Stable silicon oxynitride layer and manufacturing process thereof
The plasma-enhanced chemical vapor deposition process forms a small thickness and high resistance SiON layer, which solves the problems of large thickness and high refractive index of the existing SiON barrier layer, and realizes electronic devices with smaller size, high resolution and longer life.
Patent Information
- Application Number
- CN202380026929.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2023-02-16
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicon oxynitride (SiON) barrier layer has problems with large thickness and high refractive index in electronic devices, resulting in low equipment density, insufficient resolution and short operating life.
By depositing a silicon-containing nitrogen layer, a chemical vapor deposition process is enhanced by plasma, a SiON layer with a refractive index less than or equal to 1.6 and a low wet etching rate is formed, reducing the layer thickness and improving oxygen and moisture resistance.
A thinner, higher density SiON barrier layer is achieved, supporting smaller size, higher resolution electronic displays, and extending the operating life of the device.
Smart Images

Figure CN118947237A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of and priority to U.S. Provisional Application Serial No. 17 / 677,106, filed on February 22, 2022, which is incorporated herein by reference in its entirety for all purposes. Technical Field
[0003] The present technology relates to deposition processes, structures and systems. More specifically, the present technology relates to methods of producing stable silicon oxynitride layers. Background Art
[0004] Integrated circuits are made possible by processes that produce intricately patterned layers of material on a substrate surface. Producing patterned materials on a substrate requires controlled methods for forming and removing materials. Material properties can affect how a device operates, and can also affect how films are removed relative to each other. Plasma enhanced deposition can produce films with certain properties. Many of the films that are formed require additional processing to adjust or enhance the material properties of the film in order to provide the appropriate properties.
[0005] Therefore, there is a need for improved systems and methods that can be used to produce high quality devices and structures. These and other needs are addressed by the present technology. Summary of the invention
[0006] Embodiments of the present technology include a processing method that includes flowing a deposition gas into a substrate processing region of a processing chamber. The deposition gas includes a silicon-containing gas and a nitrogen-containing gas. The method further includes generating a deposition plasma from the deposition gas in the substrate processing region. The method further includes depositing a silicon-oxygen-nitride-containing layer on the substrate from the deposition plasma. The method further includes exposing a surface of the silicon-oxygen-nitride-containing layer to a treatment plasma to form a treated silicon-oxygen-nitride-containing layer, the treated silicon-oxygen-nitride-containing layer having a treated surface with an increased amount of silicon-nitrogen bonds and a reduced amount of silicon-oxygen bonds, wherein the treatment plasma is formed by the nitrogen-containing gas and is silicon-free.
[0007] In additional embodiments, the silicon-oxygen-nitride-containing layer is characterized by less than or about In a further embodiment, the silicon-containing gas comprises silane, and the nitrogen-containing gas comprises nitrous oxide. In a still further embodiment, the deposition gas further comprises ammonia. In yet another additional embodiment, the deposition plasma is characterized by greater than or about 1×10 11 ions / cm 3 The ion density is 200°C and the deposition of the silicon-oxygen-nitride-containing layer on the substrate is characterized by a deposition temperature of less than or about 100°C. In yet further embodiments, the treated silicon-oxygen-nitride-containing layer is characterized by a deposition temperature of less than or about In more embodiments, the treated silicon-oxygen-nitride-containing layer is characterized by a wet etch rate of greater than or about 2.1 g / cm 3 In yet more embodiments, the treated silicon oxynitride-containing layer is characterized by an index of refraction of less than or about 1.6.
[0008] Embodiments of the present technology further include an additional processing method, the additional processing method comprising depositing a first silicon-oxygen-nitride-containing layer on the substrate. The first silicon-oxygen-nitride-containing layer is characterized by less than or about The method further includes depositing at least one additional silicon-oxygen-nitride-containing layer on the first silicon-oxygen-nitride-containing layer to form a multilayer stack of silicon-oxygen-nitride-containing layers, wherein the multilayer stack is characterized by less than or about The method further includes exposing the top surface of the multilayer stack to a treatment plasma to form a treated multilayer stack. The treatment plasma is formed from a nitrogen-containing gas and is silicon-free.
[0009] In additional embodiments, the first silicon-oxygen-nitride-containing layer and the at least one additional silicon-oxygen-nitride-containing layer are deposited using a deposition plasma characterized by a temperature greater than or about 1×10 11 ions / cm 3 In further embodiments, the deposition plasma is generated from a deposition gas that includes a silicon-containing gas and a nitrogen-containing gas. In still further embodiments, the treated multilayer stack of silicon-oxygen-nitride-containing layers is characterized by a refractive index of less than or about 1.6. In yet additional embodiments, the treated multilayer stack of silicon-oxygen-nitride-containing layers is characterized by a refractive index of less than or about In further embodiments, the nitrogen-containing gas in the treatment plasma includes ammonia.
[0010] Embodiments of the present technology further include a structure comprising a substrate and at least one silicon-oxygen-nitride-containing layer. The silicon-oxygen-nitride-containing layer is characterized by less than or about A thickness of less than or about 1.6, a refractive index of less than or about 1.6, and a / min wet etching rate.
[0011] In additional embodiments, the at least one silicon oxynitride-containing layer is a single layer. In further embodiments, the at least one silicon oxynitride-containing layer comprises at least two layers of silicon oxynitride-containing material, wherein each of the at least two layers is characterized by less than or about In yet further embodiments, the at least two layers of silicon-oxygen-nitride-containing material include a top layer characterized by a stress level different from that of the other layers of silicon-oxygen-nitride-containing material. In yet additional embodiments, at least one silicon-oxygen-nitride-containing layer is characterized by a stress level greater than or about 2.1 g / cm 3In further embodiments, at least one silicon-oxygen-nitride-containing layer comprises silicon oxynitride (SiON).
[0012] Compared to conventional processing methods for making silicon-oxygen-nitrogen barrier layers, this technology can provide numerous advantages. For example, compared to conventional barrier layers with the same resistance to oxygen and moisture migration through the barrier layer, the barrier layer formed by the present processing method is significantly thinner. This allows thinner barrier layers to be incorporated into electronic products (such as electronic displays) with smaller device sizes and higher device densities. Among other benefits, thinner barrier layers make it possible to reduce device sizes and produce higher resolution displays. In addition, the improved oxygen and moisture resistance of the present silicon-oxygen-nitrogen barrier layer can increase the operating life of electronic products incorporating the barrier layer. Since the time it takes for oxygen and moisture to penetrate the barrier layer and react with oxygen- and moisture-sensitive materials in the underlying substrate is significantly longer, the electronic product can have a longer operating life. These and other embodiments, together with many of their advantages and features, are described in more detail in conjunction with the following description and accompanying drawings.
[0013] BRIEF DESCRIPTION OF THE DRAWINGS
[0014] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the accompanying drawings.
[0015] Figure 1A A top plan view of an exemplary processing system in accordance with embodiments of the present technology is shown.
[0016] Figure 1B A schematic cross-sectional view of an exemplary plasma system is shown in accordance with an embodiment of the present technology.
[0017] Figure 2 The operation of an exemplary processing method according to an embodiment of the present technology is shown.
[0018] Figure 3 An exemplary structure according to an embodiment of the present technology is shown.
[0019] Figure 4 Another exemplary structure according to an embodiment of the present technology is shown.
[0020] Several of the drawings are included as schematic diagrams. It should be understood that the drawings are for illustrative purposes and should not be considered to scale unless specifically noted to be to scale. Additionally, as schematic diagrams, the drawings are provided to aid understanding and may not include all aspects or information compared to realistic representations and may include material that is exaggerated for illustrative purposes.
[0021] In the accompanying drawings, similar components and / or features may have the same reference numerals. In addition, various components of the same type may be distinguished by following the reference numeral with a letter that distinguishes the similar components. If only the first reference numeral is used in the specification, the description applies to any of the similar components having the same first reference numeral, regardless of the letter. DETAILED DESCRIPTION
[0022] More and more electronic devices are made with more moisture-sensitive materials. For example, more and more electronic displays are made with organic light-emitting diodes (OLEDs), which include complex organic molecules that emit light in response to an electric current. These molecules can lose their light-emitting properties when exposed to small amounts of moisture.
[0023] The development of protective barriers to block oxygen and moisture from reaching moisture-sensitive materials plays an important role in the widespread adoption of moisture-sensitive electronic devices such as OLED displays. These protective barriers include thin film encapsulation (TFE) barriers that cover moisture-sensitive materials and prevent oxygen and moisture in the surrounding environment from reaching the moisture-sensitive materials. Examples of materials used to make TFE barriers include hydrophobic organic polymers and moisture-resistant inorganic materials. The effectiveness of these TFE barriers is evaluated for their ability to block oxygen and moisture, their crack resistance, and their ability to dissipate heat, as well as other properties.
[0024] One material that has gained wide acclaim for TFE barriers is silicon oxynitride (SiON). SiON is relatively easy to deposit on moisture-sensitive materials using a plasma enhanced chemical vapor deposition process. Under typical operating conditions for electronic devices such as OLED displays, TFE barriers including SiON have good oxygen and moisture resistance over the currently recognized lifetime of these devices. However, the continued development of these devices requires TFE barriers to be more compact and have a lower refractive index without sacrificing their effectiveness in blocking oxygen and moisture.
[0025] Embodiments of the present technology address the desire to make TFE barriers from SiON that is smaller than conventional SiON barriers. The present technology includes embodiments that deposit SiON-containing layers that have the same or greater resistance to oxygen and moisture penetration than conventional SiON layers that are twice as thick or thicker. The present technology also includes embodiments that deposit SiON-containing layers that have refractive indices less than or about 1.6 without reducing their effectiveness as barriers to moisture and oxygen. In contrast, conventional SiON layers experience significant degradation in their moisture and oxygen resistance when the RI drops below 1.63. In various embodiments, the present SiON barrier layers may be characterized by less than or about and an RI of less than or about 1.6, whereas conventional SiON barrier layers having comparable moisture resistance are characterized by having a thickness of greater than or about and a thickness of greater than or about 1.63.
[0026] Among other benefits, the present technology provides SiON-containing barrier layers with reduced thickness for moisture-sensitive electronic components and devices characterized by reduced size and increased complexity. Embodiments of the present technology reduce the thickness of the SiON barrier layer to less than half the thickness of a conventional SiON barrier layer, thereby permitting a higher density of electronic components (such as OLED pixels) to occupy a given area. In additional embodiments, the SiON barriers are characterized by a refractive index of less than or about 1.6 without reducing their effectiveness as a barrier to moisture and oxygen. This permits the manufacture of more compact, higher resolution display devices without reducing the operating lifetime due to moisture and oxygen degradation of moisture-sensitive materials in the device.
[0027] Embodiments of the present technology include methods of forming and processing one or more silicon-oxygen-nitride-containing layers on a substrate. Embodiments further include structures made by the method. The following description begins with an embodiment of a system of the present technology, on which the method can be performed. Although specific deposition and processing processes utilizing the present technology are described, it will be readily understood that the system and method are equally applicable to other deposition and processing systems, and processes that may occur in the described systems. Therefore, the present technology should not be limited to the specific processes, structures, and systems described herein. A system embodiment is first described, which includes a chamber used in the system to perform deposition and processing processes according to embodiments of the present technology.
[0028] Figure 1A 1 shows a top plan view of an embodiment of a processing system 100 according to an embodiment of the present technology. In various embodiments, the processing system 100 may include deposition chambers, process chambers, etching chambers, baking chambers, and curing chambers, among other types of chambers. Figure 1A As shown, a pair of front opening unified pods 102 supply substrates of various sizes, which are received by a robot 104 and placed in a low pressure holding area 106 before being placed in one of the substrate processing chambers 108a to 108f positioned in the series sections 109a to 109c. A second robot 105 can be used to transport substrate wafers from the holding area 106 to the substrate processing chambers 108a to 108f and back. Each substrate processing chamber 108a to 108f can be equipped to perform one or more substrate processing operations, including deposition and processing of barrier layer materials as described herein. In various embodiments, the substrate processing chambers 108a to 108f can be configured to perform plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, etching, pre-cleaning, degassing, orientation, and other substrate processing (including annealing, ashing, etc.).
[0029] The substrate processing chambers 108a to 108f may include one or more system components for depositing, processing, annealing, curing and / or etching barrier layer materials on substrates. In one configuration, two pairs of processing chambers (e.g., 108c to 108d and 108e to 108f) may be used to deposit and process barrier layer materials on substrates, and a third pair of processing chambers (e.g., 108a to 108b) may be used to etch the deposited and processed barrier layer materials. In another configuration, the three pairs of chambers (e.g., 108a to 108f) may be configured to deposit a multilayer stack of layers of barrier material on a substrate. Any one or more of the described processes may be performed in a chamber separate from the manufacturing system shown in different embodiments. It should be understood that the system 100 encompasses additional configurations of deposition chambers, processing chambers, etching chambers, annealing chambers, and curing chambers for barrier layer materials.
[0030] Figure 1B A schematic cross-sectional view of an exemplary plasma system 110 is shown in accordance with an embodiment of the present technology. Figure 1B In the illustrated embodiment, system 110 is a HDP-CVD system that includes chamber 113 , vacuum system 170 , source plasma system 180A, bias plasma system 180B, gas delivery system 133 , and remote plasma cleaning system 150 .
[0031] In various embodiments, the upper portion of the chamber 113 includes a dome 114, which can be made of a ceramic dielectric material such as aluminum oxide or aluminum nitride, sapphire, SiC, or quartz, among other materials. A heater plate 123 and a cold plate 124 can be on top of the dome 114 and thermally coupled to the dome. The heater plate 123 and the cold plate 124 can allow the dome temperature to be controlled within about ±10° C. in a range of greater than or about 70° C., greater than or about 80° C., greater than or about 90° C., greater than or about 100° C., greater than or about 110° C., or more. In various embodiments, the dome 114 can define an upper boundary of the plasma processing region 116. In further embodiments, the bottom of the plasma processing region 116 can be defined by an upper surface of the substrate 117 and the substrate support member 118.
[0032] In additional embodiments, the lower portion of the chamber 113 may include a body member 122 that couples the chamber to a vacuum system. A base portion 121 of a substrate support member 118 may be mounted on the body member 122 and form a continuous inner surface with the body member. The substrate may be transferred into and out of the chamber 113 by a robot (not shown) through an insertion / removal opening (not shown) in the side of the chamber 113. A lift pin (not shown) may be raised and then lowered under the control of a motor (also not shown) to move the substrate from the robot at the upper loading position 157 to the lower processing position 156, where the substrate is placed on a substrate receiving portion 119 of the substrate support member 118. The substrate receiving portion 119 may include an electrostatic chuck 120 that secures the substrate to the support member 118 during substrate processing. In various embodiments, the substrate support member 118 may be made of an alumina or aluminum ceramic material.
[0033] In further embodiments, the vacuum system 170 may include a throttle body 125 that may house a dual blade throttle valve 126 and may be attached to a gate valve 127 and a turbomolecular pump 128. It should be noted that the throttle body 125 may provide minimal obstruction to gas flow and allow for symmetrical pumping. The gate valve 127 may also isolate the pump 128 from the throttle body 125 and may also control chamber pressure by limiting exhaust flow capacity when the throttle valve 126 is fully open. The arrangement of the throttle valve, gate valve, and turbomolecular pump may be operable to accurately and stably control chamber pressure between about 1 mTorr and about 2 Torr.
[0034] In yet further embodiments, the source plasma system 180A may include a top coil 129 and a side coil 130 mounted on the dome 114. A symmetrical ground shield (not shown) reduces electrical coupling between the coils. The top coil 129 may be powered by a top source RF (SRF) generator 131A, while the side coil 130 may be powered by a side SRF generator 131B, thereby allowing independent power levels and operating frequencies for each coil. This dual coil system may allow control of radial ion density in the chamber 113 to improve plasma uniformity. The side coil 130 and the top coil 129 may be inductively driven, which does not require complementary electrodes. In various embodiments, the top source RF generator 131A may provide an RF power greater than or about 1,500 watts at a nominal 13.56 MHz, and the side source RF generator 131B may provide an RF power greater than or about 2,500 watts at a nominal 13.56 MHz. The operating frequencies of the top RF generator and the side RF generators may be deviated from the nominal operating frequencies (eg, 1.7 MHz to 1.9 MHz and 1.9 MHz to 2.1 MHz, respectively) to improve plasma generation efficiency.
[0035] In further embodiments, the bias plasma system 180B may include a bias RF ("BRF") generator 131C and a bias matching network 132C. The bias plasma system 180B may be capacitively coupled to the substrate portion 117 to the body member 122, which acts as a complementary electrode. The bias plasma system 180B may be used to enhance the transport of plasma species (e.g., ions) generated by the source plasma system 180A to the surface of the substrate. In various embodiments, the bias RF generator may provide greater than or about 5,000 watts of RF power at 4 MHz.
[0036] In yet more embodiments, the RF generators 131A and 131B may include digitally controlled synthesizers and operate in a frequency range between about 1.8 MHz and about 2.1 MHz. Each generator may include an RF control circuit (not shown) that measures the reflected power returned from the chamber and coil to the generator and adjusts the operating frequency to obtain the lowest reflected power. The RF generator may be designed to operate in a load having a characteristic impedance of 50 ohms. The RF power may be reflected from a load having a different characteristic impedance than the generator. This may reduce the power delivered to the load. Additionally, the power reflected back from the load to the generator may overload and damage the generator. Since the impedance of the plasma may range from less than 5 ohms to greater than 900 ohms, depending on the plasma ion density, and other factors, and since the reflected power may vary with frequency, adjusting the generator frequency based on the reflected power increases the power delivered from the RF generator to the plasma and protects the generator. Another way to reduce reflected power and improve efficiency is to use a matching network.
[0037] In additional embodiments, matching networks 132A and 132B can match the output impedance of generators 131A and 131B to the top coil 129 and the side coil 130, respectively. The RF control circuit can tune the matching networks by changing the values of the capacitors within the two matching networks to match the generator to the load as the load changes. The RF control circuit can tune the matching networks when the power reflected from the load back to the generator exceeds a certain limit. One way to provide a constant match and effectively inhibit the RF control circuit from tuning the matching networks is to set the reflected power limit higher than any expected value of the reflected power. This can help stabilize the plasma under some conditions by keeping the matching networks constant at their most recent condition.
[0038] Other measures may also help stabilize the plasma. For example, RF control circuitry may be used to determine the power delivered to the load (plasma), and the generator output power may be increased or decreased to keep the delivered power substantially constant during deposition of the layer.
[0039] In various embodiments, the gas delivery system 133 may provide gases from several sources (134A to 134E chambers) via gas delivery lines 138 (only some of the gas delivery lines are shown) for processing the substrate. As will be appreciated by those skilled in the art, the actual sources for the sources 134A-134E and the actual connections of the delivery lines 138 to the chamber 113 vary depending on the deposition and cleaning processes performed within the chamber 113. The gases may be introduced into the chamber 113 via the gas ring 137 and / or the gas distributor 111. In various embodiments, the gas distributor 111 may include a first channel adapted to inject a silicon-containing gas (such as SiH4) and a second channel adapted to inject one or more nitrogen-containing gases (such as N2O and / or NH3) that undergo a chemical reaction with the source gas to form a silicon-oxygen-nitrogen-containing material on the substrate. Work related to embodiments of the present invention has shown that such a gas distributor can provide uniform deposition of silicon-oxygen-nitride-containing materials that avoids silicon-rich deposition in the central region of the substrate, such as embodiments using a gas ring having nozzles distributed around the substrate near the sidewalls of the chamber.
[0040] In further embodiments, the first and second gas sources 134A and 134B and the first and second gas flow controllers 135A' and 135B' may provide gas to the ring plenum in the gas ring 137 via gas delivery lines 138 (only some of the gas delivery lines are shown). In more embodiments, the gas ring 137 has a plurality of source gas nozzles 139 (only one of the source gas nozzles is shown for illustrative purposes) that provide a uniform gas flow over the substrate. The nozzle length and nozzle angle may be varied to allow the uniformity distribution and gas utilization efficiency to be adjusted for specific processes in individual chambers. In various embodiments, the gas ring 137 may have twelve source gas nozzles made of alumina ceramic. In further embodiments, the source gas nozzles 139 inject a silicon-containing gas (such as SiH4) into the chamber, which may be mixed with a nitrogen-containing gas (such as nitrous oxide (N2O)) injected from additional nozzles to form a dielectric layer.
[0041] In yet further embodiments, the gas ring 137 may also have a plurality of oxidant gas nozzles 140 (only one of which is shown), which in preferred embodiments are coplanar with and shorter than the source gas nozzles 139, and in various embodiments receive gas from a bulk gas chamber. In additional embodiments, it may be desirable not to mix the source gas and the oxidant gas prior to injecting the gas into the chamber 113. In other embodiments, the oxidant gas and the source gas may be mixed prior to injecting the gas into the chamber 113 by providing an orifice (not shown) between the bulk gas chamber and the gas ring gas chamber. In one embodiment, a third gas source 134C, a fourth gas source 134D, and a fifth gas source 134D' and a third gas flow controller 135C and a fourth gas flow controller 135D' provide gas to the bulk gas chamber via a gas delivery line 138. Additional valves, such as 143B (other valves not shown), may shut off gas from the flow controllers to the chamber.
[0042] In embodiments where flammable, toxic, or corrosive gases are used, it may be desirable to eliminate gases remaining in the gas delivery line after deposition. For example, this may be accomplished using a three-way valve, such as valve 143B, to isolate chamber 113 from delivery line 138A and vent delivery line 138A to vacuum foreline 144. Figure 1B As shown, other similar valves (such as 143A and 143C) may be incorporated on other gas delivery lines.
[0043] In various embodiments, the chamber 113 may also have a gas distributor 111 (or top nozzle) and a top vent 146. The gas distributor 111 and the top vent 146 may allow independent control of the top and side flows of the gas, which improves film uniformity and allows fine-tuning of the deposition and doping parameters of the film. The top vent 146 may have an annular opening around the gas distributor 111. In further embodiments, the gas distributor 111 may include a plurality of holes in the steps according to embodiments of the present invention for improved gas distribution. In yet further embodiments, the first gas source 134A may supply the source gas nozzle 139 and the gas distributor 111. In additional embodiments, the source nozzle multifunction controller (MFC) 135A' may control the amount of gas delivered to the source gas nozzle 139, and the top nozzle MFC 135A controls the amount of gas delivered to the gas distributor 111. Similarly, two MFCs 135B and 135B' may be used to control the flow of oxygen from a single oxygen source, such as source 134B, to top vent 146 and oxidant gas nozzle 140. The gases supplied to gas distributor 111 and top vent 146 may be kept separate prior to flowing the gases into chamber 113, or the gases may be mixed in top plenum 148 prior to flowing the gases into chamber 113. Separate sources of the same gas may be used to supply various portions of the chamber.
[0044] In still further embodiments, baffles 158 may be formed on the gas distributor 111 to direct the clean gas flow toward the chamber walls and may also be used to direct the remotely generated plasma and clean gas flow. The gas distributor may include two separate channels that pass two separate gases into the chamber 113 where they mix and react above the semiconductor substrate.
[0045] In a further embodiment, a remote microwave generated plasma cleaning system 150 may be provided to periodically clean deposition residues from chamber components. The cleaning system includes a remote microwave generator 151 that generates plasma in a reactor cavity 153 from a cleaning gas source 134E (e.g., molecular fluorine, nitrogen trifluoride, other fluorocarbons, or equivalent). Reactive species generated from this plasma are transported through a cleaning gas feed port 154 to the chamber 113 via an applicator tube 155. The materials used to contain the cleaning plasma (e.g., the cavity 153 and the applicator tube 155) are resistant to erosion by the plasma. Generating a cleaning plasma in a remote cavity allows the use of an efficient microwave generator and does not subject chamber components to the temperatures, radiation, or bombardment of a glow discharge that may be present in an in-situ formed plasma. Therefore, relatively sensitive components (such as an electrostatic chuck 120) may not be covered or otherwise protected by a dummy wafer.
[0046] In the illustrated embodiment, the plasma cleaning system 150 is below the chamber 113, but other locations may alternatively be used, for example, above the chamber 113. In this alternative embodiment, the distance between the reactor cavity and the feed port may be kept short, since the concentration of the desired plasma species may decrease with distance from the reactor cavity. With a clean gas feed positioned above the baffle at the top of the chamber, remotely generated plasma species may be provided through the clean gas feed port and may be directed to the side of the chamber by the baffle.
[0047] In various embodiments, the system controller 160 may control the operation of the system 110. In various embodiments, the controller 160 may include a memory 162, which includes a tangible medium coupled to the processor 161, such as a solid state drive, a hard disk drive, a floppy disk drive (not shown), and / or a card rack (not shown). The card rack may accommodate a single board computer (SBC) (not shown), analog and digital input / output boards (not shown), an interface board (not shown), and a stepper motor controller board (not shown). In various embodiments, the system controller may conform to the Versatile Module Europe ("VME") standard, which defines board, card cage, and connector sizes and types. The system controller 160 operates under the control of a computer program stored on a tangible medium (e.g., a hard disk drive), or through other computer programs (such as programs stored on a removable disk). The computer program may control, for example, the timing of a particular process, the mixing of gases, RF power levels, and other parameters. In additional embodiments, the interface between the user and the system controller may be via a touch screen display and a keyboard.
[0048] In various embodiments, the system controller 160 can control the seasoning time of the chamber and the gas used to season the chamber, control the cleaning time and gas used to clean the chamber, and control the application of plasma with the HDP CVD process. To achieve such control, the system controller 160 can be coupled to many of the components of the system 110. For example, the system controller 160 can be coupled to one or more of the vacuum system 170, the source plasma system 180A, the bias plasma system 180B, the gas delivery system 133, and the remote plasma cleaning system 150. In various embodiments, the system controller 160 can be coupled to the vacuum system 170 using line 163. In more embodiments, the system controller 160 can be coupled to the source plasma system 180 using line 164A and to the bias plasma system 180B using line 164B. In still more embodiments, the system controller 160 can be coupled to the gas delivery system 133 using line 165. In yet additional embodiments, the system controller 160 can be coupled to the remote plasma cleaning system 150 using line 166. In various embodiments, lines 163, 164A, 164B, 165, and 166 may transmit control signals from system controller 160 to vacuum system 170, source plasma system 180A, bias plasma system 180B, gas delivery system 133, and remote plasma cleaning system 150. For example, system controller 160 may separately control each of flow controllers 135A to 135E and 135A' to 135D' using line 165. Line 165 may include a separate control line connected to each flow controller. In further embodiments, system controller 160 may include several distributed processors to control components of system 110.
[0049] Figure 2 Operations of an exemplary processing method 200 in accordance with some embodiments of the present technology are shown. Method 200 forms a silicon-oxygen-nitride-containing barrier to prevent moisture and oxygen from contacting a substrate on which the barrier is formed. In some embodiments, the barrier may include a single silicon-oxygen-nitride-containing layer, while in additional embodiments, the barrier may include multiple layers forming a multi-layer stack barrier layer. For both single-layer and multi-layer stack barrier layers, the thickness of the barrier layer is significantly less than a conventional silicon-oxygen-nitride-containing barrier layer having the same moisture resistance and a lower refractive index. In various embodiments, the present silicon-oxygen-nitride-containing barrier layer may be characterized by less than or about Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Or a smaller thickness.
[0050] In various embodiments, the silicon-oxygen-nitride-containing barrier layer slows down or prevents moisture and oxygen on one side of the barrier layer from reaching a substrate in contact with the opposite side of the barrier layer. In further embodiments, the substrate protected from moisture and oxygen may include moisture and oxygen sensitive materials, such as complex light-emitting organic molecules used in OLED displays. In still further embodiments, the barrier layer may cover or encapsulate pixels or components of pixels in an OLED display.
[0051] Method 200 includes providing a deposition gas for depositing a silicon-oxygen-nitride-containing material at operation 205. In various embodiments, the deposition gas may include one or more silicon-containing gases and one or more nitrogen-containing gases. In still further embodiments, the silicon-containing gas may include silane (SiH4), as well as other silicon-containing gases. In further embodiments, the nitrogen-containing gas may include nitrous oxide (N2O), nitric oxide (NO), nitrogen dioxide (NO2) and ammonia (NH3), as well as other nitrogen-containing gases. In further embodiments, the deposition gas is substantially free of moisture (H2O) and may be characterized as having a moisture level of less than or about 0.1 wt%, less than or about 0.01 wt%, less than or about 0.001 wt%, or less.
[0052] In various embodiments, a deposition gas may be provided to a substrate processing region of a substrate processing chamber. In further embodiments, a silicon-containing gas may be provided at a flow rate greater than or about 10 sccm, greater than or about 20 sccm, greater than or about 30 sccm, greater than or about 40 sccm, greater than or about 50 sccm, greater than or about 60 sccm, greater than or about 70 sccm, greater than or about 80 sccm, greater than or about 90 sccm, greater than or about 100 sccm, or greater. In still further embodiments, a nitrogen-containing gas may be provided at a flow rate greater than or about 10 sccm, greater than or about 25 sccm, greater than or about 50 sccm, greater than or about 75 sccm, greater than or about 100 sccm, greater than or about 125 sccm, greater than or about 150 sccm, greater than or about 175 sccm, greater than or about 200 sccm, or greater. In yet more embodiments, the silicon-containing gas to nitrogen-containing gas may be characterized by a Si gas to N gas flow rate ratio of less than or about 1:2, less than or about 1:3, less than or about 1:4, less than or about 1:5, less than or about 1:6, less than or about 1:7, less than or about 1:8, less than or about 1:9, less than or about 1:10, or less.
[0053] In further embodiments, the nitrogen-containing gas may include two or more nitrogen-containing gases. In yet more embodiments, the nitrogen-containing gas may include nitrous oxide (N2O) and ammonia (NH3). In yet further embodiments, the NH3:N2O flow rate ratio may be higher than or about 1:1, higher than or about 1.5:1, higher than or about 2:1, higher than or about 2.5:1, higher than or about 3:1, higher than or about 3.5:1, higher than or about 4:1, higher than or about 4.5:1, higher than or about 5:1 or higher. In yet more embodiments, the deposition gas may include silane, ammonia and nitrous oxide, and the SiH4:NH3:N2O flow rate ratio of the gas may be characterized as lower than or about 1:4:2. In additional embodiments, the deposition gas may be free of inert carrier gases, such as helium, argon or molecular nitrogen (N2), and other inert carrier gases. In yet additional embodiments, the deposition gas may be free of molecular hydrogen (H2). In yet further additional embodiments, the deposition gas is free of molecular oxygen (O2) or ozone (O3).
[0054] In further embodiments, a deposition gas can be provided to a substrate processing region of a processing chamber. In various embodiments, the deposition gas can pressurize the processing chamber to a pressure of less than or about 200 mTorr, less than or about 150 mTorr, less than or about 100 mTorr, less than or about 75 mTorr, less than or about 50 mTorr, less than or about 25 mTorr, or less.
[0055] The method 200 further includes generating a deposition plasma from the deposition gas at operation 210. In various embodiments, the deposition plasma may be characterized as a high density plasma. In further embodiments, the high density plasma may be characterized as greater than or about 1×10 11 ions / cm 3 , greater than or about 2×10 11 ions / cm 3 , greater than or about 3×10 11 ions / cm 3 , greater than or about 4×10 11 ions / cm 3 , greater than or about 5×10 11 ions / cm 3 , greater than or about 6×10 11 ions / cm 3 , greater than or about 7×10 11 ions / cm 3 , greater than or about 8×10 11 ions / cm 3 , greater than or about 9×10 11 ions / cm 3 , greater than or about 1×10 12 ions / cm3 In still further embodiments, the high density plasma can generate a deposition temperature in the processing chamber that is characterized as less than or about 200° C., less than or about 175° C., less than or about 150° C., less than or about 125° C., less than or about 100° C., or less.
[0056] The method 200 also includes depositing one or more silicon-oxygen-nitride-containing layers on the substrate in the processing chamber at operation 215. In various embodiments, the one or more layers may be deposited on an exposed surface of a substrate positioned in a substrate processing region of the processing chamber. In additional embodiments, the processing chamber may be an inductively coupled plasma chemical vapor deposition (ICP-CVD) processing chamber, such as Figure 1B In further embodiments, the gap between the plasma induction coil and the substrate can be characterized as greater than or about 5000 mils, greater than or about 6000 mils, greater than or about 7000 mils, greater than or about 8000 mils, greater than or about 9000 mils, greater than or about 10,000 mils, greater than or about 11,000 mils, greater than or about 12,500 mils, or greater. In further embodiments, the silicon-oxygen-nitride-containing material can be greater than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute, higher than or about / minute or higher deposition rate deposition.
[0057] In various embodiments, one or more silicon-oxygen-nitride-containing layers may be deposited as a single layer. In further embodiments, a single silicon-oxygen-nitride-containing layer may be characterized by less than or about Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately In additional embodiments, the one or more silicon-oxygen-nitride-containing layers may be deposited as a multilayer stack comprising two or more silicon-oxygen-nitride-containing layers. In yet additional embodiments, each of the silicon-oxygen-nitride-containing layers in the multilayer stack may be characterized by less than or about Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately In further embodiments, the multilayer stack of silicon-oxygen-nitride-containing layers may include more than or about two layers, more than or about three layers, more than or about four layers, more than or about five layers, more than or about six layers, more than or about seven layers, more than or about eight layers, more than or about nine layers, more than or about ten layers, or more layers. In still further embodiments, the multilayer stack of silicon-oxygen-nitride-containing layers may be characterized by less than or about Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Less than or approximately Or less overall thickness.
[0058] In some embodiments, a multilayer stack may be used in place of a single barrier layer of the same thickness to adjust one or more properties of the barrier layer, such as the type and magnitude of mechanical stress in the layer, and the refractive index of the layer, as well as other barrier layer properties. In some embodiments, the mechanical stress in the barrier layer may be characterized as a tensile stress of less than or about 200 MPa, less than or about 175 MPa, less than or about 150 MPa, less than or about 125 MPa, less than or about 100 MPa, less than or about 75 MPa, less than or about 50 MPa, less than or about 25 MPa, less than or about 10 MPa, or less. In additional embodiments, the mechanical stress in the barrier layer may be characterized as a compressive stress greater than or about -200 MPa, greater than or about -175 MPa, greater than or about -150 MPa, greater than or about -125 MPa, greater than or about -100 MPa, greater than or about -75 MPa, greater than or about -50 MPa, greater than or about -25 MPa, greater than or about -10 MPa, or greater. In more embodiments, the barrier layer may be characterized as having a neutral stress with substantially no tensile or compressive stress (i.e., a stress level of about 0 MPa). In further embodiments, the barrier layer may be characterized by a refractive index of less than or about 1.6, less than or about 1.59, less than or about 1.58, less than or about 1.57, less than or about 1.56, less than or about 1.55, less than or about 1.54, less than or about 1.53, less than or about 1.52, less than or about 1.51, less than or about 1.50, or less. In a multilayer stack of barrier layers, mechanical stress and refractive index may vary between layers.
[0059] In further embodiments, the deposited silicon-oxygen-nitride-containing layer can be characterized as a high quality layer. In still further embodiments, the deposited silicon-oxygen-nitride-containing layer can be characterized as having a density greater than or about 2.0 g / cm 3 , greater than or about 2.1 g / cm 3 , greater than or about 2.2 g / cm 3 , greater than or about 2.3 g / cm 3 , greater than or about 2.4 g / cm 3 , greater than or about 2.5 g / cm 3 or greater. The high density of the deposited silicon-oxygen-nitride-containing layer contributes to a low wet etch rate of the barrier layer. In various embodiments, the deposited layer may be characterized by less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about / minute, less than or about The barrier layer has a wet etch rate (WER) of 1000 nm / min or less. The high density and low wet etch rate characteristics of the barrier layer slow down the migration of oxygen and moisture through the layer. This allows a thinner barrier layer to provide the same level of oxygen and moisture protection as a thicker barrier layer made of a less dense material.
[0060] In yet further embodiments, the deposited silicon-oxygen-nitride-containing layer may be characterized as a silicon oxynitride (SiON) layer. In additional embodiments, the silicon oxynitride material in the SiON layer may be characterized by the formula SiO x N y , wherein x may be in the range of 0.25 to 1.9, and y may be in the range of 0.02 to 1.5. In further embodiments, the as-deposited SiON layer may be characterized by a hydrogen content of less than or about 5 mol%, less than or about 4 mol%, less than or about 3 mol%, less than or about 2 mol%, less than or about 1 mol%, or less.
[0061] The method 200 further includes exposing the deposited silicon-oxygen-nitride-containing layer to a treatment plasma at operation 220. In various embodiments, the treatment plasma may be formed of at least one nitrogen-containing gas that reacts with hydrophilic groups on an exposed surface of the silicon-oxygen-nitride-containing layer. In additional embodiments, these hydrophilic groups may include ionically charged groups, oxygen-containing groups, and hydroxyl-containing groups on the exposed surface of the layer. The reaction of these hydrophilic groups with nitrogen-containing species in the treatment plasma produces less hydrophilic nitrogen-containing groups and a silicon-oxygen-nitride-containing layer that is more resistant to oxygen and moisture transport through one or more layers.
[0062] In various embodiments, the exposed surface of the silicon-oxygen-nitride-containing layer treated with the treatment plasma may have more silicon-nitrogen bonds and fewer silicon-oxygen bonds than the surface of the as-deposited layer. In additional embodiments, the treated surface may be characterized by an increase in the amount of silicon-nitrogen bonds by greater than or about 10%, greater than or about 20%, greater than or about 30%, greater than or about 40%, greater than or about 50%, or more, as compared to the untreated surface of the as-deposited silicon-oxygen-nitride-containing layer. In further embodiments, the treated surface may be characterized by a reduction in the amount of silicon-oxygen bonds to less than or about 90%, less than or about 80%, less than or about 70%, less than or about 60%, less than or about 50%, or less of the silicon-oxygen bonds on the untreated surface of the as-deposited silicon-oxygen-nitride-containing layer.
[0063] In additional embodiments, the treatment plasma may be formed from one or more nitrogen-containing gases, such as nitrous oxide (N2O) and ammonia (NH3), among other nitrogen-containing gases. In further embodiments, the treatment plasma is silicon-free. In still further embodiments, the treatment plasma may be formed by terminating the flow of a silicon-containing gas in a deposition plasma while continuing to flow a nitrogen-containing gas. In various embodiments, the treatment plasma may be formed from a mixture of N2O and NH3 characterized by a flow ratio of N2O:NH3 of less than or about 10:1, less than or about 5:1, less than or about 2:1, less than or about 1:1, or less. In further embodiments, the treatment plasma may be formed from a treatment gas consisting of N2O. In still further embodiments, the treatment plasma may be formed from a mixture of NH3 and N2O characterized by a flow ratio of NH3:N2O of greater than or about 1:1, greater than or about 2:1, greater than or about 5:1, greater than or about 10:1, or greater. In additional embodiments, the treatment plasma may be formed from a treatment gas consisting of NH3. In various embodiments, the surface of the deposited silicon oxynitride-containing layer may be exposed to the treatment plasma for less than or about 60 seconds, less than or about 45 seconds, less than or about 30 seconds, less than or about 15 seconds, less than or about 10 seconds, less than or about 5 seconds, less than or about 4 seconds, less than or about 3 seconds, less than or about 2 seconds, less than or about 1 second, or less.
[0064] In various embodiments, the treated silicon-oxygen-nitride-containing layer has fewer hydrophilic groups, such as ionically charged groups, oxygen groups, and hydroxyl groups, as well as other hydrophilic groups. The reduction in the number of these hydrophilic groups on the surface of the treated silicon-oxygen-nitride-containing layer increases the layer's resistance to oxygen and moisture. In additional embodiments, the treated The silicon oxynitride-containing layer may be characterized by a relative humidity of less than or about 1×10 -3 g / m 2 days, less than or about 9×10 -4 g / m 2 days, less than or about 8×10 -4 g / m 2 days, less than or about 7×10 -4 g / m 2 days, less than or about 6×10 -4 g / m 2 days, less than or about 5×10 -4 g / m 2 days, less than or about 4×10 -4 g / m 2 days, less than or about 3×10 -4 g / m 2 days, less than or about 2×10 -4 g / m 2days, less than or about 1×10 -4 g / m 2 days or less water vapor transmission rate (WVTR).
[0065] The method 200 may also optionally include exposing the treated silicon-oxygen-nitride-containing layer to a surface plasma at operation 225. In various embodiments, the surface plasma treatment further reduces the free electrostatic charge present on the exposed surface of one or more treated layers. The reduced electrostatic charge level on the treated silicon-oxygen-nitride-containing layer further reduces the hydrophilicity of the layer. In additional embodiments, the surface plasma may be formed by one or more inert gases that do not react with chemical moieties on the exposed surface of the treated silicon-oxygen-nitride-containing layer. In yet additional embodiments, the inert gas may include molecular nitrogen (N2), helium (He), and argon (Ar), among other inert gases. In further embodiments, the treated silicon-oxygen-nitride-containing layer may be exposed to the surface plasma for less than or about 10 seconds, less than or about 7.5 seconds, less than or about 5 seconds, less than or about 2.5 seconds, less than or about 1 second, or less.
[0066] Figure 3 and Figure 4 Embodiments of exemplary structures 300 and 400 according to embodiments of the present technology are shown, respectively. Embodiments include substrates 302, 402 on which a silicon-oxygen-nitrogen barrier layer is formed. In various embodiments, the substrates 302, 402 may include silicon-containing materials, such as amorphous silicon, polycrystalline silicon, or crystalline silicon, as well as other silicon-containing materials. In further embodiments, the substrates 302, 402 may include inorganic dielectric materials, such as silicon oxide or silicon nitride, as well as other inorganic dielectric materials. In still further embodiments, the substrates 302, 402 may include organic polymer materials. In further embodiments, the exemplary structures 300 and 400 may include a layer or region of oxygen-sensitive materials 304, 404 positioned on the substrates 302, 402. In various embodiments, the oxygen-sensitive materials 304, 404 may include complex light-emitting organic molecules used in OLED displays, as well as other types of oxygen-sensitive materials.
[0067] exist Figure 3 In the illustrated embodiment, the silicon-oxygen-nitride-containing barrier layer 306 comprises a single layer positioned over the layer of oxygen-sensitive material 304. In various embodiments, the barrier layer 306 covers or encapsulates the oxygen-sensitive material 304 to prevent oxygen and moisture in the area above the barrier layer from contacting the oxygen-sensitive material. In further embodiments, the single layer 306 of the barrier material may be characterized by being greater than or about and less than or approximately In further embodiments, the barrier layer 306 may be characterized by a thickness of greater than or about 2.0 g / cm 3The density of the barrier layer 306 can be less than or about 100% at 40° C. and 100% humidity. / min wet etching rate and less than or about 9×10 -4 g / m 2 Water vapor transmission rate per day.
[0068] The improved oxygen and moisture resistance of barrier layer 306 can be accompanied by a refractive index that does not interfere with efficient transmission of light from the oxygen-sensitive luminescent material in layer 304. This can be achieved in part by a low refractive index of barrier layer 306. In various embodiments, barrier layer 306 can be characterized by a refractive index of less than or about 1.6.
[0069] Figure 4 Another embodiment of a barrier layer comprising a plurality of stacked layers 406a-406d of silicon-oxygen-nitride-containing materials is shown. In various embodiments, each of the layers 406a-406d may independently be less than or about and the total thickness of the layers may amount to less than or about In further embodiments, barrier layers 406a-406d may be characterized by a relative humidity of greater than or about 2.0 g / cm 3 density, less than or about In yet other embodiments, the barrier layers 406a to 406d may have a common characteristic of being less than or about 9×10 -4 g / m 2 In additional embodiments, barrier layers 406a-406d can also be independently characterized by a refractive index of less than or about 1.6. In still further embodiments, top barrier layer 406a can have the highest refractive index of all barrier layers 406a-406d.
[0070] In various embodiments, the exemplary structures 300 and 400 may further include a treated surface 308, 408, which may be a surface of the barrier layer 306, 406a opposite the surface of the contact layer 304, 404. In various embodiments, the treated surface 308, 408 may be characterized by a higher nitrogen content than the bulk of the barrier layer 306, 406a. In additional embodiments, the treated surface 308, 408 may be characterized by a higher hydrophobicity than the bulk of the barrier layer 306, 406a. In still further embodiments, the treated surface 308, 408 may be characterized by a thickness of less than or about 50 nm, less than or about 40 nm, less than or about 30 nm, less than or about 20 nm, less than or about 10 nm, less than or about 5 nm, or less.
[0071] Embodiments of the present technology provide oxygen and moisture barriers with reduced water vapor transmission rates at reduced barrier thickness and reduced refractive index. This permits incorporation of thinner barrier layers into electronic products (such as electronic displays) with smaller device sizes and higher device densities. Among other benefits, thinner barrier layers enable reduced device sizes to produce higher resolution, more flexible, and brighter displays. Additionally, the improved oxygen and moisture resistance of the present silicon-oxygen-nitride-containing barrier layers can increase the operating life of electronic products incorporating the barrier layers.
[0072] In the foregoing description, for the purpose of explanation, numerous details are set forth in order to provide an understanding of various embodiments of the present technology. However, it will be apparent to one skilled in the art that certain embodiments may be practiced without some of these details or with additional details.
[0073] Several embodiments have been disclosed, and those skilled in the art will recognize that various modifications, alternative configurations, and equivalents may be used without departing from the spirit of the embodiments. Additionally, a variety of well-known processes and elements are not described in order to avoid unnecessary confusion of the present technology. Therefore, the above description should not be considered to limit the scope of the present technology.
[0074] Where a range of values is provided, it is understood that each intermediate value between the upper and lower limits of the range is specifically disclosed, unless the context clearly indicates otherwise, up to the smallest fraction of the unit of the lower limit. Any narrower range between any stated value or unstated intermediate value and any other stated value or intermediate value within the stated range is contemplated. The upper and lower limits of those smaller ranges may be independently included in or excluded from the range, and each range in which any one, none or both limits are included in the smaller range is also contemplated within the present technology, subject to any specifically excluded limits within the stated range. Where a stated range includes one or both of the limits, a range excluding either or both of those included limits is also contemplated.
[0075] As used herein and in the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a material" includes a plurality of such materials and reference to "the precursor" includes reference to one or more precursors and equivalents thereof known to those skilled in the art, and so forth.
[0076] Furthermore, when used in this specification and the appended claims, the words “comprise,” “comprising,” “contain,” “containing,” “include,” and “including” are intended to specify the presence of stated features, integers, components, or operations, but they do not preclude the presence or addition of one or more other features, integers, components, operations, actions, or groups.
Claims
1. A processing method, comprising: flowing a deposition gas into a substrate processing region of a processing chamber, wherein the deposition gas comprises a silicon-containing gas and a nitrogen-containing gas; generating a deposition plasma from the deposition gas in the substrate processing region; depositing a silicon-oxygen-nitride-containing layer on a substrate from the deposition plasma; and The surface of the silicon-oxygen-nitride-containing layer is exposed to a treatment plasma to form a treated silicon-oxygen-nitride-containing layer having a treated surface with increased silicon-nitrogen bonds and reduced silicon-oxygen bonds, wherein the treatment plasma is formed from a nitrogen-containing gas and is silicon-free.
2. The process of claim 1, wherein the silicon-oxygen-nitride-containing layer is characterized by less than or about Thickness.
3. The process of claim 1, wherein the silicon-containing gas comprises silane and the nitrogen-containing gas comprises nitrous oxide.
4. The process of claim 1 wherein the deposition gas further comprises ammonia.
5. The process of claim 1 wherein the deposition plasma is characterized by greater than or about 1×10 11 ions / cm 3 The method further comprises: providing an ion density of at least 100° C. and wherein the silicon-oxygen-nitride-containing layer deposited on the substrate is characterized by a deposition temperature of less than or about 100° C.
6. The method of claim 1, wherein the treated silicon-oxygen-nitride-containing layer is characterized by less than or about The wet etching rate.
7. The method of claim 1, wherein the treated silicon-oxygen-nitride-containing layer is characterized by a relative humidity of greater than or about 2.1 g / cm 3 density.
8. The process of claim 1, wherein the treated silicon-oxygen-nitride-containing layer is characterized by a refractive index of less than or about 1.
6.
9. A processing method, comprising: A first silicon-oxygen-nitride-containing layer is deposited on the substrate, wherein the first silicon-oxygen-nitride-containing layer is characterized by less than or about Thickness; At least one additional silicon-oxygen-nitride-containing layer is deposited on the first silicon-oxygen-nitride-containing layer to form a multilayer stack of silicon-oxygen-nitride-containing layers, wherein the multilayer stack is characterized by less than or about thickness; and The top surface of the multilayer stack is exposed to a treatment plasma to form a treated multilayer stack, wherein the treatment plasma is formed from a nitrogen-containing gas and is silicon-free.
10. The process of claim 9 wherein the first silicon-oxygen-nitride-containing layer and the at least one additional silicon-oxygen-nitride-containing layer are deposited using a deposition plasma characterized by a temperature greater than or about 1×10 11 ions / cm 3 ion density.
11. The processing method of claim 10 wherein the deposition plasma is generated from a deposition gas comprising a silicon-containing gas and a nitrogen-containing gas.
12. The process of claim 9, wherein the processed multilayer stack is characterized by a refractive index of less than or about 1.
6.
13. The process of claim 9, wherein the processed multilayer stack is characterized by less than or about The wet etching rate.
14. The processing method of claim 9 wherein said nitrogen-containing gas in said processing plasma comprises ammonia.
15. A structure comprising: substrate; and at least one silicon-oxygen-nitride-containing layer, the at least one silicon-oxygen-nitride-containing layer being positioned on the substrate, wherein the at least one silicon-oxygen-nitride-containing layer is characterized by less than or about A thickness of less than or about 1.6, a refractive index of less than or about 1.6, and a The wet etching rate.
16. The structure of claim 15, wherein the at least one silicon-oxygen-nitride-containing layer is a single silicon-oxygen-nitride-containing layer.
17. The structure of claim 15, wherein the at least one silicon oxynitride-containing layer comprises at least two layers of silicon oxynitride-containing material, and wherein each of the at least two layers is characterized by less than or about Thickness.
18. The structure of claim 17, wherein the at least two layers of silicon-oxygen-nitride-containing material include a top layer characterized by a stress level different from other layers of the silicon-oxygen-nitride-containing material.
19. The structure of claim 15, wherein the at least one silicon-oxygen-nitride-containing layer is characterized by a relative humidity of greater than or about 2.1 g / cm 3 density.
20. The structure of claim 15 wherein the at least one silicon oxynitride containing layer comprises silicon oxynitride.