam pipe 36 and spraying water vapor 38 to the accumulation surface of the sintering raw material. It should be noted that water vapor is an example of steam. The rotation axis in the drum mixer 32 can be roughly horizontal. In addition, in order to efficiently discharge the quasi-particles, the rotation axis can also be tilted in a manner that the discharge port 35 is located below the input port 34 in the vertical direction.
[0026] The cylindrical drum 33 is provided with an inlet 34 provided at one end face side of the drum 33 for feeding the sintering raw material, and an outlet provided at the other end face side of the drum 33 for discharging the granulated sintering raw material (hereinafter referred to as quasi-particles) after granulation. The steam pipe 36 is provided only in the drum 33, which is the area from the middle position between the inlet 34 and the outlet 35 to the latter half of the outlet 35, and water vapor is blown toward the accumulation surface of the sintering raw material through a plurality of nozzles 37 from this position.
[0027] In this way, by blowing water vapor into the sintering raw material in the rear half of the drum 33 while granulating the sintering raw material, quasi-particles having an average particle size of about 3.0 mm at a higher temperature than the sintering raw material granulated without blowing water vapor are produced. The quasi-particles are transported to the sintering machine 40 by the conveyor 39. In the present embodiment, the average particle size of the quasi-particles is the arithmetic average particle size, which is defined by Σ(Vi×di) (where Vi is the existence ratio of particles in the i-th particle size range, and di is the representative particle size of the i-th particle size range). In addition, the drum mixer 32 is an example of a granulating device for granulating the sintering raw material.
[0028] The sintering machine 40 is, for example, a Dwight-Lloyd type sintering machine of the downward suction type. The sintering machine 40 includes a sintering raw material supply device 42, an endlessly movable tray trolley 44, an ignition furnace 46, and a wind box 48. The sintering raw material is loaded into the tray trolley 44 from the sintering raw material supply device 42 to form a loading layer of the sintering raw material. The loading layer is ignited by the ignition furnace 46. Air is sucked through the wind box 48, thereby causing the condensed material 18 to burn in the loading layer while causing the combustion and melting zone in the loading layer to move downwardly in the loading layer. Thus, the loading layer is sintered to form a sintered cake. In this embodiment, a gas fuel supply device 47 may also be provided. The gas fuel supplied from the gas fuel supply device 47 is any combustible gas selected from blast furnace gas, coke oven gas, blast furnace and coke oven mixed gas, converter gas, city gas, natural gas, methane gas, ethane gas, propane gas, shale gas, and mixed gases thereof.
[0029] The sintered cake is crushed by the crusher 50 to become a sintered ore. The sintered ore crushed by the crusher 50 is cooled by the cooler 52. The sintered ore cooled by the cooler 52 is screened by a screening device 54 having a plurality of sieves, and is screened into a finished sintered ore 56 with a particle size exceeding 5 mm and a return ore 58 with a particle size of 5 mm or less. The finished sintered ore 56 is used as a blast furnace raw material. On the other hand, the return ore 58 is transported to the matching trough 28 of the raw material supply unit 20 by the conveyor 60. In this embodiment, the particle size of the finished sintered ore 56 and the particle size of the return ore 58 mean the particle size screened by the sieve, for example, the particle size exceeding 5 mm is screened into the particle size on the sieve using a sieve with a mesh of 5 mm, and the particle size below 5 mm is screened into the particle size under the sieve using a sieve with a mesh of 5 mm. The values of the particle sizes of the finished sintered ore 56 and the return ore 58 are just examples and are not limited to the values.
[0030] Thus, in the production of sintered ore using the sintered ore production facility 10, granulation is performed while heating the sintered raw material by blowing steam into the sintered raw material using the drum mixer 32. This improves the air permeability of the sintered raw material charging layer and improves the productivity of the sintered raw material.
[0031] Figure 2 This is a graph showing the relationship between the temperature increase of the quasi-particles loaded into the tray car 44 of the sintering machine and the rate of increase in the productivity of the sintered ore. Figure 2The horizontal axis is the rising temperature (°C) of the quasiparticles when they are loaded into the tray trolley 44 of the sintering machine. The rising temperature is the difference between the average temperature of the quasiparticles after granulation by blowing water vapor when loading into the tray trolley 44 and the average temperature of the quasiparticles after granulation without blowing water vapor. It should be noted that the average temperature of the quasiparticles after granulation without blowing water vapor is 18.3°C, and the plotted points in the figure are examples of the average temperatures of the quasiparticles when loaded into the tray trolley 44 being 38.0°C, 35.0°C, 35.5°C, 45.0°C, and 51.0°C. In addition, Figure 2 The vertical axis represents the effect of improving the productivity of the sintered ore (%), which is a value calculated by the following formula (1).
[0032] (T2-T1)×100 / T1···(1)
[0033] In the above formula (1), T1 is the productivity (t / (hr×m 2 )), T2 is the productivity of sintered ore when sintered ore is produced using quasi-particles granulated by blowing water vapor (t / (hr×m 2 )).
[0034] like Figure 2 As shown, the productivity increase rate of the sintered ore increases as the average temperature of the quasiparticles when loaded into the tray truck 44 increases. From this result, it can be seen that the productivity of the sintered ore can be improved by blowing water vapor into the sintering raw material using the drum mixer 32 to form high-temperature quasiparticles and using the quasiparticles to produce sintered ore.
[0035] On the other hand, if the average temperature of the quasiparticles reaches 60°C or more, the water evaporates and quasiparticles of a predetermined particle size are not granulated. If the particle size of the quasiparticles decreases, the air permeability of the charge layer deteriorates, and the productivity of the sintered ore decreases significantly.
[0036] Figure 3 : is a graph showing the water content of the sintering raw materials of Experimental Examples 1 to 3. Figure 3 The bar graph shown with diagonal hatching in the figure represents the moisture content (mass %) of the sintering raw material at the inlet side of the drum mixer, and the bar graph shown with horizontal hatching represents the moisture content (mass %) of the sintering raw material when it is loaded into the sintering machine. Experimental Example 1 is an example of manufacturing quasiparticles using an average temperature of 33°C for the sintering raw material when it is loaded into the sintering machine. Experimental Example 2 is an example of manufacturing quasiparticles using an average temperature of 60°C for the sintering raw material when it is loaded into the sintering machine. Experimental Example 3 is an example of manufacturing quasiparticles using an average temperature of 62°C for the sintering raw material when it is loaded into the sintering machine.
[0037] like Figure 3As shown, it can be seen that the moisture content of the raw material can be ensured to be 6.5% by mass when it is charged into the sintering machine in Experimental Examples 1 and 3. On the other hand, in Experimental Example 2, although the moisture content of 6.5% by mass can be ensured at the inlet side of the drum mixer, the moisture content decreases to about 5.5% by mass when it is charged into the sintering machine because the water evaporates due to heating.
[0038] Figure 4 Graph showing the particle size of the quasiparticles and the air permeability index JPU of the loading layer in Experimental Examples 1 to 3. Figure 4 In the figure, the bar graph shown by the hatching of the diagonal lines represents the particle size (mm) of the quasiparticles, and the bar graph shown by the hatching of the horizontal lines represents the air permeability index JPU(-) ((-) means dimensionless). It should be noted that the particle size of the quasiparticles is the calculated average particle size mentioned above, and the air permeability index JPU of the loading layer is an index calculated using the following formula (2).
[0039] JPU=V / [S×(ΔP / h) 0.6 ]···(2)
[0040] In the above formula (1), V is the air volume (m 3 / min), S is the effective area of the sintering machine (m 2 ), h is the loading layer height (mm), ΔP is the pressure loss (mmH2O).
[0041] like Figure 4 As shown in Figure 2, in Experimental Examples 1 and 3, quasiparticles with a particle size of about 3 mm were granulated, but in Experimental Example 2, only quasiparticles with a particle size of about 1 mm were granulated. It can be considered that the decrease in the particle size of the quasiparticles in Experimental Example 2 is due to Figure 3 The decrease in the moisture content of the raw material shown in the figure is caused by the decrease in the moisture content of the raw material. In Experimental Example 3, high-temperature quasiparticles with a particle size of about 3 mm were granulated, so the air permeability index of the loading layer became about 17. In Experimental Example 1, although quasiparticles of the same particle size were granulated, the average temperature of the quasiparticles was low, so the air permeability index of the loading layer became about 15. In Experimental Example 2, although high-temperature quasiparticles were obtained, only quasiparticles with a particle size of about 1 mm were granulated, so the air permeability index of the loading layer dropped significantly to about 12.
[0042] Figure 5 Graph showing the productivity of sintered ore in Experimental Examples 1 to 3. The productivity of sintered ore is calculated for each m 2 The production volume (t) of finished sintered ore produced by the loading layer in 1 hour. Figure 5 As shown in FIG. 1 , the productivity of Experimental Example 3 is 1.39, compared with the productivity of Experimental Example 1, which is 1.29. The productivity of sintered ore is greatly increased. It can be considered that the increase in productivity of Experimental Example 3 is due to Figure 4On the other hand, in Experimental Example 2, the air permeability of the filling layer was greatly reduced, sintering did not progress, and the sintering raw material was not agglomerated.
[0043] Thus, when the average temperature of the quasi-particles discharged from the granulation device becomes 60°C or higher, the water evaporates due to the temperature, so the water required for granulation is insufficient, and the quasi-particles of the specified particle size cannot be granulated, and the air permeability of the loading layer will be deteriorated. Therefore, the amount of water evaporated when the quasi-particles discharged from the drum mixer 32 are heated in a manner such that the average temperature is 60°C or higher and lower than 80°C, and the result is that the amount of water evaporated in the range of 0.5% by mass or higher and 3.0% by mass or lower in terms of the amount of water after granulation. In addition, the amount of water evaporated when the quasi-particles discharged from the drum mixer 32 are heated in a manner such that the average temperature is 80°C or higher, and the result is that the amount of water evaporated in the range of 2.0% by mass or lower and 4.5% by mass or lower in terms of the amount of water after granulation.
[0044] According to these results, when the average temperature of the quasi-particles discharged from the granulation device is made to be above 60°C, it is preferred to further add water in the range of 0.5% by mass and 4.5% by mass to the sintering raw material in the granulation, based on the moisture content after granulation. Thus, even if the quasi-particles are heated to above 60°C, the moisture content required for granulation can be ensured, and quasi-particles with a particle size of about 3 mm heated to above 60°C can be manufactured from the sintering raw material. By using the heated quasi-particles to manufacture sintered ore, the air permeability of the loading layer is improved, thereby achieving an increase in the productivity of the sintered ore. It should be noted that, when the average temperature of the quasi-particles is made to be above 60°C and below 80°C, it is preferred to further add water in the range of 0.5% by mass and 3.0% by mass to the sintering raw material in the granulation, and when the average temperature of the quasi-particles is made to be above 80°C, it is preferred to further add water in the range of 2.0% by mass and 4.5% by mass to the moisture content after granulation.
[0045] The amount of water to be added can be determined by measuring the water content of the quasi-particles discharged from the drum mixer 32 at predetermined intervals and within the above range. Water can be added by adding factory water, hot water or condensed water to the sintering raw material during granulation.
[0046] Next, the installation position of the steam pipe 36 in the drum mixer 32 is described. Table 1 shows the results of the experiment of blowing water vapor into the sintering raw material by changing the installation position of the steam pipe 36 to the inlet side and the outlet side. It should be noted that the temperature on the outlet side in the table is the average temperature of the quasiparticles discharged from the drum mixer 32.
[0047]
[0048] Experimental Examples 11 and 12 are granulation examples in which the steam pipe 36 is provided only in the first half from the inlet 34 to the middle position between the inlet and the outlet, and water vapor is blown into the sintering raw material to perform granulation. Experimental Examples 13 to 15 are granulation examples in which the steam pipe 36 is provided only in the second half from the middle position between the inlet 34 and the outlet 35 to the outlet 35, and water vapor is blown into the sintering raw material to perform granulation.
[0049] According to the comparison between Experimental Example 11 and Experimental Example 13 and the comparison between Experimental Example 12 and Experimental Example 14, the average temperature of the outlet side of the quasiparticles after granulation by blowing water vapor when the steam pipe 36 is set in the second half is 8 to 11°C higher than the average temperature of the outlet side of the quasiparticles after granulation by blowing water vapor when the steam pipe 36 is set in the first half. In addition, according to the comparison between Experimental Example 11 and Experimental Example 15, if the temperature of the outlet side of the quasiparticles is the same, the amount of water vapor blown in the granulation can be reduced by 17% when the steam pipe 36 is set in the second half. From these results, it is confirmed that by setting the steam pipe 36 having a plurality of nozzles 37 only in the second half of the drum mixer 32 and blowing steam into the sintering raw material from the nozzle 37, the sintering raw material can be efficiently heated compared with the case where the steam pipe having a plurality of nozzles is set in other positions of the drum mixer 32.
[0050] As described above, the drum mixer 32 as the granulation device involved in this embodiment can blow steam into the sintering raw material to heat it efficiently. Therefore, if the amount of steam used is the same, the sintering raw material can be heated to a higher temperature, and if the temperature of the outlet side is the same, the sintering raw material can be heated with less steam. In this way, by using the granulation device involved in this embodiment, the sintering raw material can be heated to a specified temperature while reducing the amount of steam used in the production of sintered ore, thereby achieving the improvement of the productivity of the sintered ore and the suppression of the increase in the production cost of the sintered ore.
[0051] Description of Reference Numerals
[0052] 10 Sintered ore manufacturing equipment
[0053] 11 Venues
[0054] 12 Iron-containing raw materials
[0055] 14 Conveyor
[0056] 16 Raw materials containing CaO
[0057] 17 Raw materials containing MgO
[0058] 18 Condensation materials
[0059] 20 Raw material supply department
[0060] 22 Mating groove
[0061] 24 Mating groove
[0062] 26 Matching groove
[0063] 28 Mating groove
[0064] 30 Conveyor
[0065] 32 Drum Mixer
[0066] 33 Roller
[0067] 34 Input port
[0068] 35 Exhaust
[0069] 36 Steam piping
[0070] 37 Nozzle
[0071] 38 Water vapor
[0072] 39 Conveyor
[0073] 40 Sintering Machine
[0074] 42 Sintering raw material supply device
[0075] 44 Pallet Trolley
[0076] 46 Ignition furnace
[0077] 48 Bellows
[0078] 50 Crusher
[0079] 52 Cooling machine
[0080] 54 Screening device
[0081] 56 Finished sintered ore
[0082] 58 Return to Mine
[0083] 60 Conveyor
[0084] 62 Sintering raw materials.
Claims
1. A granulation device for granulating a sintered raw material comprising an iron-containing raw material, a CaO-containing raw material and a condensing material, wherein: have: The cylindrical drum is provided with an inlet for the sintering raw material to be put in and an outlet for the granulated sintering raw material to be discharged, and rotates with the horizontal direction as the rotation axis; The steam pipe is provided only in the drum from the middle position between the input port and the discharge port to the rear half of the discharge port; and A plurality of nozzles are connected to the steam pipe to eject steam toward the deposited surface of the sintering raw material.
2. A method for producing a granulated sintering raw material, comprising granulating a sintering raw material comprising an iron-containing raw material, a CaO-containing raw material and a coagulating material using a granulating device, wherein: The granulation device has a cylindrical drum, which is provided with an inlet for the sintering raw material to be put in and an outlet for the granulated sintering raw material to be discharged, and rotates with the horizontal direction as the rotation axis. The granulated sintering raw material is formed by blowing steam into the sintering raw material only in the drum from the middle position between the input port and the discharge port to the latter half of the discharge port.
3. The method for producing a granulated sintering raw material according to claim 2, When the temperature of the granulated sintering raw material discharged from the granulating device becomes 60° C. or higher, 0.5 mass % or higher and 4.5 mass % or lower of water is further added to the sintering raw material.
4. A method for producing sintered ore, The granulated sintered raw material granulated by the method for producing a granulated sintered raw material according to claim 2 or 3 is sintered in a sintering machine to produce a sintered ore.
Citation Information
Patent Citations
Method for manufacturing granular sintered raw material
WO2019167888A1