Photocatalytic material for treating nonyl phenol and nonyl phenol derivative wastewater as well as preparation method and process of photocatalytic material

By using photocatalytic materials with crystalline SiO2 cores and multi-interface nanoscale SrTiO3/TiO2 heterojunction shells, combined with ultraviolet light and ozone oxidation processes, nonylphenol and its derivatives are difficult to remove in conventional photocatalytic systems. The problem has achieved efficient oxidative degradation and mineralization effects.

CN118949967AInactive Publication Date: 2024-11-15AOP ENVIRONMENTAL TECH (YANCHENG) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410959964.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nonylphenol and its derivatives are difficult to be adsorbed and completely mineralized in conventional photocatalytic systems, making it difficult to completely remove water pollution.

Method used

The photocatalytic material consisting of a crystalline SiO2 core and a thick layer of SrTiO3/TiO2 coated on its surface and a multi-interface nanoscale SrTiO3/TiO2 heterojunction shell, the preparation method includes amorphous SiO2 microspheres, high-temperature calcination, and water. The materials are formed by thermal preparation and combined with ultraviolet light and ozone oxidation processes for oxidation and degradation.

Benefits of technology

Improve the light absorption efficiency and bulk carrier transfer path of photocatalytic materials, significantly improve the mineralization efficiency of nonylphenol and its derivatives, and can be combined with ozone open-ring chain break reaction and later radical oxidation in the early stage. The mineralization rate is achieved by 98%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949967A_ABST
    Figure CN118949967A_ABST
Patent Text Reader

Abstract

The invention relates to a photocatalytic material for treating nonyl phenol and nonyl phenol derivative wastewater, a preparation method and a process. Wherein the photocatalytic material is composed of a crystalline SiO2 inner core, a layer of thick-layer SrT iO3 / T iO2 shell and a layer of multi-interface nanoscale SrT iO3 / T iO2 shell, and the chemical formula of the photocatalytic material is SiO2 (at) SrT iO3 / T iO2; the preparation method comprises the following steps: firstly preparing amorphous SiO2 microspheres wrapped by single-layer TiO2, calcining crystal SiO2 at high temperature, then preparing thick-layer SrT O < 3 > / T O < 2 > in a hydrothermal manner, and then preparing the multi-interface nanoscale SrT O < 3 > / T O < 2 > shell in a manner of repeatedly coating thin-layer T O < 2 > and preparing SrT O < 3 > in a hydrothermal manner; wherein the process is a treatment process adopting ozone bubbling, ultraviolet light and a photocatalytic material in an initial degradation process, a catalyst process adopting photocatalysis, a photocatalytic material and an oxidizing agent in a middle and later degradation process, the initial reaction stage is a period when most organic matters are in a ring opening stage in the degradation process, and the degradation time is 0-0.5 h; the middle and later periods of the reaction are periods when most organic matters are in chain scission and mineralization periods in the degradation process, and the degradation time is 0.5-3 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of photocatalytic materials and wastewater treatment, and specifically relates to a photocatalytic material, preparation method and process for treating wastewater of nonylphenol and its derivatives. Background Art

[0002] In recent decades, with the rapid development of the global economy and the continuous progress of society, environmental problems, especially water pollution, have become increasingly serious. New pollutants that are widely distributed in the water environment can bioaccumulate through the food chain, posing a significant risk to human health. As an efficient advanced oxidation technology, photocatalysis has been widely studied in wastewater treatment because of its mild reaction conditions, strong oxidation ability, and ability to remove most organic pollutants.

[0003] The photocatalytic system oxidizes organic pollutants through the holes in the valence band of the photocatalytic material or the strong oxidizing free radicals in the solution. However, nonylphenol and its derivatives have the characteristics of low concentration in water and high hydrophobicity, which makes it difficult to be adsorbed on the surface of the material and difficult to react with the oxidizing free radicals in the water. Therefore, it is extremely difficult to completely mineralize them in conventional photocatalytic systems. Therefore, it is of great significance to find an effective photocatalytic material and applicable process to completely remove nonylphenol and its derivatives from water. Summary of the invention

[0004] The present application aims to solve the problems mentioned in the above background technology.

[0005] The present invention discloses a photocatalytic material for treating wastewater of nonylphenol and its derivatives: the photocatalytic material is composed of crystalline SiO 2 The core and the coating are in crystalline SiO 2 A thick layer of SrTiO on the surface of the core 3 / TiO 2 and a multi-interface nanoscale SrTiO 3 / TiO 2 The composition of the heterojunction shell is SiO 2 @SrTiO 3 / TiO 2 .

[0006] The photocatalytic material preparation method of the present invention comprises: firstly preparing a thick layer of TiO 2 Encapsulated amorphous SiO 2 Microspheres, high temperature calcined crystalline SiO 2 After that, thick layer SrTiO was prepared hydrothermally. 3 / TiO 2 , and then repeat the coating with thin layer of TiO 2 Hydrothermal preparation of SrTiO 3 Preparation of multi-interface nanoscale SrTiO 3 / TiO2 Heterojunction shell.

[0007] Furthermore, wherein the TiO 2 is anatase type; wherein the SiO 2 The microsphere size is 0.1-10 μm;

[0008] Furthermore, S1: amorphous SiO 2 Preparation of microspheres: SiO 2 Microspheres, ethanol, ammonia, water, and chloride salt are fully mixed, and then the ethanol solution containing Si ester compound is slowly added while stirring, and maintained at 20-50°C for 1-3h, and then white powder is separated and dried;

[0009] S2: single layer TiO 2 Preparation of the shell, the SiO 2 The microspheres are fully mixed with ethanol and ammonia water, and the Ti-containing ester compound is added during stirring. The mixture is maintained at 40-60°C for 24-48 hours, and then the white powder is separated and dried. The dried powder is then calcined at high temperature to obtain SiO 2 @TiO 2 ;

[0010] S3: Crystalline SiO 2 @TiO 2 Preparation of SiO 2 @TiO 2 After being evenly mixed with alkaline earth chloride and water, it was shaken for 0.5-1h, dried, and calcined at high temperature for a certain period of time in an air atmosphere to obtain crystalline SiO 2 @TiO 2 , wherein the alkaline earth chloride is CaCl 2 、SrC l 2 、BaC l 2 and one or more of its corresponding hydrates. Preferably, the molar amount of alkaline earth chloride is 0.01-0.5 times the molar amount of the material obtained from S2, the calcination temperature is preferably 800-1200°C, and the calcination time is preferably 3-8h.

[0011] S4: Thick layer SrTiO 3 / TiO 2 Preparation of crystalline SiO in S3 2 @TiO 2 The Sr-containing compound, NaOH and deionized water are fully stirred and mixed in a beaker, and then transferred to a hydrothermal kettle. After being maintained at a certain temperature for a period of time, a white powder is separated and dried; wherein the Sr-containing compound is Sr(OH) 2 、Sr(NO3)2 、Sr(CO3) 2 and one or more of its corresponding hydrates, preferably, the molar amount of the Sr-containing compound is 0.2-0.6 times the molar amount of the material obtained from S3. The hydrothermal temperature is preferably 150-200°C, and the hydrothermal time is preferably 12-24h.

[0012] S5: Multi-interface Nanoscale SrTiO 3 / TiO 2 The material obtained in S4 is prepared by repeating the operations of steps S2 and S4 alternately, and the SrTiO nanoparticles are formed by adjusting the hydrolysis time in S2 and the amount of the Sr-containing compound in S4. 3 / T i 2 Materials, namely, crystalline SiO 2 Core and multi-interface nanoscale SrTiO 3 / T i 2 Photocatalytic materials for heterojunction shells.

[0013] Further, in S1, the Si-containing ester compound is a silicate compound, preferably tetramethyl silicate or tetraethyl silicate; wherein the concentration of the ester compound in ethanol solution is 50-200 g / L, preferably 100-200 g / L; wherein the amount of ester compound added is 6-20 ml / h; wherein the ethanol concentration is not less than 95%, and the amount of ethanol used is 10-20 times, preferably 15-20 times, of the Si-containing ester compound added per hour; wherein the ammonia concentration is 25-28%, and the amount of ammonia used is 0.5-2 times, preferably 1-1.5 times, of the Si-containing ester compound added per hour; wherein the chloride salt is NaCl, KCl, CaCl 2 One or more of the above, the amount of chloride salt used is 0.005-0.02 times the amount of Si-containing ester compound added per hour; wherein SiO 2 The size of the spheres is 0.5-3 μm.

[0014] Further, in S2, the ester compound containing Ti is a titanate compound, preferably one or more of tetraethyl titanate, isopropyl titanate, and tetrabutyl titanate; wherein the amount of the Ti ester compound added is 0.5-2 times the molar amount of the material obtained from S1; wherein the ethanol concentration is not less than 95%, and the amount of ethanol used is 50-100 times the mass of the material obtained from S1; wherein the ammonia concentration is 25-28%, and the amount of ammonia used is 1-2 times the mass of the material obtained from S1;

[0015] Wherein, the calcination temperature is 500-800°C.

[0016] Furthermore, in the S2, TiO 2The layer thickness is 20-100nm, preferably 20-50nm; the multi-interface nanoscale SrTiO 3 / T i 2 The size of the heterojunction is 2-20nm.

[0017] The present invention discloses a photocatalytic process for treating wastewater containing nonylphenol and its derivatives. The process comprises adding the photocatalytic material, ultraviolet light and other oxides described above to the wastewater containing nonylphenol and its derivatives, and utilizing photocatalysis to carry out oxidation and degradation reaction.

[0018] Furthermore, the initial stage of the reaction is the period when most of the organic matter in the degradation process is in the ring-opening stage, preferably 0-0.5h; and the middle and late stages of the reaction are the period when most of the organic matter in the degradation process is in the chain breaking and mineralization stage, preferably 0.5-3h.

[0019] Furthermore, in the initial stage of the reaction, a dual oxidation treatment process of ozone and photocatalytic materials is adopted, and the ozone flow rate per minute is 0.1-0.5 times the amount of wastewater to be treated; in the middle and late stages of the reaction, a treatment process of adding photocatalytic materials and oxidants is adopted, and the oxidant is a chemical substance with strong oxidizing properties or the decomposition product has strong oxidizing properties, preferably persulfate or hydrogen peroxide.

[0020] Compared with the prior art, the present application has the following beneficial effects:

[0021] (1) The present application provides a crystalline SiO 2 Microsphere core and coated with crystalline SiO 2 A thick layer of SrTiO on the surface of the core 3 / TiO 2 and a multi-interface nanoscale SrTiO 3 / TiO 2 Photocatalytic materials for heterojunction shells. SiO 2 The backscattered light can be trapped in the lattice to produce a light confinement effect, and the light absorption path can be increased through forward scattering, thereby improving the light absorption efficiency. 2 , cristobalite SiO 2 It has higher light transmittance and refractive index, which significantly improves the photocatalytic efficiency of the material. 2 In the synthesis of SrTiO 3 When reducing SiO 2 dissolution, promoting Sr 2+ With TiO 2 Combined to form SrTiO 3 A thick layer of SrTiO 3 / TiO 2 Encapsulated in SiO 2The surface of the microspheres can reduce the burning of crystalline SiO 2 The outer layer is a multi-interface nanoscale SrTiO 3 / T i 2 , through a small amount of multiple synthesis method to form a small-size, multi-interface heterojunction, significantly shorten the bulk carrier transfer path and improve the photocatalytic performance of the material.

[0022] (2) The present application provides a photocatalytic process for treating wastewater containing nonylphenol and its derivatives. In the initial degradation process, a combination of ultraviolet light, photocatalyst and ozone is used for oxidation. The introduction of ozone has two beneficial effects: ① Ozone can directly react with the material to undergo a ring-opening and chain-breaking reaction, thereby reducing the hydrophobicity of nonylphenol and its derivatives, and facilitating the degradation of organic matter in water; ② Ozone bubbling is used to enhance mechanical disturbance, thereby increasing the probability of collision between pollutants and materials, promoting the adsorption of pollutants on the surface of materials, and further enhancing the degradation efficiency of nonylphenol and its derivatives in the initial stage of the reaction. In the mid- and late-stage degradation process, pollutants are decomposed into smaller molecular organic matter. At this time, the solubility and biodegradability of pollutants are greatly improved, and the use of free radical oxidation is more conducive to the mineralization of organic matter. Different processes are used in the early and mid- to late-stage to specifically degrade pollutants, significantly improving the mineralization efficiency of nonylphenol and its derivatives. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is SiO in the present invention 2 @SrT iO 3 / T i 2 SEM images of

[0024] Figure 2 is SiO in the present invention 2 @SrT iO 3 / T i 2 TEM images of

[0025] Figure 3 It is a diagram of TOC removal of nonylphenol by photocatalytic materials in Example 2 of the present invention and Comparative Examples 1, 2, and 3. DETAILED DESCRIPTION

[0026] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0027] In the description of the present invention, it should be understood that the terms "center", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "counterclockwise", "clockwise", "axial", "radial", "circumferential" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0028] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection, it can be a direct connection, it can be an indirect connection through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0029] Example 1

[0030] See also Figure 1-Figure 3 This embodiment provides a crystalline SiO 2 Microsphere core and coated with crystalline SiO 2 A thick layer of SrTiO on the surface of the core 3 / TiO 2 and a multi-interface nanoscale SrTiO 3 / TiO 2 Photocatalytic material of heterojunction shell and preparation method thereof. The preparation method comprises the following steps:

[0031] S1: Amorphous SiO 2 For the preparation of microspheres, 300 ml of ethanol, 20 ml of ammonia water, 10 ml of water, and 70 mg of sodium chloride were mixed and stirred at 30° C. Then, 100 g / L of tetraethyl silicate ethanol solution was added at a flow rate of 12 ml / h for 3 h, and then the white powder was separated by suction filtration and dried.

[0032] S2: Thick TiO 2 Preparation of the shell, take 0.5g of S1 obtained SiO 2The microspheres were ultrasonically mixed with 100 ml of ethanol and 1 ml of ammonia water, and 1 g of tetrabutyl titanate was added while stirring at 50°C for 24 hours, and then the white powder was separated by suction filtration and dried. The dried powder was then calcined at 600°C for 3 hours.

[0033] S3: Crystalline SiO 2 @TiO 2 Preparation, take 0.5g S2 obtained material and 0.02g CaCl 2 The mixture was mixed with 1 ml of water and shaken for 1 h, then dried for 30 min to evaporate the water, and then calcined at 1000 °C for 3 h in air atmosphere.

[0034] S4: Thick layer SrTiO 3 / TiO 2 Preparation, take 0.5g of the material obtained in step S3 and 0.4gSr(OH) 2 8H 2 O, 0.5 g NaOH and 70 ml water were fully stirred and mixed in a beaker, and then transferred to a hydrothermal kettle for hydroheating at 160 °C for 20 h. The white powder was then separated by suction filtration and dried.

[0035] S5: Multi-interface Nanoscale SrTiO 3 / TiO 2 Preparation of heterojunction shell: The material obtained by S4 is subjected to S2 and S4 operations alternately. The difference between S2 and S4 is that the amount of tetrabutyl titanate used is 0.1 g, and Sr(OH) 2 8H 2 The amount of O used is 0.1g. That is, crystalline SiO 2 Core and multi-layer SrTiO 3 / T i 2 The semiconductor photocatalytic material (SiO 2 @SrT iO 3 / TiO 2 ).

[0036] Result analysis:

[0037] The SiO 2 @SrT iO 3 / T i 2 The powder was characterized by SEM. Figure 1 As shown, the material is a microspherical structure. 2 @SrT iO 3 / T i 2 The powder was subjected to TEM standard, and the results were as follows Figure 2 As shown, SrT iO 3The group size is 5*7nm, TiO 2 The group size is 4*7nm.

[0038] Example 2

[0039] This embodiment provides a photocatalytic process for treating wastewater containing nonylphenol and its derivatives.

[0040] 1L nonylphenol simulated wastewater was prepared, with a nonylphenol concentration of 10mg / L. After ultrasonic mixing with 5g of the catalytic material obtained in Example 1, it was transferred to a photocatalytic device, and the ultraviolet light power was set to 200W. The total reaction time was 2.5h. From 0 to 0.5h, 0.2L / min of 10% ozone gas was introduced into the device; from 0.5 to 2.5h, a total of 5ml of hydrogen peroxide solution (30%) was added into the device twice. Samples were taken every 30min during the process and the TOC content was tested. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that TOC removal is not obvious in the first 30 minutes, which is mainly in the process of ring opening and chain breaking. After adding the oxidant, TOC removal is rapid, and a mineralization rate of 98% is achieved within 2.5 hours. This shows that the process of this embodiment has excellent performance in photocatalytic degradation of nonylphenol wastewater.

[0041] Comparative Example 1

[0042] This comparative example provides a method for preparing a photocatalytic material for treating wastewater of nonylphenol and its derivatives and a photocatalytic process.

[0043] The preparation method thereof is similar to that of Example 1, except that step S3 is changed to remove SiO 2 And do not perform S5 operation. Remove SiO 2 The steps are to add NaOH solution at 50°C for etching for 1 hour, and then wash with dilute acetic acid after separation by suction.

[0044] The photocatalytic process was carried out in accordance with Example 2. The difference was that the photocatalytic material was replaced by the material obtained in Comparative Example 1. During the process, samples were taken every 30 minutes and the TOC content was tested. The results were as follows: Figure 3 It is shown that the material obtained in Example 1 has better nonylphenol mineralization ability.

[0045] Comparative Example 2

[0046] This comparative example provides a photocatalytic process for treating wastewater of nonylphenol and its derivatives.

[0047] The photocatalytic process was similar to that of Example 2, except that 0.2 L / min of 10% ozone was introduced into the photocatalytic system during the reaction time. Samples were taken every 30 minutes and the TOC content was tested. The results are shown in Figure 3This indicates that the mineralization rate in the late stage of the ozone + photocatalyst oxidation process is slow, and it is more suitable for early stage treatment.

[0048] Comparative Example 3

[0049] This comparative example provides a photocatalytic process for treating wastewater of nonylphenol and its derivatives.

[0050] The photocatalytic process was similar to that of Example 2, except that a hydrogen peroxide solution was added to the photocatalytic system during the reaction time, and a total of 5 ml of a hydrogen peroxide solution (30%) was added three times. Samples were taken every 30 minutes during the process and the TOC content was tested. The results are shown in Figure 3 This indicates that the oxidant + photocatalyst process can only partially remove nonylphenol and is not suitable for mineralizing nonylphenol alone.

[0051] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A photocatalytic material for treating wastewater of nonylphenol and its derivatives, Features: The photocatalytic material is made of crystalline SiO 2 The core and the coating are in crystalline SiO 2 A thick layer of SrTiO on the surface of the core 3 / TiO 2 and a multi-interface nanoscale SrTiO 3 / TiO 2 The heterojunction shell is composed of SiO 2 @SrTiO 3 / TiO 2 .

2. A method for preparing the photocatalytic material according to claim 1, Features: First prepare a thick layer of TiO 2 Encapsulated amorphous SiO 2 Microspheres, high temperature calcined crystalline SiO 2 After that, thick layer SrTiO was prepared hydrothermally. 3 / TiO 2 , and then by repeatedly coating with a thin layer of TiO 2 Hydrothermal preparation of SrTiO 3 Preparation of multi-interface nanoscale SrTiO 3 / TiO 2 Heterojunction shell.

3. The method for preparing a photocatalytic material according to claim 2, characterized in that: in, The TiO 2 It is anatase type; Wherein, the SiO 2 The size of the microspheres is 0.1-10 μm.

4. The method for preparing a photocatalytic material according to claim 2 or 3, Features: S1: Amorphous SiO 2 Preparation of microspheres: SiO 2 Microspheres, ethanol, ammonia, water, and chloride salt are fully mixed, and then the ethanol solution containing Si ester compound is slowly added while stirring, and maintained at 20-50°C for 1-3h, and then white powder is separated and dried; S2: Thick layer of TiO 2 Preparation of the shell, the SiO 2 The microspheres are fully mixed with ethanol and ammonia water, and the Ti-containing ester compound is added during stirring. The mixture is maintained at 40-60°C for 24-48 hours, and then the white powder is separated and dried. The dried powder is then calcined at high temperature to obtain SiO 2 @TiO 2 ; S3: Crystalline SiO 2 @TiO 2 Preparation of SiO 2 @TiO 2 After being evenly mixed with alkaline earth chloride and water, it was shaken for 0.5-1h, dried, and calcined at high temperature for a certain period of time in an air atmosphere to obtain crystalline SiO 2 @TiO 2 . The alkaline earth chloride is CaCl 2 、SrCl 2 、BaCl 2 and one or more of its corresponding hydrates; the molar amount of alkaline earth chloride is 0.01-0.5 times the molar amount of the material obtained from S2, the calcination temperature is 800-1200°C, and the calcination time is 3-8h. S4: Thick layer SrTiO 3 / TiO 2 Preparation of crystalline SiO in S3 2 @TiO 2 The mixture is fully stirred and mixed with the Sr-containing compound, NaOH and deionized water in a beaker, and then transferred to a hydrothermal kettle. After being maintained at a certain temperature for a period of time, a white powder is separated and dried. The Sr-containing compound is Sr(OH) 2 、Sr(NO3) 2 、Sr(CO3) 2 and one or more of its corresponding hydrates, the molar amount of the Sr-containing compound is 0.2-0.6 times the molar amount of the material obtained from S3; the hydrothermal temperature is 150-200°C, and the hydrothermal time is preferably 12-24h. S5: Multi-interface Nanoscale SrTiO 3 / TiO 2 Preparation of heterojunction shell, repeating the operation of steps S2 and S4 alternately for the material obtained in S4, and adjusting the hydrolysis time in S2 and the amount of Sr-containing compound in S4 to form nano-sized SrTiO 3 / TiO 2 Materials, namely, crystalline SiO 2 Core and multi-interface nanoscale SrTiO 3 / TiO 2 Photocatalytic materials for heterojunction shells.

5. The method for preparing a photocatalytic material according to claim 4, Features: In S1, The Si-containing ester compounds are silicate compounds; Wherein, the concentration of the ethanol solution of the ester compound is 50-200 g / L; Wherein, the amount of ester compound added is 6-20ml / h; Wherein, the ethanol concentration is not less than 95%, and the amount of ethanol used is 10-20 times the amount of Si-containing ester compound added per hour; The concentration of ammonia water is 25-28%, and the amount of ammonia water used is 0.5-2 times the amount of Si-containing ester compound added per hour; Among them, chloride salts are NaCl, KCl, CaCl 2 One or more of the above, the amount of chloride salt used is 0.005-0.02 times the amount of Si-containing ester compound added per hour; Among them, SiO 2 The size of the spheres is 0.5-3 μm.

6. The method for preparing a photocatalytic material according to claim 4, Features: In S2, The Ti-containing ester compound is a titanate compound; The amount of Ti ester compound added is 0.5-2 times the molar amount of the material obtained in S1; Wherein, the concentration of ethanol is not less than 95%, and the amount of ethanol used is 50-100 times the mass of the material obtained in S1; The concentration of ammonia water is 25-28%, and the amount of ammonia water used is 1-2 times the mass of the material obtained by containing S1; Wherein, the calcination temperature is 500-800°C.

7. The method for preparing a photocatalytic material according to claim 6, Features: The S2TiO 2 The layer thickness is 20-100nm; the multi-interface nanoscale SrTiO 3 / TiO 2 The size of the heterojunction is 2-20nm.

8. A photocatalytic process for treating wastewater of nonylphenol and its derivatives, Features: The process adds the photocatalytic material, ultraviolet light and other oxides described in claim 1 to the wastewater of nonylphenol and its derivatives, and uses photocatalysis to carry out oxidation degradation reaction.

9. A photocatalytic process for treating wastewater of nonylphenol and its derivatives as described in claim 8: the initial stage of the reaction is the period when most of the organic matter in the degradation process is in the ring-opening stage, and the degradation time is 0-0.5h; the middle and late stages of the reaction are the period when most of the organic matter in the degradation process is in the chain breaking and mineralization stage, and the degradation time is 0.5-3h.

10. A photocatalytic process for treating wastewater of nonylphenol and its derivatives as claimed in claim 9: in, In the initial stage of the reaction, a dual oxidation treatment process of ozone and photocatalytic materials is adopted, and the ozone flow rate per minute is 0.1-0.5 times the amount of wastewater to be treated. Among them, a treatment process of adding photocatalytic materials and oxidants is adopted in the middle and late stages of the reaction. The oxidants are chemical substances with strong oxidizing properties or whose decomposition products have strong oxidizing properties.

Citation Information

Patent Citations

  • SiO2-TiO2 composite nanomaterial of core-shell structure and preparation method and application thereof

    CN104998629A

  • Double-layer core-shell platinum catalyst and preparation method and application thereof

    CN108837827A

  • SrTiO3 / TiO2 heteroepitaxial photocatalyst as well as preparation method and application thereof

    CN115007128A

  • Photocatalyst having molecule-recognition function and method for eliminating harmful substance using it

    JP2003245558A

  • Dielectric ceramic and multi-layer ceramic capacitor

    JP2009096671A