Preparation method of chitosan-citral-zinc tannate particles with anti-vibrio activity
Through Schiff base and complexation reaction, combined with supercritical high-pressure homogenization technology, chitosan-citral-zinc tannate particles were prepared, which solved the problems of citral instability and limited application, and realized its biological system The improvement of stability and anti-Vibiral activity in the pharmaceutical field have expanded the scope of application.
Patent Information
- Application Number
- CN202411006861.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
Citral is unstable, easy to decompose and insoluble in water, which limits its application in the field of biomedicine. There are few studies on antibacterial treatments on chitosan-citral-tanninate complexes, making it difficult to expand its application field.
Chitosan-citral-zinc tanninate particles were prepared by using Schiff base and complexation reaction, combined with supercritical high-pressure homogenization technology, to improve the stability of citral and enhance its anti-Vibiral activity.
It has achieved the improvement of citral stability and enhanced anti-vibrio activity, expanded its application field, and its application potential in food, medicine and other fields, and met the safety requirements of food additives.
Smart Images

Figure CN118948890A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedicine, and in particular relates to a method for preparing chitosan-citral-zinc tannate microparticles with anti-vibrio activity. Background Art
[0002] Chitosan is a natural cationic alkaline amino polysaccharide, rich in amino and hydroxyl groups, with good biological activity, safety, non-toxicity, low cost, and biodegradability, which provides the possibility of introducing active functional substances and constructing stimulus-responsive biomaterials. In addition, chitosan also has a broad-spectrum antibacterial property, and has a significant inhibitory effect on a variety of microorganisms such as bacteria and fungi. Its antibacterial mechanism mainly includes destroying cell membrane permeability, affecting bacterial cell phospholipid and protein synthesis, and chelating metal ions.
[0003] Citral is also known as 3,7-dimethyl-2,6-octadienal, with a molecular formula of C 10 H 16 O, colorless or light yellow liquid, with lemon aroma, no optical rotation, there are two cis-trans isomers, geranial and neral, the content ratio is about 2:3. Citral is widely found in plants such as Litsea cubeba, lemongrass, and Ocimum tiliaceum. In my country, natural citral is usually extracted from Litsea cubeba. The citral content in Litsea cubeba essential oil is the highest, reaching 85%. Citral has antibacterial and anti-inflammatory functions, and has a good inhibitory effect on the growth and reproduction of bacteria and fungi. In recent years, more and more studies have used embedding technology to prepare citral into sustained-release preparations. This preparation can improve the stability of citral, protect citral from the influence of the external environment, and at the same time play a sustained-release role and prolong the action time, which is of great significance to broaden the application range of citral.
[0004] Tannin acid contains abundant catechol groups and catechol derivatives, which can inhibit the growth of various microorganisms such as bacteria, fungi, yeasts, and Gram-positive / negative bacteria. The catechol groups contain a large number of hydroxyl groups, which can produce various strong interactions and have super strong adhesion.
[0005] Zinc salts have the advantages of broad spectrum, safety, low resistance and durability. In addition, zinc nanoparticles are easy to form complexes with amino and hydroxyl groups on chitosan. Zinc nanoparticles can also be used as animal zinc nutritional supplements to improve animal immunity.
[0006] As a natural antibacterial material, natural citral has great application potential and promotion value. However, citral is unstable, easily decomposed and insoluble in water, which limits its application range. Its derivatives and biological activities have attracted extensive attention from scientists, opening up new ways to develop new biopharmaceuticals to replace antibiotics, but there are relatively few studies on the antibacterial effects of chitosan-citral-zinc tannate complexes. Summary of the invention
[0007] In order to solve the above technical problems, the present invention proposes a method for preparing chitosan-citral-tannic acid zinc microparticles with anti-Vibrio activity, using chitosan, citral, tannic acid and zinc salt as main raw materials, utilizing Schiff base and complex reaction, and adopting supercritical high-pressure oxygen isolation homogenization to prepare chitosan-citral-tannic acid zinc microparticles with improved stability of citral and anti-Vibrio activity, so as to achieve the purpose of expanding its application field.
[0008] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0009] The invention discloses a method for preparing chitosan-citral-zinc tannate microparticles with antivibrio activity. The method uses chitosan, citral, tannic acid and zinc salt as raw materials, utilizes Schiff base reaction and complex reaction, and adopts supercritical high pressure homogenization to prepare chitosan-citral-zinc tannate microparticles with antivibrio activity.
[0010] Furthermore, the method for preparing the chitosan-citral-zinc tannate microparticles having anti-Vibrio activity comprises the following steps:
[0011] (1) slowly dropping the citral solution into the acid-containing chitosan dispersion, stirring at a constant temperature of 40 to 60° C. until the color of the system dispersion changes from white to a stable yellow, thereby obtaining a chitosan-citral dispersion;
[0012] (2) slowly dropping the zinc salt dispersion containing nano zinc into the tannic acid dispersion, and slowly stirring to prepare a tannic acid-zinc dispersion;
[0013] (3) The tannic acid-zinc dispersion obtained in the above step (2) is slowly added dropwise to the chitosan-citral dispersion obtained in step (1), stirred at a constant temperature of 40-60° C., and homogenized by supercritical high pressure for 1 hour. Since chitosan and tannic acid are macromolecular substances and difficult to disperse, high-speed shearing is used to achieve uniform dispersion of the microparticles. After the system is stabilized, freeze-drying is performed to obtain chitosan-citral-tannic acid zinc microparticles.
[0014] Furthermore, in step (1), the mass percentage of citral contained in the citral solution is 1% to 5%, and the solvent used is ethanol; the mass percentage of chitosan contained in the acid-containing chitosan dispersion is 10% to 30%, the solvent used is ethanol, and the acid contained is acetic acid, and the mass percentage of acetic acid is 1% to 2%.
[0015] Furthermore, in step (1), the volume ratio of the citral solution to the acid-containing chitosan dispersion is 1:1 to 1:5.
[0016] Furthermore, in step (2), the zinc salt contained in the zinc salt dispersion containing nano-zinc is any one of zinc acetate, zinc sulfate, zinc gluconate and zinc chloride, the zinc nanoparticles contained in the zinc salt account for 1wt% to 5wt% of the total mass percentage of the mixture of zinc salt and tannic acid, and the solvent used is ethanol.
[0017] Furthermore, the dosage ratio of the zinc salt dispersion containing nano zinc to the tannic acid dispersion is 1:1 to 5:1.
[0018] Furthermore, in step (3), the usage ratio of tannic acid-zinc dispersion to chitosan-citral dispersion is 1:2 to 1:10.
[0019] Further, in step (3), supercritical CO 2 The conditions of the extraction instrument are: CO 2 Heater 45℃~50℃, MMV Heater 100℃, Vessel Heater 45℃~50℃, CO 2 Pump Pressure 250~300Bar.
[0020] Furthermore, chitosan-citral-zinc tannate microparticles with anti-Vibrio activity are prepared by any of the above methods.
[0021] Furthermore, the chitosan-citral-zinc tannate microparticles with anti-Vibrio activity have a citral release rate of 51.17% and a citral content in the minimum inhibitory concentration of less than 20 μg / ml.
[0022] Compared with the prior art, the advantages of the present invention are as follows:
[0023] 1) The present invention uses environmentally friendly, biodegradable chitosan (CS), citral (CT) and tannic acid (TA) as main raw materials, as well as a broad-spectrum, safe and non-resistant zinc salt, to prepare CS-CT Schiff base by supercritical CO 2The extraction and separation technology provides a high-pressure, low-temperature and oxygen-isolated environment for the preparation of sustained-release preparations, preventing citral from denaturing due to high temperature and oxidation during the reaction. CS-CT and TA-Zn are homogenized under high pressure to improve the stability of the antibacterial component - citral, protect the antibacterial component - citral from the influence of the external environment, and at the same time play a sustained-release role.
[0024] 2) The present invention can release citral by triggering cleavage through an acidic solution system, which can effectively ensure the stability of citral and maintain the original functional activity of citral, and can meet the requirements of scientific research related biological activity experiments. The raw materials used also meet the requirements of Chinese food additive raw materials. The solvents used are all low-toxic solvents. The preparation method is simple, the process stability is good, and it can be applied to food, medicine and other fields. In addition, the present invention shows a release difference over time under pH 1.5 conditions, and the release of active substances can be regulated according to actual needs to inhibit bacteria.
[0025] 3) The citral release rate of the chitosan-citral-zinc tannate complex prepared by the present invention is 51.17%, and the citral content in the minimum inhibitory concentration is about 20 μg / ml, and its antibacterial effect is much better than the minimum inhibitory concentration of 100 μg / ml of citral monomer in inhibiting Vibrio parahaemolyticus.
[0026] 4) The composite prepared by the present invention has good Vibrio inhibition activity and can be developed into food or feed additives, antibacterial agents, etc.; and the composite has rich zinc content and can also be used as an animal zinc nutritional supplement to improve animal immunity, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The scanning electron micrographs of chitosan and chitosan-citral-zinc tannate microparticles;
[0028] Figure 2 The energy spectrum analysis diagram of chitosan and chitosan-citral-tannic acid zinc particles;
[0029] Figure 3 This is the infrared analysis diagram of chitosan-citral-zinc tannate microparticles;
[0030] Figure 4 is the X-ray diffraction analysis diagram of chitosan-citral-zinc tannate microparticles;
[0031] Figure 5 This is a graph showing the release effects of chitosan-citral-zinc tannate microparticles at different time periods in simulated gastric fluid;
[0032] Figure 6 This is the antibacterial graph of chitosan-citral-tannic acid zinc microparticles. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.
[0034] Example 1
[0035] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0036] (1) Preparation of chitosan-citral dispersion
[0037] 50 mL of 0.02 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 45°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0038] (2) Preparation of Tannic Acid-Zinc Dispersion
[0039] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 1% zinc nanoparticles by mass in 10 mL of ethanol at 40°C.
[0040] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0041] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at a constant temperature of 40 °C, supercritical high pressure homogenization was performed for 1 h. The supercritical parameters were set as follows: CO 2 The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 250Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve the purpose of uniform dispersion of particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0042] The morphology of the prepared chitosan-citral-zinc tannate microparticles was observed by scanning electron microscopy. Figure 1 As shown in the figure, chitosan and citral sustained-release preparations have obvious morphological differences. Chitosan has a relatively smooth surface, while citral sustained-release preparations have a porous and rough surface due to Schiff base reaction and the addition of tannic acid-zinc. It is inferred that Schiff base reaction and metal chelation change the internal force of the polymer and thus change the surface roughness. From the distribution characteristics of elements, such as Figure 2 As shown, the distribution of C, O, N and Zn elements on the sample surface is relatively uniform, and it can be inferred that the prepared sustained-release preparation has good uniformity.
[0043] The chemical structure of the chitosan-citral-zinc tannate microparticles prepared according to the method of Example 1 was determined by Fourier transform infrared spectrometer. Figure 3 As shown in the figure, the CS, CS-CT and CS-CT-TA-Zn samples are located at 3356 cm -1 The characteristic broad peak is the multiple absorption peaks of -OH and -NH stretching vibration superposition, 2870cm -1 The characteristic peaks come from -CH 2 Contraction vibration. 1590cm -1 and 1655cm -1 The 1376cm-1 is the bending vibration peak of chitosan amide II (NH) and the stretching vibration peak of amide I bond (C=O). -1 、1148cm -1 and 1023cm -1 The characteristic absorption peaks of 890 cm-1 correspond to the contraction vibrations of COC, CO and CH on the chitosan main chain. -1 The absorption peak of is from the contraction vibration of NH. Meanwhile, compared with CS, CS-CT and CS-CT-TA-Zn have a peak at 1644 cm -1 A new absorption peak appears, which belongs to the Schiff base (C=N) of CS-CT, and the C=N band in CS-CT-TA-Zn becomes weaker, but no new absorption peak appears, indicating that no chemical reaction occurs among the components, and the main reason for the movement of the characteristic peak position is due to electrostatic interaction and hydrogen bonding. In general, the FTIR spectrum shows that the characteristic peaks of CS, CS-CT and CS-CT-TA-Zn raw materials still exist, indicating that the infrared spectrum of the mixture is that the four raw materials are combined through electrostatic interaction and hydrogen bonding to form a stable structure, and no new chemical groups are formed.
[0044] The crystallinity of the chitosan-citral-zinc tannate microparticles prepared according to the method of Example 1 was measured by X-ray diffractometer. Figure 4As shown in the figure, the XRD diffraction patterns of the three samples of CS, CS-CT and CS-CT-TA-Zn show a gentle and a sharp diffraction peak near the diffraction angle 2θ of 11.32° and 20.01°, which are the characteristic diffraction peaks of chitosan type I and type II crystals, respectively, and can characterize the degree of crystallization of chitosan. The intensity of the diffraction peak at 2θ angle of 20.01° is weakened, indicating that the Schiff base reaction and the addition of tannic acid-zinc lead to a decrease in the number of free amino groups in the chitosan chain segment, destroying the order of the molecular chain; the crystallization peak at 2θ angle of 11.32° is weakened, indicating that the groups introduced after the Schiff base reaction destroy the microcrystalline structure of chitosan and reduce the crystallinity of the polymer; the crystallization peaks at 2θ angles of 10.08° and 15.07° are enhanced, indicating that the introduced tannic acid-zinc groups increase the microcrystalline structure of chitosan and improve the crystallinity of the crystals. These results confirm that the combination of chitosan and citral will destroy the original hydrogen bonding force, change the crystallization properties, and cause the peak position to become wider and weaker. However, the addition of tannic acid-zinc can increase the crystallization properties of the sustained-release preparation and improve the crystallinity of the sustained-release preparation.
[0045] The chitosan-citral-zinc tannate microparticles prepared according to the method of Example 1 were placed in simulated gastric fluid (pH 1.5, 37° C.), and the release of citral was determined by GC-MS. The chromatographic peak retention time was used for qualitative analysis, and the peak area was used for relative quantitative analysis. Figure 5 As shown. According to the standard curve calculation, under the conditions of pH 1.5 and 37°C, the content of citral released by the sustained-release preparation first increased, reaching a maximum release rate of 51.17% at 90 minutes, and then decreased. This shows that the release of citral by the microparticles is best within a certain time range, and the optimal time is 90 minutes.
[0046] Example 2
[0047] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0048] (1) Preparation of chitosan-citral dispersion
[0049] 50 mL of 0.01 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 50°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0050] (2) Preparation of Tannic Acid-Zinc Dispersion
[0051] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 2% zinc nanoparticles by mass in 10 mL of ethanol at 50°C.
[0052] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0053] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at 50 °C, the mixture was homogenized by supercritical high pressure for 1 h. The supercritical parameters were set as follows: CO 2 The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 250Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve the purpose of uniform dispersion of particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0054] Example 3
[0055] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0056] (1) Preparation of chitosan-citral dispersion
[0057] 50 mL of 0.05 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 60°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0058] (2) Preparation of Tannic Acid-Zinc Dispersion
[0059] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 5% zinc nanoparticles by mass in 10 mL of ethanol at 60°C.
[0060] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0061] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at a constant temperature of 45 °C, supercritical high pressure homogenization was performed for 1 h. The supercritical parameters were set as follows: CO 2 The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 250Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve the purpose of uniform dispersion of particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0062] Example 4
[0063] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0064] (1) Preparation of chitosan-citral dispersion
[0065] 50 mL of 0.02 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 45°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0066] (2) Preparation of Tannic Acid-Zinc Dispersion
[0067] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 1% zinc nanoparticles by mass in 20 mL of ethanol at 45°C.
[0068] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0069] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at a constant temperature of 45 °C, supercritical high pressure homogenization was performed for 1 h. The supercritical parameters were set as follows: CO 2 The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 280Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve uniform dispersion of the particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0070] Example 5
[0071] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0072] (1) Preparation of chitosan-citral dispersion
[0073] 50 mL of 0.02 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 45°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0074] (2) Preparation of Tannic Acid-Zinc Dispersion
[0075] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 1% zinc nanoparticles by mass in 50 mL of ethanol at 45°C.
[0076] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0077] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at a constant temperature of 45 °C, supercritical high pressure homogenization was performed for 1 h. The supercritical parameters were set as follows: CO 2 The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 280Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve uniform dispersion of the particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0078] Example 6
[0079] The preparation method of the chitosan-citral-zinc tannate microparticles of the present embodiment comprises the following steps:
[0080] (1) Preparation of chitosan-citral dispersion
[0081] 50 mL of 0.02 g / mL citral-ethanol solution was slowly added dropwise to 50 mL of 0.1 g / mL chitosan-ethanol dispersion, placed in a magnetic stirring water bath, and stirred at a constant temperature of 45°C until the color of the system dispersion deepened from white to a stable yellow to obtain a chitosan-citral dispersion.
[0082] (2) Preparation of Tannic Acid-Zinc Dispersion
[0083] A tannic acid-zinc dispersion was prepared by slowly stirring 35 mg / mL tannic acid and 1% zinc nanoparticles by mass in 50 mL of ethanol at 45°C.
[0084] (3) Preparation of chitosan-citral-zinc tannate microparticles
[0085] 10 mL of tannic acid-zinc dispersion was slowly added dropwise to the chitosan-citral dispersion, and then placed in a magnetic stirring water bath. After stirring overnight at a constant temperature of 45 °C, supercritical high pressure homogenization was performed for 1 h. The supercritical parameters were set as follows: CO 2The heater temperature is 45°C, the MMV heater temperature is 100°C, the reactor temperature is 45°C, and the carbon dioxide pump pressure is 300Bar. Since chitosan and tannic acid are macromolecular substances and are not easy to disperse, high-speed shearing is used to achieve uniform dispersion of the particles. After the system is stable, chitosan-citral-tannic acid zinc particles are obtained by freeze drying.
[0086] According to the data of Examples 1 to 6, in the test results of pH responsiveness and stable release of citral, the citral release rates of Examples 1, 2, and 3 showed a downward trend, and the release rate of Example 1 was the highest, which was 51.17%, indicating that the relative saturated combination can be achieved when the ratio of citral-ethanol solution to chitosan-ethanol dispersion is changed to 1:5, which is the most cost-effective combination ratio, and as the reaction temperature increases, the chitosan-citral-tannic acid zinc microparticle release rate value also decreases, indicating that the release rate of Implementation Case 1 is more stable than that of other cases; in the change of the dosage ratio of chitosan-citral dispersion to tannic acid-zinc dispersion, there is no significant difference in the values between the groups of Examples 1, 4, 5 and 6, but as the supercritical reaction temperature increases, there will be a slight downward trend, indicating that the dosage ratio of chitosan-citral dispersion to tannic acid-zinc dispersion in Example 1 is the most cost-effective; in the anti-Vibrio test results, the minimum inhibitory concentrations of Examples 1, 4, 5 and 6 are lower than those of Examples 2 and 3, indicating that the anti-Vibrio properties of the first four are stronger than the latter two.
[0087] The minimum inhibitory concentration was determined by the two-fold dilution method and the plate count method, and the minimum bactericidal concentration was determined by the plate coating method. Figure 6 The sustained-release preparation solution was mixed with TSB culture medium (10 5 -10 6 CFU / mL) was inoculated with Vibrio parahaemolyticus for culture, incubated at 30±0.5℃ for 1d, stirred at 150r / min, and MIC was obtained. 0.1mL was drawn from all the clear test tubes in the MIC test and evenly coated on TSB solid culture medium. After culturing at 30±0.5℃ for 24h, the counts were observed and the concentration of citral sustained-release preparation corresponding to the culture medium with less than 5 colonies was taken as MBC. Chitosan-citral-tannic acid zinc microparticles had a significant inhibitory effect on Vibrio parahaemolyticus, with a minimum inhibitory concentration of 256μg / ml and a minimum bactericidal concentration of 512μg / ml. (Reference standard: GB4789.7-2013: National Food Safety Standard: Food Microbiology Inspection: Vibrio parahaemolyticus Inspection), converted in proportion, the calculation formula is as follows. The amount of citral contained in it is about 20μg / ml, and its antibacterial effect is better than the minimum inhibitory concentration of 100μg / ml of citral monomer to inhibit Vibrio parahaemolyticus.
[0088]
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity, characterized in that: Chitosan-citral-tannic acid zinc microparticles with antivibrio activity were prepared using chitosan, citral, tannic acid and zinc salt as raw materials, using Schiff base reaction and complex reaction, and adopting supercritical high pressure homogenization.
2. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 1, characterized in that: The following steps are involved: (1) slowly dropping the citral solution into the acid-containing chitosan dispersion, stirring at a constant temperature of 40 to 60° C. until the color of the system dispersion changes from white to a stable yellow, thereby obtaining a chitosan-citral dispersion; (2) slowly dropping the zinc salt dispersion containing nano zinc into the tannic acid dispersion, and slowly stirring to prepare a tannic acid-zinc dispersion; (3) slowly adding the tannic acid-zinc dispersion obtained in the above step (2) to the chitosan-citral dispersion obtained in step (1), stirring at a constant temperature of 40 to 60° C., homogenizing by supercritical high pressure for 1 hour, and freeze-drying after the system is stabilized to obtain chitosan-citral-tannic acid zinc microparticles.
3. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: In step (1), the mass percentage of citral contained in the citral solution is 1% to 5%, and the solvent used is ethanol; the mass percentage of chitosan contained in the acid-containing chitosan dispersion is 10% to 30%, the solvent used is ethanol, and the acid contained is acetic acid, and the mass percentage of acetic acid is 1% to 2%.
4. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: In step (1), the volume ratio of the citral solution to the acid-containing chitosan dispersion is 1:1 to 1:
5.
5. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: In step (2), the zinc salt contained in the zinc salt dispersion containing nano zinc is any one of zinc acetate, zinc sulfate, zinc gluconate and zinc chloride, the zinc nanoparticles contained in the zinc salt account for 1wt% to 5wt% of the total mass percentage of the mixture of zinc salt and tannic acid, and the solvent used is ethanol.
6. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: The dosage ratio of the zinc salt dispersion containing nano zinc to the tannic acid dispersion is 1:1 to 5:
1.
7. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: In step (3), the usage ratio of tannic acid-zinc dispersion to chitosan-citral dispersion is 1:2 to 1:
10.
8. The method for preparing chitosan-citral-zinc tannate microparticles having antivibrio activity according to claim 2, characterized in that: In step (3), the conditions of the supercritical CO2 extractor are: CO2 Heater 45℃~50℃, MMV Heater 100℃, Vessel Heater 45℃~50℃, CO2 pump Pressure 250~300Bar.
9. Chitosan-citral-zinc tannate microparticles having anti-Vibrio activity prepared by the method of any one of claims 1 to 8.
10. The chitosan-citral-zinc tannate microparticles with anti-Vibrio activity according to claim 9, wherein the citral release rate is 51.17% and the citral content in the minimum inhibitory concentration is less than 20 μg / ml.
Citation Information
Cited By
Amphiphilic chitosan oligosaccharide as well as preparation method and application thereof
CN119874962A