Mixture for secondary battery, mixture sheet for secondary battery, method for producing same, and solid-state secondary battery

By using fibrillary resin as a binder, a sulfide-based solid electrolyte with a fibrous structure is solved, and the electrolyte performance deterioration caused by the use of solvents in the prior art is achieved, and a highly efficient and solvent-free secondary battery mixture preparation and High-performance mixture tablet manufacturing.

CN118946987APending Publication Date: 2024-11-12DAIKIN INDUSTRIES LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380024688.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-03-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to avoid the use of solvents when preparing the mixture for secondary batteries, resulting in deterioration of the performance of the sulfide-based solid electrolyte. When processing the mixture tablet for secondary batteries without using a support, it is difficult to manufacture efficiency and performance. promote.

Method used

Using fibrillary resin as the binder, a sulfide-based solid electrolyte with a fibrous structure is treated by shear force to prepare a solvent-free mixture and a mixture tablet for secondary batteries to ensure high productivity and good handling.

Benefits of technology

The production of a compound and a compound tablet for secondary batteries with good properties without using solvents is realized, which improves battery performance and manufacturing efficiency, reduces the deterioration of the sulfide-based solid electrolyte, and enhances the flexibility and strength of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019865010000271
    Figure BDA0005019865010000271
  • Figure BDA0005019865010000281
    Figure BDA0005019865010000281
Patent Text Reader

Abstract

The present disclosure provides a secondary battery mixture containing a sulfide-based electrolyte having good properties, a secondary battery mixture sheet containing the secondary battery mixture, and a solid secondary battery using the secondary battery mixture sheet. A mixture for secondary batteries, which contains a sulfide-based solid electrolyte and a binder, and which is characterized in that the binder is a fibrillar resin. The binder preferably has a fibrous structure having a fibril diameter (central value) of 100 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a mixture for a secondary battery, a mixture sheet for a secondary battery, a method for manufacturing the same, and a solid-state secondary battery. Background Art

[0002] In lithium-ion secondary batteries, a sheet for solid-state secondary batteries is generally produced by applying and drying a slurry obtained by mixing an electrode active material and a conductive auxiliary agent with a binder and a solvent.

[0003] On the other hand, a fibrillated resin such as a polytetrafluoroethylene resin is also used, and the fibrillated resin is used as a binder.

[0004] Patent Document 1 discloses a method for producing an electrode in which a mixture containing an active material and a polytetrafluoroethylene mixed binder material is subjected to a high shearing treatment using a jet mill to fibrillate polytetrafluoroethylene.

[0005] Patent Document 2 discloses the use of an inorganic sulfide having a specific composition in which a crystalline phase and a glass phase coexist as a binder to produce a solid electrolyte layer, a positive electrode, or a negative electrode.

[0006] Patent document 3 discloses a solid electrolyte-containing sheet, which is prepared by electrospinning, microfluidization, or wet spinning to form fibers having an average diameter d of 0.1 to 2 μm and an average length L of 0.2 to 50 mm, and has a solid electrolyte-containing layer having a thickness of t μm and comprising the fibers and an inorganic solid electrolyte, wherein the above L and the above t satisfy the relationship 100×t≤L≤2500×t.

[0007] Patent Document 4 discloses a method in which sulfur-based solid ion conductor inorganic particles and tetrafluoroethylene (TFE) polymer are mixed to form a paste, and then a membrane is produced by calendaring or extrusion.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application No. 2017-517862

[0011] Patent Document 2: International Publication No. 2018-096957

[0012] Patent Document 3: International Publication No. 2019-208347

[0013] Patent Document 4: International Publication No. 2021-043493 Summary of the invention

[0014] Problems to be solved by the invention

[0015] The present disclosure aims to provide a secondary battery mixture containing a sulfide-based solid electrolyte having good properties, a secondary battery mixture sheet containing the mixture, and a solid secondary battery using the secondary battery mixture sheet.

[0016] Another object of the present disclosure is to provide a secondary battery mixture containing a sulfide-based solid electrolyte with high productivity that can be handled even without using a support when forming a secondary battery mixture sheet, and a secondary battery mixture sheet containing the mixture.

[0017] Means for solving problems

[0018] The present disclosure relates to a secondary battery mixture, which is a secondary battery mixture containing a sulfide-based solid electrolyte and a binder, characterized in that:

[0019] The binder is a fibrillar resin.

[0020] The fibrillar resin preferably has a fibrous structure with a fibril diameter (median value) of 100 nm or less.

[0021] The fibrillar resin is preferably a polytetrafluoroethylene resin.

[0022] The sulfide-based solid electrolyte preferably has an average particle size of 0.1 μm or more and 20 μm or less.

[0023] The sulfide-based solid electrolyte is preferably represented by the following formula (A).

[0024] aLi2S-bX 1 S2-cLiX 2 -(1-abc)P2S5(A)

[0025] (where 0.6≤a≤0.86, 0≤b≤0.333, 0≤c≤0.3, 0.05≤b+c≤0.4, X 1 represents Ge, Sn, Ti or Si, X 2 represents Cl, Br or I. wherein either b or c is not 0. )

[0026] The secondary battery mixture is preferably for lithium-ion solid-state secondary batteries.

[0027] Preferably, the secondary battery mixture is a secondary battery mixture obtained using a raw material composition containing a sulfide-based solid electrolyte and a binder, wherein:

[0028] The binder in the above-mentioned raw material composition is a powdery fibrillar resin.

[0029] The raw material composition preferably contains substantially no liquid medium.

[0030] The water content of the powdery fibrillar resin is preferably 500 ppm or less.

[0031] The powdery fibrillar resin is preferably a powdery polytetrafluoroethylene resin.

[0032] The standard specific gravity of the powdery polytetrafluoroethylene resin is preferably 2.12 to 2.20.

[0033] The powdery polytetrafluoroethylene resin preferably contains 50% by mass or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more.

[0034] The present disclosure also relates to a secondary battery mixture sheet, which includes the secondary battery mixture.

[0035] The present disclosure also relates to a method for manufacturing a secondary battery composite sheet, which is a method for manufacturing a secondary battery composite sheet having the following steps:

[0036] Step (1), applying shear force while mixing a raw material composition containing a sulfide-based solid electrolyte and a binder;

[0037] Step (2), forming the secondary battery mixture obtained in the above step (1) into a block shape; and

[0038] Step (3), rolling the block-shaped secondary battery mixture obtained in the above step (2) into a sheet shape,

[0039] The manufacturing method is characterized in that

[0040] The binder is a powdered fibrillar resin.

[0041] The present disclosure also relates to a solid-state secondary battery, which comprises the above-mentioned secondary battery mixture sheet.

[0042] Effects of the Invention

[0043] In the present disclosure, a battery with little degradation of the sulfide-based solid electrolyte can be manufactured by using a powdery binder with little water content instead of a solvent when forming a secondary battery mixture sheet containing a sulfide-based solid electrolyte.

[0044] The present disclosure can also provide a secondary battery mixture containing a sulfide-based electrolyte with high productivity that can be handled even without using a support when forming a secondary battery mixture sheet, and a secondary battery mixture sheet containing the mixture. DETAILED DESCRIPTION

[0045] The present disclosure is described in detail below.

[0046] The present disclosure provides a secondary battery mixture that can be suitably used in a sulfide-based solid-state secondary battery and a mixture sheet containing the secondary battery mixture.

[0047] In the disclosed secondary battery mixture and the mixture sheet containing the secondary battery mixture, a fibrillar resin such as polytetrafluoroethylene resin (PTFE) is used as a binder. In the previous solid secondary battery mixture, the following method is usually adopted: a resin dissolved in a solvent such as a copolymer of vinylidene fluoride and hexafluoropropylene is used as a binder, and a solid secondary battery mixture is prepared by coating and drying a slurry containing the binder.

[0048] On the other hand, it is known that, for example, PTFE in a particle state is prone to fibrillation when shear stress is applied. Utilizing this fibrillation property, PTFE can be used as a binder. That is, the fibrillated PTFE is entangled with other powder components, so that the powder components are bonded, and thus can be used as a binder when the powder components are molded.

[0049] The present disclosure is based on the discovery that, when obtaining a secondary battery mixture containing a sulfide-based solid electrolyte, a secondary battery mixture having good properties and a mixture sheet containing the secondary battery mixture can be obtained even without using a solvent, thereby completing the present disclosure.

[0050] In addition, towards the practical application of solid-state secondary batteries, while improving battery performance such as battery voltage, research for industrial production of solid-state secondary batteries has also been carried out. In order to improve the handling property and manufacturing efficiency of solid-state secondary batteries when the performance of the secondary battery mixture and the mixture sheet containing the secondary battery mixture is studied, it is expected that the secondary battery mixture sheet constituting the solid-state secondary battery can be processed without using a support. Furthermore, from the aspect of manufacturing adaptability, it is expected that these secondary battery mixture sheets can withstand the winding of large curvature when being wound into a roll, etc. Therefore, it is also expected that flexibility is improved.

[0051] As described above, the present disclosure uses a fibrillar resin as a binder to manufacture a secondary battery composite sheet without using a solvent, and thus can manufacture a secondary battery composite sheet without using a support. In addition, the secondary battery composite sheet of the present disclosure uses a sulfide-based solid electrolyte to make a secondary battery composite sheet that is easy to handle and has good flexibility and strength.

[0052] The secondary battery mixture disclosed in the present invention is obtained by using a raw material composition containing a sulfide-based solid electrolyte and a binder, and the binder is preferably a powdered fibrillar resin. As a raw material, a powdered binder is used instead of a dispersion containing a binder, so that there is less water from the raw material in the secondary battery mixture, and problems caused by water mixing will not occur. Thus, it has the advantage of being able to improve battery performance. In addition, a battery with excellent ion conduction can be made.

[0053] In addition, the above-mentioned raw material composition preferably does not substantially contain a liquid medium. In this way, the secondary battery mixture disclosed in the present invention has the advantage of not using a solvent in the manufacture. That is, the previous secondary battery mixture formation method usually uses a solvent in which a binder is dissolved to prepare a slurry in which a powder as a secondary battery mixture component is dispersed, and the secondary battery mixture sheet is prepared by coating and drying the slurry. In this case, a solvent that dissolves the binder is used. However, the solvents that can dissolve the binder resin that are commonly used in the past are limited to specific solvents such as butyl butyrate. They react with sulfide-based solid electrolytes to deteriorate the performance of sulfide-based solid electrolytes, thereby becoming the cause of reduced battery performance. In addition, the binder resin that can be dissolved by low-polarity solvents such as heptane is very limited, and the flash point is low, and the handling is complicated.

[0054] From the above viewpoints, the content of the liquid medium in the secondary battery mixture of the present disclosure is preferably 1% by mass or less. In addition, the content of the liquid medium in the raw material composition is also preferably 1% by mass or less.

[0055] The secondary battery mixture disclosed in the present invention contains a binder having a fibrous structure as a constituent element when the secondary battery mixture containing a sulfide-based electrolyte is prepared. In the present invention, it is important that the binder is fibrillated. Such a fibrillated binder is present in the secondary battery mixture, and it plays a role in bonding the powders of the components constituting the secondary battery mixture to each other, thereby achieving the purpose of the present invention.

[0056] That is, the present disclosure has found that by using a fibrillar resin as a binder and giving the binder in the secondary battery mix a fibrous structure, a secondary battery mix having good properties and a mix sheet containing the secondary battery mix can be obtained, thereby completing the present disclosure.

[0057] In addition, the binder in the secondary battery mixture preferably has a fibrous structure with a fibril diameter (median value) of 100 nm or less. The presence of a binder with a fine fibril diameter in the secondary battery mixture further binds the powders of the components of the secondary battery mixture.

[0058] In the present disclosure, by finely fibrillating the binder so that it has a fibrous structure with a fibril diameter (median value) of 100 nm or less, the fibrillated binder can further reduce the degradation of the oxide-based solid electrolyte as a binder for a secondary battery mixture and can exhibit good performance.

[0059] The fibril diameter (median value) is a value measured by the following method.

[0060] (1) Using a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), a magnified photograph (7000 times) of the secondary battery mixture sheet was taken to obtain an image.

[0061] (2) Draw two lines at equal intervals horizontally on the image to divide the image into three equal parts.

[0062] (3) For all fibrillated binders located on the upper straight line, measure the diameter of each fibrillated binder at three locations, and take the average value as the diameter of the fibrillated binder. The three locations to be measured are the intersection of the fibrillated binder and the straight line, and the locations offset 0.5 μm upward and downward from the intersection. (Unfibrillated binder primary particles are not included).

[0063] (4) The above-mentioned operation (3) is performed on all the fibrillated binders located on the lower straight line.

[0064] (5) Starting from the first image, move 1 mm to the right of the screen and take another image, and measure the diameter of the fibrillated binder using the above (3) and (4). Repeat this operation until the number of measurements exceeds 80.

[0065] (6) The median value of the diameters of all fibrillated binders measured above is taken as the fibril diameter.

[0066] The fibril diameter (median value) is preferably 100 nm or less, more preferably 85 nm or less, and further preferably 70 nm or less. It should be noted that if fibrillation is excessive, there is a tendency to lose flexibility. The lower limit is not particularly limited, and from the aspect of strength, for example, it is preferably 15 nm or more, more preferably 20 nm or more, and particularly preferably 31 nm or more.

[0067] The method for obtaining the binder having the above fibril diameter (median value) is not particularly limited, and examples thereof include a method of performing the following steps:

[0068] Step (1), applying shear force while mixing a raw material composition including a sulfide-based solid electrolyte and a binder powder;

[0069] Step (2), forming the secondary battery mixture obtained in the above step (1) into a block shape; and

[0070] Step (3) is to roll the secondary battery mixture in a block shape obtained in the step (2) into a sheet shape.

[0071] In such a method, for example, by setting the mixing conditions of the raw material composition to below 3000 rpm in step (1), the binder can be fibrillated while maintaining softness, and by controlling the applied shear stress, the fibril diameter (central value) of the binder can be made below 100 nm.

[0072] Furthermore, it is also preferable to have a step (4) after the step (3) in which a larger load is applied to the obtained rolled sheet to roll it into a thinner sheet. It is also preferable to repeat the step (4).

[0073] In addition, after step (3) or step (4), the diameter of the original fibers can also be adjusted by having step (5), which is: the obtained calendered sheet is roughly crushed and then re-molded into a block shape, and calendered into a sheet shape. Step (5) is preferably repeated, for example, once or more and 12 times or less.

[0074] That is, by applying shear stress, the binder powder is fibrillated and entangled with the powder components such as the sulfide-based solid electrolyte, thereby producing a secondary battery mixture. The production method will be described later.

[0075] It should be noted that the above-mentioned "binder powder" does not refer to a dispersed state mixed with a liquid medium, but refers to a solid state as a powder. By utilizing a substance in this state and using a binder in a state without a liquid medium to manufacture a secondary battery mixture, the purpose of the present disclosure can be appropriately achieved.

[0076] The powdery fibrillar resin used as a raw material when preparing the secondary battery mixture of the present disclosure preferably has a moisture content of 500 ppm or less.

[0077] By setting the water content to 500 ppm or less, it is preferable in terms of reducing the degradation of the sulfide-based solid electrolyte.

[0078] The water content is more preferably 300 ppm or less.

[0079] In the present disclosure, a fibrillar resin refers to a resin that is easily fibrillated when a shear stress is applied. By using such a fibrillar resin as a binder, the fibrillar resin is entangled with other powder components, thereby bonding the powder components, so that it can act as a binder when the powder components are molded. For example, as a fibrillar resin, liquid crystal polymer (LCP), cellulose, acrylic resin, ultra-high molecular weight polyethylene, PTFE, etc. can be cited, among which PTFE is preferred from the aspects of chemical stability, thermal stability, and processability.

[0080] In the present disclosure, the PTFE is not particularly limited and may be a homopolymer or a fibrillable copolymer.

[0081] In the case of a copolymer, examples of the fluorine-containing monomer as a comonomer include chlorotrifluoroethylene, hexafluoropropylene, fluoroalkylethylene, perfluoroalkylethylene, fluoroalkyl / fluorovinyl ether and the like.

[0082] The standard specific gravity of the PTFE in powder form is preferably 2.12 to 2.20. By making the standard specific gravity within this range, a high-strength composite sheet can be produced, which has an advantage from this point of view. The lower limit of the above-mentioned standard specific gravity is more preferably more than 2.13. The upper limit of the above-mentioned standard specific gravity is more preferably less than 2.19, and further preferably less than 2.18.

[0083] Regarding the standard specific gravity [SSG], a sample was prepared in accordance with ASTM D-4895-89, and the specific gravity of the obtained sample was measured by the water displacement method.

[0084] The powdered PTFE preferably contains 50% by mass or more of polytetrafluoroethylene resin having a secondary particle size of 450 μm or more, more preferably 80% by mass or more. By making the PTFE having a secondary particle size of 450 μm or more within this range, a high-strength composite sheet can be produced.

[0085] By using PTFE having a secondary particle size of 450 μm or more, a composite sheet having lower electrical resistance and high toughness can be obtained.

[0086] The lower limit of the average secondary particle size of the powdered PTFE is more preferably 450 μm, and further preferably 500 μm. The upper limit of the secondary particle size is more preferably 700 μm or less, and further preferably 600 μm or less. The secondary particle size can be determined, for example, by sieving.

[0087] From the perspective of obtaining a composite sheet with higher strength and excellent homogeneity, the average primary particle size of the powdered PTFE is preferably 150 nm or more, more preferably 180 nm or more, further preferably 210 nm or more, and particularly preferably 220 nm or more.

[0088] The average primary particle size of PTFE is larger, then when using this powder to carry out extrusion molding, the rise of extrusion pressure can be suppressed more, and formability is also more excellent. The upper limit is not particularly limited, and can be 500nm. From the aspect of the productivity in the polymerization process, the upper limit is preferably 350nm.

[0089] Regarding the above-mentioned average primary particle size, a calibration curve of the average primary particle size determined by measuring the transmittance of 550nm projected light per unit length of an aqueous dispersion of PTFE obtained by polymerization and the oriented diameter in a transmission electron microscope photograph is prepared using an aqueous dispersion of PTFE obtained by polymerization. The transmittance is measured for the aqueous dispersion as the measurement object, and can be determined based on the above-mentioned calibration curve.

[0090] The PTFE used in the present disclosure can have a core-shell structure. As the PTFE with a core-shell structure, for example, the core of the polytetrafluoroethylene that comprises a high molecular weight and the polytetrafluoroethylene of a lower molecular weight or the polytetrafluoroethylene of a modified polytetrafluoroethylene shell can be enumerated. As such a modified polytetrafluoroethylene, for example, the polytetrafluoroethylene recorded in writing in the Japanese Patent Table 2005-527652 communique can be enumerated.

[0091] The powdered PTFE satisfying the above parameters can be obtained by a conventional production method, for example, by the production method described in International Publication No. 2015-080291, International Publication No. 2012-086710, etc.

[0092] In the present disclosure, in the solid secondary battery mixture, the lower limit of the content of the binder is preferably 0.2% by mass or more, more preferably 0.3% by mass or more. It is further preferably more than 0.5% by mass. In the solid secondary battery mixture, the upper limit of the content of the binder is preferably 10% by mass or less, more preferably 7% by mass or less, particularly preferably 6% by mass or less, further preferably 4% by mass or less, further preferably 1.7% by mass or less, and most preferably 1.0% by mass or less. If the binder is within the above range, it is possible to form a sheet with self-supporting properties that suppresses the rise in electrode resistance and has excellent handling properties.

[0093] The solid electrolyte used in the solid secondary battery mixture of the present disclosure is a sulfide-based solid electrolyte. When a sulfide-based solid electrolyte is used, there is an advantage of having flexibility.

[0094] Examples of the sulfide-based solid electrolyte include lithium ion conductive inorganic solid electrolytes having a composition represented by the following formula (1).

[0095] Li a1 M b1 Pc1 S d1 A e1 (1)

[0096] In the formula, M represents an element selected from B, Zn, Sn, Si, Cu, Ga, Sb, Al, Ti and Ge. A represents an element selected from I, Br, Cl and F. a1 to e1 represent the composition ratio of each element, and a1:b1:c1:d1:e1 satisfies 1 to 12:0 to 5:1:2 to 12:0 to 10. a1 is preferably 1 to 9, more preferably 1.5 to 7.5. b1 is preferably 0 to 3, more preferably 0 to 1. d1 is preferably 2.5 to 10, more preferably 3.0 to 8.5. e1 is preferably 0 to 5, more preferably 0 to 3.

[0097] In the present disclosure, the sulfide-based solid electrolyte preferably contains lithium. The sulfide-based solid electrolyte containing lithium is used for solid-state batteries using lithium ions as carriers, and is particularly preferred from the perspective of electrochemical devices having high energy density.

[0098] As described below, the composition ratio of each element can be controlled by adjusting the blending amount of the raw material compound when producing the sulfide-based inorganic solid electrolyte.

[0099] The sulfide-based inorganic solid electrolyte may be amorphous (glass), crystallized (glass ceramic), or only partially crystallized. For example, Li-PS-based glass containing Li, P, and S, or Li-PS-based glass ceramic containing Li, P, and S can be used.

[0100] Sulfide-based inorganic solid electrolytes can be manufactured, for example, by reacting at least two or more raw materials including lithium sulfide (Li2S), phosphorus sulfide (e.g., phosphorus pentasulfide (P2S5)), elemental phosphorus, elemental sulfur, sodium sulfide, hydrogen sulfide, lithium halide (e.g., LiI, LiBr, LiCl) and sulfides of the elements represented by M above (e.g., SiS2, SnS, GeS2).

[0101] As specific examples of sulfide-based inorganic solid electrolytes, examples of raw material combinations are shown below. Examples include Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S- S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2 S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li 10 GeP2S 12 Etc. However, there is no limitation on the mixing ratio of each raw material.

[0102] In particular, the sulfide-based solid electrolyte is preferably a sulfide-based solid electrolyte satisfying a composition represented by the following formula (A).

[0103] aLi2S-bX 1 S2-cLiX 2 -(1-abc)P2S5(A)

[0104] (where 0.6≤a≤0.86, 0≤b≤0.333, 0≤c≤0.3, 0.05≤b+c≤0.4, X 1 represents Ge, Sn, Ti or Si, X 2 represents Cl, Br or I. wherein either b or c is not 0. )

[0105] A sulfide-based solid electrolyte having a composition represented by the above formula (A) is advantageous in that high ion conductivity can be stably obtained.

[0106] As an example of the sulfide-based solid electrolyte represented by the above formula (A), specifically, a sulfide-based solid electrolyte selected from 0.714Li2S-0.143SnS2-0.143P2S5 (Li 10 SnP2S 12(LSPS)), 0.625Li2S-0.25LiCl-0.125P2S5(Li6PS5Cl(LPSCl)), 0.715Li2S-0.143GeS2-0.142P2S5(Li 10 GeP2S 12 (LGPS)) etc. or a mixture of two or more thereof.

[0107] The average particle size of the sulfide-based solid electrolyte is preferably 0.1 μm or more and 20 μm or less. The upper limit is more preferably 0.2 μm or more, and further preferably 0.3 μm or more. The upper limit is more preferably 18 μm or less, and further preferably 15 μm or less.

[0108] If the average particle size of the sulfide-based solid electrolyte is less than 0.1 μm, handling of the powder may become difficult. On the other hand, if the average particle size of the sulfide-based solid electrolyte exceeds 20 μm, press moldability may deteriorate.

[0109] It should be noted that the average particle size of the sulfide-based solid electrolyte particles was measured according to the following procedure.

[0110] In a 20 ml sample bottle, the sulfide-based solid electrolyte particles are diluted with water (heptane is used in the case of substances that are unstable to water) to adjust to a 1% dispersion by mass. The diluted dispersed sample is irradiated with 1 kHz ultrasound for 10 minutes and then used in the test immediately. Using the dispersion sample, a laser diffraction / scattering particle size distribution measuring device LA-920 (manufactured by HORIBA) is used to obtain data 50 times at a temperature of 25°C using a measuring quartz dish to obtain the volume average particle size. For other detailed conditions, refer to the description of JIS Z8828:2013 "Particle Size Analysis-Dynamic Light Scattering Method" as needed. Prepare 5 samples for each level and use their average value.

[0111] The method for adjusting the average particle size of the sulfide solid electrolyte is not particularly limited, and is performed, for example, as follows. A known pulverizer or classifier is used. For example, a mortar, a sand mill, a ball mill, a jet mill or a sieve is preferably used. Depending on the properties of the solid electrolyte, a solvent such as water or ethanol may be added during pulverization. In order to form a desired particle size, classification is preferably performed. Classification is not particularly limited, and may be performed using a sieve, a wind classifier, or the like.

[0112] Regarding the content of the sulfide-based solid electrolyte in the solid component of the secondary battery mixture, when considering the reduction of the interface resistance when used in a solid secondary battery and the maintenance of the reduced interface resistance, in the electrode, out of 100% by mass of the solid component, it is preferably 5% by mass or more, more preferably 9% by mass or more, and particularly preferably 12% by mass or more. As an upper limit, from the perspective of battery capacity, it is preferably 60% by mass or less, more preferably 50% by mass or less, and particularly preferably 40% by mass or less.

[0113] In addition, in the solid electrolyte layer disposed between the positive electrode and the negative electrode, preferably 50 mass % or more, more preferably 60 mass % or more, particularly preferably 70 mass % or more. As the upper limit, from the same aspect, preferably 99.9 mass % or less, more preferably 99.8 mass % or less, particularly preferably 99.7 mass % or less.

[0114] The above-mentioned sulfide-based solid electrolytes may be used alone or in combination of two or more.

[0115] In addition, in this specification, solid content (solid content) refers to the component which does not volatilize or evaporate and disappear when drying treatment is carried out at 170 degreeC for 6 hours in nitrogen atmosphere.

[0116] The secondary battery mixture disclosed in the present invention is particularly suitable for lithium-ion solid-state secondary batteries.

[0117] When used in a solid-state secondary battery, the secondary battery mixture of the present disclosure is usually used in a sheet form.

[0118] The secondary battery mixture sheet disclosed in the present invention can be used as a positive electrode sheet or a negative electrode sheet, and can also be used as a solid electrolyte layer sheet.

[0119] Among these, when an electrode sheet is made, active material particles are further contained. The active material particles can be positive electrode active materials or negative electrode active materials. The secondary battery mixture sheet disclosed in the present invention can be more suitable for use as a positive electrode sheet using a positive electrode active material. In addition, when an electrode sheet is made, a conductive auxiliary agent can be contained as needed.

[0120] Hereinafter, the electrode active material, the conductive auxiliary agent, etc. will be described.

[0121] (Electrode Active Material)

[0122] When the secondary battery composite sheet disclosed in the present invention is used as a positive electrode sheet, a positive electrode active material is mixed in the secondary battery composite sheet. The positive electrode active material can be a positive electrode active material known as a positive electrode active material for a solid-state battery. It is particularly preferred to use a positive electrode active material that can contain / release lithium ions.

[0123] As the above-mentioned positive electrode active material, there is no particular restriction as long as it can electrochemically encapsulate / release alkali metal ions, for example, preferably a material containing an alkali metal and at least one transition metal. As specific examples, transition metal composite oxides containing alkali metals, transition metal phosphate compounds containing alkali metals, conductive polymers, etc. can be cited.

[0124] Among them, as the positive electrode active material, a transition metal composite oxide containing an alkali metal that can generate a high voltage is particularly preferred. As the above-mentioned alkali metal ion, lithium ion, sodium ion, potassium ion, etc. can be cited. In a preferred embodiment, the alkali metal ion can be a lithium ion. That is, in this embodiment, the alkali metal ion secondary battery is a lithium ion secondary battery.

[0125] Examples of the alkali metal-containing transition metal composite oxide include

[0126] Formula: M a Mn 2-b M 1 b O4

[0127] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0.9≤a; 0≤b≤1.5; M 1 an alkali metal-manganese spinel composite oxide represented by at least one metal selected from the group consisting of Fe, Co, Ni, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge,

[0128] Formula: MNi 1-c M 2 cO2

[0129] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0≤c≤0.5; M 2 an alkali metal-nickel composite oxide represented by at least one metal selected from the group consisting of Fe, Co, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge, or

[0130] Formula: MCo 1-d M 3 d O2

[0131] (wherein, M is at least one metal selected from the group consisting of Li, Na and K; 0≤d≤0.5; M 3The alkali metal-cobalt composite oxide is represented by at least one metal selected from the group consisting of Fe, Ni, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge.

[0132] Among the above, M is preferably one metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.

[0133] Among them, MCoO2, MMnO2, MNiO2, MMn2O4, MNi 0.8 Co 0.15 Al 0.05 O2, or MNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., preferably a compound represented by the following general formula (3).

[0134] MNi h Co i Mn j M 5 k O2(3)

[0135] (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 5 is at least one selected from the group consisting of Fe, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge, (h+i+j+k)=1.0, 0≤h≤1.0, 0≤i≤1.0, 0≤j≤1.5, 0≤k≤0.2.)

[0136] Examples of the alkali metal-containing transition metal phosphate compound include the following formula (4):

[0137] M e M 4 f (PO4) g (4)

[0138] (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 4 represents at least one selected from the group consisting of V, Ti, Cr, Mn, Fe, Co, Ni and Cu, 0.5≤e≤3, 1≤f≤2, 1≤g≤3). In the above, M is preferably a metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.

[0139] As the transition metal of the lithium-containing transition metal phosphate compound, V, Ti, Cr, Mn, Fe, Co, Ni, Cu and the like are preferred. Specific examples include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7; cobalt phosphates such as LiCoPO4; substances obtained by replacing a part of the transition metal atoms serving as the main body of these lithium transition metal phosphate compounds with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, etc.; and the like.

[0140] The lithium-containing transition metal phosphate compound preferably has an olivine structure.

[0141] As other positive electrode active materials, MFePO4, MNi 0.8 Co 0.2 O2, M 1.2 Fe 0.4 Mn 0.4 O2、MNi 0.5 Mn 1.5 O2, MV3O6, M2MnO3 (wherein M is at least one metal selected from the group consisting of Li, Na and K), etc. In particular, M2MnO3, MNi 0.5 Mn 1.5 When the positive electrode active material such as O2 operates the secondary battery at a voltage exceeding 4.4V or a voltage above 4.6V, the crystal structure will not collapse, which is preferred from this aspect. Therefore, even when an electrochemical device such as a secondary battery using a positive electrode material containing the positive electrode active material exemplified above is stored at high temperature, the residual capacity is not easy to decrease, the resistance increase rate is not easy to change, and even if it operates at a high voltage, the battery performance will not deteriorate, so it is preferred.

[0142] Other positive electrode active materials include M2MnO3 and MM 6 O2 (wherein, M is at least one metal selected from the group consisting of Li, Na and K, M 6 Solid solution materials of transition metals such as Co, Ni, Mn, Fe, etc.

[0143] As the above-mentioned solid solution material, for example, a general formula Mx[Mn (1-y) M 7 y ]O z Here, M in the formula is at least one metal selected from the group consisting of Li, Na and K, and M 7It is composed of at least one metal element other than M and Mn, for example, it contains one or more elements selected from the group consisting of Co, Ni, Fe, Ti, Mo, W, Cr, Zr, and Sn. In addition, the values of x, y, and z in the formula are in the range of 1 < x < 2, 0 ≤ y < 1, and 1.5 < z < 3. Among them, Li 1.2 Mn 0.5 Co 0.14 Ni 0.14 A manganese-containing solid solution material such as Li2MnO3-based and solid-solved with LiNiO2 and LiCoO2 like Li 1.2 Mn 0.5 Co 0.14 Ni 0.14 O2 can provide an alkali metal ion secondary battery with high energy density and is preferred in this regard.

[0144] In addition, if lithium phosphate is included in the positive electrode active material, the continuous charging characteristics are improved, so it is preferred. The use of lithium phosphate is not limited, and it is preferably used in combination with the above positive electrode active material. The amount of lithium phosphate used is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more, based on the total lower limit of the above positive electrode active material and lithium phosphate, and the upper limit is preferably 10% by mass or less, more preferably 8% by mass or less, and further preferably 5% by mass or less.

[0145] Examples of the above conductive polymer include p-doped conductive polymers and n-doped conductive polymers. Examples of conductive polymers include polyacetylene-based, polyphenylene-based, heterocyclic polymers, ionic polymers, ladder and network polymers, etc.

[0146] In addition, a substance with a different composition can be attached to the surface of the above positive electrode active material, and the positive electrode active material thus obtained can be used. Examples of the surface-attached substance include oxides such as alumina, silica, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; carbon; and the like.

[0147] These surface-attached substances can be attached to the surface of the positive electrode active material, for example, by the following methods: a method of dissolving or suspending in a solvent, infiltrating or adding to the positive electrode active material and then drying; a method of dissolving or suspending the surface-attached substance precursor in a solvent, infiltrating and adding to the positive electrode active material, and then reacting it by heating or the like; a method of adding to the positive electrode active material precursor and firing simultaneously; and the like. It should be noted that in the case of attaching carbon, a method of mechanically attaching carbonaceous substances in the form of activated carbon or the like can also be used.

[0148] The amount of the surface-attached substance is preferably 0.1 ppm or more, more preferably 1 ppm or more, and further preferably 10 ppm or more, as the lower limit, and preferably 20% or less, more preferably 10% or less, and further preferably 5% or less, relative to the above-mentioned positive electrode active material, as the upper limit. The surface-attached substance can inhibit the oxidation reaction of the solid electrolyte on the surface of the positive electrode active material, and can improve the battery life. If the amount of attachment is too small, the effect cannot be fully demonstrated; if the amount of attachment is too large, it will hinder the entry and exit of lithium ions, so the resistance may increase.

[0149] The shape of the particles of the positive electrode active material may be a block shape, a polyhedron shape, a sphere shape, an ellipsoidal sphere shape, a plate shape, a needle shape, a column shape, etc. The primary particles may be aggregated to form secondary particles.

[0150] The tap density of the positive electrode active material is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 1.0 g / cm 3 Above. If the tap density of the positive electrode active material is less than the above lower limit, the amount of dispersion medium required when the positive electrode active material layer is formed increases, and the required amount of conductive material or binder increases. Sometimes the filling rate of the positive electrode active material in the positive electrode active material layer will be limited, and the battery capacity will be limited. By using a composite oxide powder with a high tap density, a high-density positive electrode active material layer can be formed. The larger the tap density is, the better, and there is no particular upper limit. However, if it is too large, the diffusion of lithium ions in the positive electrode active material layer with the solid electrolyte as the medium becomes rate-limiting, and sometimes the load characteristics are easily reduced. Therefore, the upper limit is preferably 4.0g / cm 3 Below, more preferably 3.7 g / cm 3 Below, more preferably 3.5 g / cm 3 the following.

[0151] It should be noted that in the present disclosure, the tap density is the powder packing density (tap density) g / cm2 when 5 to 10 g of the positive electrode active material powder is placed in a 10 ml glass cylinder and vibrated 200 times with a stroke of about 20 mm. 3 Find out.

[0152] The median diameter d50 of the particles of the positive electrode active material (secondary particle diameter when the primary particles agglomerate to form secondary particles) is preferably 0.3 μm or more, more preferably 0.5 μm or more, further preferably 0.8 μm or more, and most preferably 1.0 μm or more, and preferably 30 μm or less, more preferably 27 μm or less, further preferably 25 μm or less, and most preferably 22 μm or less. If it is less than the above lower limit, a high tap density product may not be obtained; if it exceeds the upper limit, the diffusion of lithium in the particles takes time, which may cause a decrease in battery performance, or when the positive electrode of the battery is made, that is, the active material and the conductive material, the binder, etc. are made into a slurry using a solvent and applied in a thin film, stripes and other problems may sometimes occur. Here, by mixing two or more of the above-mentioned positive electrode active materials with different median diameters d50, the filling property during the production of the positive electrode can be further improved.

[0153] It should be noted that in the present disclosure, the median diameter d50 is measured using a known laser diffraction / scattering particle size distribution measuring device. When using LA-920 manufactured by HORIBA as a particle size distribution meter, as a dispersion medium used during measurement, a 0.1% by mass sodium hexametaphosphate aqueous solution is used, and after 5 minutes of ultrasonic dispersion, the measured refractive index is set to 1.24 for measurement.

[0154] In the case where the primary particles are agglomerated to form secondary particles, the average primary particle size of the positive electrode active material is preferably 0.05 μm or more, more preferably 0.1 μm or more, and further preferably 0.2 μm or more, and the upper limit is preferably 5 μm or less, more preferably 4 μm or less, further preferably 3 μm or less, and most preferably 2 μm or less. If the upper limit is exceeded, it is difficult to form spherical secondary particles, which has an adverse effect on the powder filling property, or the specific surface area is greatly reduced, so the possibility of reduced battery performance such as output characteristics is sometimes increased. On the contrary, if it is less than the lower limit, problems such as poor reversibility of charge and discharge are usually caused due to poor crystallization.

[0155] It should be noted that in the present disclosure, the average primary particle size of the above-mentioned positive electrode active material is measured by observation using a scanning electron microscope (SEM). Specifically, in a photo with a magnification of 10,000 times, the longest value of the slice generated by the left and right boundary lines of the primary particles relative to the straight line in the horizontal direction is obtained for any 50 primary particles, and the average value is taken to obtain the average primary particle size.

[0156] The BET specific surface area of ​​the positive electrode active material is preferably 0.1 m 2 / g or more, more preferably 0.2m 2 / g or more, more preferably 0.3m 2 / g or more, and the upper limit is preferably 50m2 / g or less, more preferably 40m 2 / g or less, more preferably 30m 2 If the BET specific surface area is smaller than this range, the battery performance is likely to be reduced; if the BET specific surface area is larger than this range, it is difficult to increase the tap density, and the coating property when the positive electrode active material layer is formed may be problematic.

[0157] It should be noted that in the present disclosure, the BET specific surface area is defined as follows: using a surface area meter (for example, a fully automatic surface area measuring device manufactured by Okura Riken Co., Ltd.), the sample is pre-dried at 150°C for 30 minutes under nitrogen flow, and then a nitrogen-helium mixed gas accurately adjusted to a relative pressure value of 0.3 relative to atmospheric pressure is used to measure the sample by the nitrogen adsorption BET single-point method based on the gas flow method, and the obtained value is used to define the BET specific surface area.

[0158] When the secondary battery of the present disclosure is used as a large lithium ion secondary battery for hybrid vehicles or distributed power sources, high output is required, so the particles of the positive electrode active material preferably mainly contain secondary particles.

[0159] The particles of the positive electrode active material preferably have an average particle size of 40 μm or less for the secondary particles and contain 0.5% to 7.0% by volume of microparticles having an average primary particle size of 1 μm or less. By containing microparticles having an average primary particle size of 1 μm or less, the contact area with the solid electrolyte becomes larger, which can further accelerate the diffusion of lithium ions between the all-solid-state secondary battery sheet and the solid electrolyte, and as a result, the output performance of the battery can be improved.

[0160] As a method for manufacturing positive electrode active materials, a common method for manufacturing inorganic compounds is used. In particular, various methods are considered for making spherical or ellipsoidal active materials, for example, the following methods can be cited: dissolving or crushing the raw material of the transition metal and dispersing it in a solvent such as water, adjusting the pH under stirring, making a spherical precursor and recovering it, drying it as needed, then adding LiOH, Li2CO3, LiNO3 and other Li sources and firing at high temperature to obtain the active material.

[0161] In order to manufacture the positive electrode, the above-mentioned positive electrode active materials can be used alone, or two or more of different compositions can be used together in any combination or ratio. As a preferred combination in this case, LiCoO2 and LiNi 0.33 Co 0.33 Mn 0.33A combination of ternary systems such as O2, a combination of LiCoO2 and LiMn2O4 or a material in which a portion of Mn is replaced by other transition metals, or a combination of LiFePO4 and LiCoO2 or a material in which a portion of Co is replaced by other transition metals.

[0162] The content of the positive electrode active material is preferably 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more. In addition, the upper limit is preferably 94.8% by mass or less, more preferably 90.5% by mass or less, and particularly preferably 87.5% by mass or less. If the content of the positive electrode active material in the positive electrode mixture is low, the capacitance is sometimes insufficient. On the contrary, if the content is too high, the electron / ion conduction and strength of the positive electrode are sometimes insufficient.

[0163] The negative electrode active material is not particularly limited, and examples thereof include materials selected from lithium metal, artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolysis vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-fired carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and carbon containing carbonaceous materials such as non-graphitizable carbon, silicon-containing compounds such as silicon and silicon alloys, Li4Ti5O 12 Among them, a substance containing at least a part of a carbonaceous material or a silicon-containing compound can be particularly preferably used.

[0164] The content of the above-mentioned negative electrode active material is preferably 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more. In addition, the upper limit is preferably 94.8% by mass or less, more preferably 90.5% by mass or less, and particularly preferably 87.5% by mass or less. If the content of the negative electrode active material in the negative electrode mixture is low, the capacitance sometimes becomes insufficient. On the contrary, if the content is too high, the electron / ion conduction and strength of the negative electrode are sometimes insufficient.

[0165] (Conductive additive)

[0166] As the above-mentioned conductive auxiliary agent, any known conductive material can be used. As specific examples, metal materials such as copper and nickel, graphite (graphite) such as natural graphite and artificial graphite, carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, needle coke, carbon nanotubes, fullerene, carbon materials such as amorphous carbon such as VGCF, etc. can be cited. It should be noted that they can be used alone or in any combination and ratio. Two or more carbon materials can be used together.

[0167] When a conductive aid is used, the conductive aid is used in an amount of usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and usually 50% by mass or less, preferably 30% by mass or less, more preferably 15% by mass or less in the electrode active material layer. If the content is lower than this range, the conductivity is sometimes insufficient. On the contrary, if the content is higher than this range, the battery capacity is sometimes reduced.

[0168] (Other ingredients)

[0169] The secondary battery mixture sheet may further contain a thermoplastic resin.

[0170] Examples of the thermoplastic resin include vinylidene fluoride, polypropylene, polyethylene, polystyrene, polyethylene terephthalate, and polyethylene oxide, etc. One type may be used alone, or two or more types may be used in any combination and ratio.

[0171] Thermoplastic resin is generally more than 0.01 mass %, preferably more than 0.05 mass %, more preferably more than 0.10 mass %, and generally below 3.0 mass %, preferably below 2.5 mass %, more preferably below 2.0 mass %.By adding thermoplastic resin, the mechanical strength of electrode can be improved.If it exceeds this scope, the ratio of active material in mixture is reduced, and sometimes the problem of the capacity reduction of battery or the problem of resistance increase between active material are produced.

[0172] In the secondary battery composite sheet disclosed in the present invention, about the content of the binder, as the ratio of the binder in the secondary battery composite sheet, it is usually 0.2% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and usually 10% by mass or less, preferably 6.0% by mass or less, more preferably 4% by mass or less, more preferably 1.7% by mass or less, and most preferably 1.0% by mass or less. If the ratio of the binder is too low, the active material cannot be fully maintained in the secondary battery composite sheet, and the mechanical strength of the secondary battery composite sheet is insufficient, which sometimes deteriorates the battery performance such as the cycle characteristics. On the other hand, if the ratio of the binder is too high, it sometimes leads to a reduction in battery capacity and conductivity.

[0173] (Manufacturing method)

[0174] The manufacturing method of the secondary battery composite sheet disclosed in the present invention preferably uses the raw material composition obtained by mixing the above-mentioned components and sheets it. In sheeting, in order to save the drying process, it is preferably a method of applying shear stress to the raw material composition as a powder by reducing or completely not using the amount of liquid medium, not preparing slurry, and performing the process. In addition, in order to reduce the load of the device, a small amount of solvent can also be added as a lubricant. The solvent is preferably an organic solvent, and as the amount of solvent contained, it is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less relative to the raw material composition.

[0175] The method for producing the secondary battery mixture sheet disclosed in the present invention is not limited, and an example of a specific production method is shown below.

[0176] The secondary battery mixture sheet disclosed in the present invention can be obtained by a method for producing a secondary battery mixture sheet having the following steps:

[0177] Step (1), applying shear force while mixing a raw material composition containing an oxide-based solid electrolyte and a binder;

[0178] Step (2), forming the secondary battery mixture obtained in the above step (1) into a block shape; and

[0179] Step (3) is to roll the block-shaped secondary battery mixture obtained in the step (2) into a sheet.

[0180] In the step (1) of applying shear force while mixing the raw material composition, the obtained secondary battery mixture exists in a state where the oxide solid electrolyte, the binder, etc. are simply mixed without a fixed shape. As a specific mixing method, a method of mixing using a W-type mixer, a V-type mixer, a drum mixer, a ribbon mixer, a conical screw mixer, a single screw mixer, a twin screw mixer, a milling machine, a stirring mixer, a planetary mixer, a Henschel mixer, a high-speed mixer, etc. can be cited.

[0181] In the above-mentioned process (1), the mixing conditions only need to appropriately set the rotation speed and mixing time. For example, the rotation speed is suitably below 15000rpm. It is preferably above 10rpm, more preferably above 1000rpm, and more preferably above 3000rpm, and preferably below 12000rpm, more preferably below 11000rpm, and more preferably within the range of 10000rpm. If it is lower than the above-mentioned range, mixing takes time and productivity is affected. In addition, if it exceeds the above-mentioned range, fibrillation is excessively performed, and it is possible to become a composite sheet with poor strength.

[0182] In the above step (1), the temperature is preferably 30°C or higher, more preferably 60°C or higher.

[0183] In addition, it is preferred that a step (A) of mixing the raw material compositions to disperse the binder is included before the step (1). In the step (A), mixing is preferably performed with as small a shear force as possible.

[0184] In the above-mentioned step (A), the mixing conditions only need to appropriately set the rotation speed and mixing time. For example, the rotation speed is preferably below 500 rpm. It is preferably above 20 rpm, more preferably above 30 rpm, and further preferably above 40 rpm, and is preferably below 400 rpm, more preferably below 300 rpm, and further preferably in the range of 200 rpm.

[0185] In the above step (A), the mixing temperature is preferably 19° C. or lower.

[0186] By adopting such a temperature range, it is possible to process into a desired sheet shape in a shorter time.

[0187] PTFE has two transition temperatures at about 19°C and about 30°C. At less than 19°C, PTFE can be easily mixed while maintaining its shape. However, if it exceeds 19°C, the structure of the PTFE particles becomes loose and becomes more sensitive to mechanical shear. At a temperature exceeding 30°C, a higher degree of fibrillation occurs.

[0188] As described above, the raw material composition preferably contains substantially no liquid medium and is preferably in the form of a powder. In the raw material composition in the form of a powder, the content of the liquid medium is preferably 1% by mass or less.

[0189] Therefore, when a PTFE resin is used as the fibrillar resin, the step (A) is preferably carried out at a temperature of 19°C or lower, preferably 0°C to 19°C.

[0190] That is, in such step (A), it is preferred to mix and homogenize without causing fibrillation. Then, it is preferred to perform fibrillation in the subsequent steps (1) to (5).

[0191] In the above step (2), forming into a block shape means forming the secondary battery mixture into a single block.

[0192] Specific examples of the method for forming the block include extrusion molding, press molding, and the like.

[0193] In addition, the so-called "block-shaped" is not a particularly specific shape, as long as it is in a block-shaped state, including strips, sheets, spheres, cubes, etc. The size of the block is preferably such that the diameter of the cross section or the smallest side is 10000 μm or more, and more preferably 20000 μm or more.

[0194] As a specific rolling method in the above step (3), a method of rolling using a roll press, a flat plate press, a calender roll machine or the like can be mentioned.

[0195] In addition, after step (3), it is also preferred to have step (4): applying a greater load to the obtained calendered sheet to calender it into a thinner sheet. It is also preferred to repeat step (4). In this way, the calendered sheet is not thinned all at once, but is calendered little by little in stages, thereby making the softness better.

[0196] The number of times of performing step (4) is preferably 2 to 10 times, and more preferably 3 to 9 times.

[0197] As a specific calendering method, for example, there is a method in which two or more rolls are rotated and a calendered sheet is passed between the rolls to thereby process the sheet into a thinner sheet.

[0198] In addition, from the perspective of adjusting the diameter of the fibrils, it is also preferred to have a step (5) after the step (3) or the step (4): the rolled sheet is roughly crushed and then re-molded into a block shape, and rolled into a sheet shape. It is also preferred to repeat the step (5). The number of times of the step (5) is preferably 1 to 12 times, and more preferably 2 to 11 times.

[0199] In step (5), as a specific method for roughly crushing the rolled sheet and forming it into a block, there can be cited a method of folding the rolled sheet, a method of forming it into a rod or a film sheet, a method of forming it into a chip, etc. In the present disclosure, "roughly crushing" means changing the shape of the rolled sheet obtained in step (3) or step (4) into another shape in order to roll it into a sheet in the next step, and also includes the case of simply folding the rolled sheet.

[0200] In addition, step (4) may be performed after step (5), or the steps may be performed repeatedly.

[0201] Furthermore, uniaxial stretching or biaxial stretching may be performed in step (2) or (3), (4), or (5).

[0202] In addition, the fibril diameter (median value) can also be adjusted by adjusting the degree of coarse pulverization in step (5).

[0203] Steps (2) to (5) are preferably performed at 30°C or higher, more preferably 60°C or higher.

[0204] In the above steps (3), (4) or (5), the calendering rate is preferably 10% or more, more preferably 20% or more, and preferably 80% or less, more preferably 65% ​​or less, and more preferably 50% or less. If it is less than the above range, it takes time as the number of calendering increases, which affects productivity. In addition, if it exceeds the above range, fibrillation is excessively performed, which may result in a composite sheet with poor strength and flexibility.

[0205] It should be noted that the rolling rate mentioned here refers to the reduction rate of the thickness of the sample after processing relative to the thickness before the rolling process. The sample before rolling can be a block-shaped mixture or a sheet-shaped mixture. The thickness of the sample refers to the thickness in the direction of applying the load during rolling.

[0206] As mentioned above, PTFE powder is fibrillated by applying shearing force. And, in order to have the fibrous structure that fibril diameter (median value) is below 100nm, excessive shearing stress can excessively promote fibrillation, sometimes damages flexibility. In addition, in terms of intensity, weak shearing stress is sometimes insufficient. Therefore, when mixing or calendering, by applying shearing stress to appropriate PTFE in the above-mentioned scope to promote fibrillation, calendering mixture and extend into the operation of lamellar, it is possible to have the fibrous structure that fibril diameter (median value) is below 100nm.

[0207] As described above, the secondary battery mixture sheet of the present disclosure can be used as either a positive electrode sheet or a negative electrode sheet. In addition, it can be used as a solid electrolyte layer sheet.

[0208] When the positive electrode mixed material sheet or the negative electrode mixed material sheet is produced, the positive electrode active material or the negative electrode active material may be mixed together with the solid electrolyte and the binder in the production of the mixed material sheet for the secondary battery.

[0209] Hereinafter, the positive electrode and the negative electrode will be described.

[0210] (positive electrode)

[0211] In the present disclosure, the positive electrode is preferably composed of a current collector and the positive electrode sheet described above.

[0212] Examples of the material of the positive electrode current collector include metals such as aluminum, titanium, tantalum, stainless steel, nickel, or alloys thereof, and carbon materials such as carbon cloth and carbon paper. Among them, metal materials, particularly aluminum or alloys thereof, are preferred.

[0213] As the shape of the current collector, in the case of metal materials, metal foil, metal cylinder, metal coil, metal plate, metal plate net, stamping metal, foamed metal, etc. can be enumerated, and in the case of carbon materials, carbon plate, carbon film, carbon cylinder, etc. can be enumerated. Among these, metal foil is preferred. It should be noted that metal foil can be suitably formed into a mesh.

[0214] The thickness of the metal foil is arbitrary, usually 1 μm or more, preferably 3 μm or more, more preferably 5 μm or more, and usually 1 mm or less, preferably 100 μm or less, more preferably 50 μm or less. If the metal foil is thinner than this range, the strength required as a current collector is sometimes insufficient. On the contrary, if the metal foil is thicker than this range, the handling property is sometimes impaired.

[0215] In addition, from the perspective of reducing the electrical contact resistance between the current collector and the positive electrode mixture sheet, it is also preferred that a conductive auxiliary agent is coated on the surface of the current collector. Examples of the conductive auxiliary agent include carbon or precious metals such as gold, platinum, and silver.

[0216] The positive electrode may be produced by a conventional method, for example, a method in which the positive electrode sheet and the current collector are laminated with a binder and then dried.

[0217] The density of the positive electrode sheet is preferably 2.0 g / cm 3 More preferably, 2.1 g / cm 3 More preferably, 2.3 g / cm 3 Above, and preferably 4.0 g / cm 3 Below, more preferably 3.9 g / cm 3 Below, more preferably 3.8 g / cm 3 If the range is exceeded, the conductivity between the active materials decreases, and sometimes the battery resistance increases and high output cannot be obtained. If it is less than this range, the content of hard and easily broken active materials is low, and sometimes the battery has a low capacity.

[0218] The thickness of the positive electrode is not particularly limited. From the perspective of high capacity and high output, the thickness of the composite sheet after subtracting the thickness of the collector is preferably 10 μm or more, more preferably 20 μm or more, and preferably 500 μm or less, more preferably 450 μm or less, relative to a single side of the collector as a lower limit.

[0219] In addition, a positive electrode having a substance having a different composition attached to the surface of the positive electrode may also be used. Examples of the surface-attached substance include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; carbon; and the like.

[0220] (negative electrode)

[0221] In the present disclosure, the negative electrode is preferably composed of a current collector and the negative electrode sheet described above.

[0222] The material of the negative electrode current collector includes metals such as copper, nickel, titanium, tantalum, stainless steel, or alloys thereof; and carbon materials such as carbon cloth and carbon paper. Among them, metal materials are preferred, and copper, nickel, or alloys thereof are particularly preferred.

[0223] As the shape of the current collector, in the case of metal materials, metal foil, metal cylinder, metal coil, metal plate, metal plate mesh, stamping metal, foamed metal, etc. can be cited, and in the case of carbon materials, carbon plate, carbon film, carbon cylinder, etc. can be cited. Among these, metal foil is preferred. It should be noted that the metal foil can be suitably formed into a mesh. The thickness of the metal foil is arbitrary, usually more than 1 μm, preferably more than 3 μm, more preferably more than 5 μm, and usually less than 1 mm, preferably less than 100 μm, more preferably less than 50 μm. If the metal foil is thinner than this range, the strength required as a current collector is sometimes insufficient. On the contrary, if the metal foil is thicker than this range, the handleability is sometimes impaired.

[0224] The negative electrode may be produced by a conventional method, for example, a method in which the negative electrode sheet and the current collector are laminated with a binder and then dried.

[0225] The density of the negative electrode sheet is preferably 1.3 g / cm 3 More preferably, 1.4 g / cm 3 More preferably, 1.5 g / cm 3 Above, and preferably 2.0 g / cm 3 Below, more preferably 1.9 g / cm 3 Below, more preferably 1.8 g / cm 3 If the range is exceeded, the permeability of the solid electrolyte to the interface between the current collector and the active material is reduced, and the charge-discharge characteristics under high current density are reduced, and sometimes high output cannot be obtained. In addition, if it is less than this range, the conductivity between the active materials is reduced, and sometimes the battery resistance increases and high output cannot be obtained.

[0226] The thickness of the negative electrode is not particularly limited. From the perspective of high capacity and high output, the thickness of the composite sheet after deducting the thickness of the metal foil of the collector is preferably 10 μm or more, more preferably 20 μm or more, and preferably 500 μm or less, more preferably 450 μm or less, relative to a single side of the collector.

[0227] (Solid-state secondary battery)

[0228] The present disclosure also relates to a solid-state secondary battery using the secondary battery mixture sheet.

[0229] The solid-state secondary battery may be an all-solid-state secondary battery or a hybrid solid-state secondary battery in which a gel-like polymer electrolyte and a solid electrolyte are combined.

[0230] In addition, the solid-state secondary battery is preferably a lithium-ion battery.

[0231] The solid-state secondary battery disclosed in the present invention is a solid-state secondary battery having a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, and the positive electrode, the negative electrode, and the solid electrolyte layer contain a positive electrode sheet, a negative electrode sheet, or a solid electrolyte layer sheet as the secondary battery mixture sheet disclosed above. It should be noted that the solid-state secondary battery disclosed in the present invention may use a substance that is not a secondary battery mixture sheet disclosed in the present invention in part of the positive electrode, the negative electrode, and the solid electrolyte layer.

[0232] In the present disclosure, a laminated structure of a solid secondary battery includes: a positive electrode including a positive electrode sheet and a positive electrode current collector; a negative electrode including a negative electrode sheet and a negative electrode current collector; and a sulfide-based solid electrolyte layer sandwiched between the positive electrode and the negative electrode.

[0233] Hereinafter, the separator and the battery case used in the solid-state secondary battery of the present disclosure will be described in detail.

[0234] (Diaphragm)

[0235] The solid-state secondary battery disclosed herein may include a separator between the positive electrode and the negative electrode. Examples of the separator include porous films such as polyethylene and polypropylene, and nonwoven fabrics such as nonwoven fabrics made of resins such as polypropylene and nonwoven fabrics made of glass fiber.

[0236] (Battery Design)

[0237] The solid-state secondary battery of the present disclosure may further include a battery case. The shape of the battery case used in the present disclosure is not particularly limited as long as it can accommodate the above-mentioned positive electrode, negative electrode, sulfide-based solid-state battery electrolyte layer, etc. Specifically, cylindrical, square, button-shaped, laminated, etc. can be cited.

[0238] The method for manufacturing a solid-state secondary battery disclosed herein can be, for example, firstly stacking and pressing the above-mentioned positive electrode, solid electrolyte layer sheet, and negative electrode in sequence to produce a solid-state secondary battery.

[0239] By using the secondary battery mixture sheet of the present disclosure, a solid-state secondary battery can be produced in a state where the water content in the system is low, and a solid-state secondary battery having good performance can be obtained, which is suitable.

[0240] Example

[0241] The present disclosure will be described in detail below based on examples.

[0242] In the following examples, "part" and "%" mean "part by mass" and "mass %", respectively, unless otherwise specified.

[0243] [Production example 1]

[0244] At the moment when 367g of TFE is consumed from the start of polymerization (35.6% by mass relative to the total polymerization amount of 1032g of TFE), an aqueous solution (concentration of 4.0ppm relative to the aqueous medium) obtained by dissolving 12.0mg of hydroquinone as a free radical scavenger in 20ml of water is pressed into TFE. Then the polymerization is continued, and the supply of TFE is stopped when the polymerization amount of TFE reaches 1000g from the start of polymerization, and the gas in the system is immediately released to reach normal pressure, and the polymerization reaction is terminated to obtain a polytetrafluoroethylene aqueous dispersion (solid content 31.2% by mass). The obtained polytetrafluoroethylene aqueous dispersion is diluted to a solid content concentration of 15%, and slowly stirred in a container with a stirrer in the presence of nitric acid to solidify the polytetrafluoroethylene. The solidified polytetrafluoroethylene is separated and dried at 160°C for 18 hours to obtain powdered PTFE-1.

[0245] [Production example 2]

[0246] With reference to Preparation Example 3 of International Publication No. 2015-080291, powdered PTFE-2 was prepared.

[0247] [Production example 3]

[0248] With reference to Preparation Example 1 of International Publication No. 2012 / 086710, powdered PTFE-3 was prepared.

[0249] [Production example 4]

[0250] With reference to Preparation Example 1 of International Patent No. 2012-063622, powdered PTFE-4 was prepared.

[0251] Table 1 shows the physical properties of the produced PTFE.

[0252] [Table 1]

[0253] Making PTFE Standard specific gravity Moisture content after drying (ppm) PTFE-1 2.16 <250 PTFE-2 2.15 <250 PTFE-3 2.16 <250 PTFE-4 2.19 <250

[0254] (Example 1)

[0255] Weighing sulfide solid electrolyte Li 10 SnP2S 12(LSPS, 0.714Li2S-0.143SnS2-0.143P2S5) (average particle size: 7 μm) and powdered PTFE-1 were mixed using a high-speed mixer (500 rpm, 1 minute). The container was cooled to 10°C and stirred. Then, the mixture was stirred using a high-speed mixer (10000 rpm, 3 minutes). The container was heated to 60°C and stirred.

[0256] The solid content was calculated by mass ratio of solid electrolyte to binder = 98.5:1.5.

[0257] The powdered PTFE-1 was dried in a vacuum dryer at 50° C. for 1 hour before use. The powdered PTFE used was PTFE that had been previously sieved with a stainless steel sieve having an opening of 500 μm and remained on the sieve.

[0258] The obtained mixture was formed into a block, rolled into a sheet, and heated to 80°C for rolling.

[0259] After that, the rolled sheet just obtained was folded in half and roughly crushed, and after being formed into a block again, it was rolled into a sheet on a flat plate with a metal roller to promote fibrillation, and the above process was repeated 4 times. Then, by further rolling, a sheet-like solid electrolyte layer with a thickness of 500 μm was obtained. Furthermore, the sheet-like solid electrolyte layer was cut out and put into a press for rolling.

[0260] Furthermore, a load of 5 kN was repeatedly applied to adjust the thickness. The gap was adjusted so that the final thickness of the solid electrolyte layer would be 120 μm. The above operation was performed in an Ar glove box (dew point about −80° C.).

[0261] (Example 2)

[0262] Weighing sulfide solid electrolyte Li 10 SnP2S 12 (LSPS) and powdered PTFE-2 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 2.

[0263] (Example 3)

[0264] Weighing sulfide solid electrolyte Li 10 SnP2S 12 (LSPS) and powdered PTFE-3 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 2.

[0265] (Example 4)

[0266] Weighing sulfide solid electrolyte Li 10 SnP2S12 (LSPS) and powdered PTFE-4 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 2.

[0267] (Example 5)

[0268] Weigh the sulfide solid electrolyte Li6PS5Cl (LPSCl, 0.625Li2S-0.25LiCl-0.125P2S 5 ) (average particle size: 8 μm) and powdered PTFE-1 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 2.

[0269] (Example 6)

[0270] Weighing the positive electrode active material LiNi 0.8 Mn 0.1 Co 0.1 O2, sulfide-based solid electrolyte LPSCl (average particle size: 8 μm) and powdered PTFE-1 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 3.

[0271] (Example 7)

[0272] Weighing the positive electrode active material LiNi 0.8 Co 0.15 Al 0.05 O2, sulfide-based solid electrolyte LPSCl (average particle size: 8 μm) and powdered PTFE-1 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 3.

[0273] (Example 8)

[0274] Weighing sulfide solid electrolyte Li 10 GeP2S 12 (LGPS, manufactured by Ampcera, average particle size: 18 μm) and powdered PTFE-2 were molded into a sheet in the same manner as in Example 1. The composition ratio was adjusted to the mass ratio shown in Table 3.

[0275] Each test was performed by the following method.

[0276] [Determination of water content]

[0277] The powdered PTFE was dried in a vacuum dryer at 50°C for 1 hour before use. Regarding the moisture content of the vacuum-dried PTFE, a Karl Fischer moisture meter (ADP-511 / MKC-510N manufactured by Kyoto Electronics Industry Co., Ltd.) with a boat-type moisture vaporizer was used, and the moisture vaporizer was heated to 210°C to measure the vaporized moisture. As a carrier gas, nitrogen was circulated at a flow rate of 200 mL / min, and the measurement time was set to 30 minutes. In addition, Chem-Aqua was used as a Karl Fischer reagent. The sample amount was set to 1.5 g.

[0278] [PTFE fibril diameter (median value)]

[0279] (1) Using a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), a magnified photograph (7000 times) of the sheet-like solid electrolyte layer was taken to obtain an image.

[0280] (2) Draw two lines at equal intervals horizontally on the image to divide the image into three equal parts.

[0281] (3) For all PTFE fibers located on the upper straight line, measure the diameter of each PTFE fiber at three locations, and take the average value as the diameter of the PTFE fiber. The three locations to be measured are the intersection of the PTFE fiber and the straight line, and the locations offset 0.5 μm upward and downward from the intersection. (Not including unfiberized PTFE primary particles).

[0282] (4) The above-mentioned operation (3) is performed on all PTFE fibers located on the lower straight line.

[0283] (5) Starting from the first image, move 1 mm to the right of the screen and take another photo, and measure the diameter of the PTFE fiber using the above (3) and (4). Repeat this operation until the number of measured fibers exceeds 80.

[0284] (6) The median value of the diameters of all the PTFE fibers measured above is taken as the size of the fibril diameter.

[0285] [Ionic conductivity measurement]

[0286] The electrical conductivity was measured by the following method.

[0287] After sputtering a gold electrode on the surface of the solid electrolyte sheet, it was punched into Φ10 mm. It was clamped with a stainless steel collector and sealed to make a measurement battery. After the battery was left to stand in a thermostatic chamber at 80°C for 12 hours, an impedance analyzer (1260 manufactured by Solartron) was used to perform AC impedance measurement in a frequency range of 0.1 Hz to 8 MHz to determine the ion conductivity.

[0288] [Softness evaluation]

[0289] The prepared solid electrolyte sheet was cut into 2 cm long and 6 cm wide as a test piece. After being wound onto a round rod with a diameter of 4 mm, the test piece was visually inspected and evaluated according to the following criteria. The case where no damage or cracks were confirmed was evaluated as ○, and the case where cracks were confirmed was evaluated as ×.

[0290] [Strength measurement]

[0291] A digital dynamometer (IMADA manufactured ZTS-20N) was used to measure the strength of each sample using a 4 mm wide strip electrode mixture test piece at 100 mm / min. The distance between the chucks was set to 30 mm. Displacement was given until fracture, and the maximum stress of the measurement result was used as the strength of each sample. The test was performed 5 times, and the average value was used as the evaluation result.

[0292] The test results are shown in Tables 2 and 3.

[0293]

[0294]

[0295] According to the results in Tables 2 and 3, the sheet-like solid electrolyte layer of the example is excellent in physical properties.

[0296] Next, after sputtering a gold electrode on the surface of the positive electrode mixture sheet prepared in Example 8, the solid electrolyte sheet prepared in Example 2 was overlapped with the Li foil and the insulating sheet, and uniaxial molding was performed for 3 minutes at a load of 60 kN to integrate them, thereby making a punched half-cell with a diameter of 10 mm. The prepared half-cell was placed in a flat battery and placed in a tank at 25°C for 12 hours. Charge and discharge were performed at 0.1C (0.05C cutoff).

[0297] Eight cycles of charge and discharge were performed. As a result, when the capacity retention rate at the third cycle was set as 100%, the capacity retention rate at the eighth cycle was 98.4%.

[0298] Industrial Applicability

[0299] The secondary battery mixture disclosed in the present invention and the secondary battery mixture sheet containing the same can be used for manufacturing a solid-state secondary battery.

Claims

1. A secondary battery mixture, comprising a sulfide-based solid electrolyte and a binder, characterized in that: The binder is a fibrillar resin.

2. The secondary battery mixture according to claim 1, wherein The fibrillar resin has a fibrous structure in which the median value of the fibril diameter, that is, the binder diameter, is 100 nm or less.

3. The secondary battery mixture according to claim 1 or 2, wherein: The fibrillar resin is polytetrafluoroethylene resin.

4. The secondary battery mixture according to any one of claims 1, 2 or 3, wherein The average particle size of the sulfide solid electrolyte is 0.1 μm or more and 20 μm or less.

5. The secondary battery mixture according to any one of claims 1, 2, 3 or 4, wherein The sulfide solid electrolyte is represented by the following formula (A): aLi2S-bX 1 S2-cLiX 2 -(1-a-b-c)P2S5(A) Among them, 0.6≤a≤0.86, 0≤b≤0.333, 0≤c≤0.3, 0.05≤b+c≤0.4, X 1 represents Ge, Sn, Ti or Si, X 2 represents Cl, Br or I; wherein either b or c is not 0.

6. The secondary battery mixture according to claim 1, 2, 3, 4 or 5, which is for lithium ion solid state secondary batteries.

7. The secondary battery mixture according to claim 1 or 2, which is the secondary battery mixture according to claim 1 obtained using a raw material composition containing a sulfide-based solid electrolyte and a binder, wherein: The binder in the raw material composition is a powdery fibrillar resin.

8. The secondary battery mixture according to claim 7, wherein The raw material composition contains substantially no liquid medium.

9. The secondary battery mixture according to claim 7 or 8, wherein The moisture content of the powdery fibrillar resin is 500 ppm or less.

10. The secondary battery mixture according to claim 7, 8 or 9, wherein: The powdery fibrillar resin is a powdery polytetrafluoroethylene resin.

11. The secondary battery mixture according to claim 10, wherein The standard specific gravity of powdered polytetrafluoroethylene resin is 2.12 to 2.

20.

12. The secondary battery mixture according to claim 10 or 11, wherein The powdery polytetrafluoroethylene resin contains 50 mass % or more of a polytetrafluoroethylene resin having a secondary particle size of 450 μm or more. 13 . A secondary battery mixture sheet comprising the secondary battery mixture according to claim 1 .

14. A method for producing a secondary battery composite sheet, comprising the following steps: Step (1), applying shear force while mixing a raw material composition containing a sulfide-based solid electrolyte and a binder; Step (2), forming the secondary battery mixture obtained in step (1) into a block shape; and Step (3), rolling the block-shaped secondary battery mixture obtained in step (2) into a sheet shape, The manufacturing method is characterized in that The binder is a powdered fibrillar resin. 15 . A solid-state secondary battery comprising the secondary battery mixture sheet according to claim 13 .

Citation Information

Cited By

  • Thick electrode and preparation method and application thereof

    CN121054629A