Tween-80 auxiliary synthesized catalyst, preparation method thereof and application of Tween-80 auxiliary synthesized catalyst in catalytic decomposition of N2O
The catalyst is prepared by using the sol-gel method assisted by Tween-80, and the problem of poor activity and high cost of catalytic decomposition of N2O catalysts under impurity gases is solved, and high efficiency of low temperature and high resistance to N2O is achieved. It is suitable for use in low temperature and high efficiency of N2O decomposition and good antioxidant properties. Application in actual exhaust gas environment.
Patent Information
- Application Number
- CN202411025485.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing catalytic decomposition N2O catalysts are poorly active and costly under the atmosphere of impurity gas, making it difficult to effectively decompose N2O at low temperatures and resist the influence of O2, H2O, and NOx.
Using Tween-80 as a nonionic surfactant, the transition metal oxide catalyst is synthesized by the sol-gel method to reduce the preparation cost, improve the catalytic activity and anti-impact gas capacity. The specific steps include typing Tween-80 with the transition metal salt in a specific way. The reaction was carried out under conditions to form a gel-like shape, then dried and calcined to obtain a highly catalytically active transition metal N2O decomposition catalyst.
It significantly increases the specific surface area and number of active positions of the catalyst, reduces the reaction activation energy, and the catalyst has high conversion rate and good antioxidant properties to N2O, can effectively decompose N2O at low temperatures, and maintain high activity in the presence of impurity gas. Suitable for N2O elimination in actual exhaust gas environment.
Smart Images

Figure CN118949991A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic decomposition of N2O, and specifically relates to a Tween-80 assisted synthesis catalyst and a preparation method thereof and application in catalytic decomposition of N2O. Background Art
[0002] Nitrous oxide (N2O) is the third most powerful greenhouse gas after CO2 and CH4. It has strong atmospheric stability and infrared radiation absorption capacity. It can permanently destroy ozone in the atmosphere, aggravate the ozone hole, and bring great pressure to the environment. With the rapid development of science and technology, the amount of N2O emissions from human industrial production is increasing day by day, mainly from the production of chemical products such as nitric acid plants and oxalic acid plants, as well as exhaust emissions from motor vehicles. Since N2O can stay in the atmosphere for 150 years, reducing emissions cannot immediately alleviate environmental pressure. Therefore, its elimination has become the main focus of researchers.
[0003] In the current research on the elimination of N2O, N2O pollution caused by industrial production has become the main elimination target of researchers due to the concentrated emission sources and large emission volume. However, in the industrial production process, in addition to the emission of N2O, it is often accompanied by some other gases, such as O2, H2O, NO, CO2, etc. The presence of these impurity gases often hinders the elimination of N2O pollution sources. Therefore, seeking an elimination method that is less affected by impurity gases has become the key to whether it can be applied in actual production.
[0004] Among the three commonly used methods for eliminating N2O, the high-temperature decomposition method requires a relatively high reaction temperature (>800°C) and consumes a lot of energy, so it cannot be industrialized. Although the selective catalytic method has a lower catalytic temperature, it requires the addition of a reducing agent, which usually increases costs and produces secondary pollution. Therefore, the direct catalytic decomposition method has become the most promising N2O decomposition method due to its many advantages such as low energy consumption, low cost, and no secondary pollution. Among all direct catalytic decomposition catalysts, transition metal oxides not only have excellent catalytic performance and excellent adjustable denaturation, but also have low cost. They are currently the most widely studied N2O decomposition catalysts. In particular, Co3O4 plays a vital role in the research on the catalytic decomposition of N2O. In order to apply this type of catalyst to actual production and life, it is necessary to improve its catalytic activity at low temperatures and its resistance to impurity gases (O2, H2O, NO x ) ability becomes the key to its application in real scenarios.
[0005] Among the many methods for preparing Co3O4, the sol-gel method is a common one. Among them, the sol-gel method with citric acid as the complexing agent is the most widely used. Liu et al. (Liu et al., Chemical Engineering Journal. 2021, 414, 128643) used this method to synthesize a series of Sm-doped Co3O4 catalysts for the direct catalytic decomposition of N2O. 0.1 -Co3O4 has the best catalytic activity and tolerance to impurity gases, and the activation energy is only 24.7 kJ mol -1 , which is only 1 / 4 of Co3O4. Hu and his team (Hu et al., Molecular Catalysis. 2021, 509, 111-656) used C3N4-modified citric acid sol-gel method to prepare a series of N-doped Co3O4 catalysts, among which N-Co3O4-0.05 showed better activity and stability and stronger resistance to impurity gases, and produced more oxygen vacancies, which enhanced the Co on the catalyst. 2+ and Co 3+ redox cycle.
[0006] In recent years, we have found that adding various surfactants to the preparation process of the sol-gel method will also have a regulatory effect on the target reaction. Song et al. (Song et al., ACS Applied Materials & Interfaces. 2016, 8, 32, 20802-20813) used surfactant P123 to synthesize a batch of Ni / Mn-promoted mesoporous Co3O4 catalysts, among which 5% Ni-Co showed the best activity. The catalyst surface has a large number of surface oxygen vacancies, which promotes the target reaction. In addition, the previous authorized invention patent CN115739090A of this research group provides a method of using a simple sol-gel method to add non-ionic surfactant F127 (PEO 106 PPO 70 PEO 106 , Mav=12600) as the complex to prepare the transition metal oxide 3.0F-Co3O4, which was used to directly catalyze the decomposition of N2O. At the same time, its catalytic activity under ideal conditions and its catalytic activity against O2, H2O, NO in the exhaust gas environment of a simulated nitric acid plant were investigated. x The catalyst not only has high catalytic activity, but also shows better resistance to impurity gases and stability than the conventional precipitation method Co3O4. It can be seen that adding non-ionic surfactants to the sol-gel method to synthesize low-temperature and high-efficiency transition metal oxide catalysts has gradually come into the researchers' field of vision and has great potential.
[0007] Tween-80 is a nonionic surfactant that can be used as a food additive and is very cheap. In order to improve the performance of the catalyst and further reduce the preparation cost, the surfactant Tween-80 was selected as a complexing agent and a transition metal oxide catalyst was prepared using the sol-gel method. So far, there has been no report on the use of the sol-gel method and the addition of Tween-80 to synthesize a catalyst for catalytic decomposition of N2O, and there has been no report on the performance of such catalysts on NO x , O2, H2O impurity tolerance research report. Summary of the invention
[0008] In order to solve the problem that the existing catalytic decomposition of N2O catalysts has poor activity in an impurity gas atmosphere and the cost of improving performance is high, the present invention provides a preparation process and application of a transition metal oxide catalyst which is low in cost, simple to prepare, has good low-temperature activity, good stability, good resistance to impurity gases and particularly outstanding antioxidant properties.
[0009] The technical solution provided by the present invention is as follows:
[0010] A preparation method for a Tween-80-assisted synthesis of a transition metal N2O decomposition catalyst with high catalytic activity comprises the following steps: completely dissolving an appropriate amount of a specific emulsifier, polyoxyethylene sorbitan monooleate (Tween-80), in a beaker containing water and an inorganic acid, adding a transition metal salt, heating and stirring until the mixture is completely dissolved, drying and calcining the mixture when the mixture reacts to a gel state to obtain a target product.
[0011] The above-mentioned Tween-80-assisted preparation method of a transition metal N2O decomposition catalyst with high catalytic activity, wherein the transition metal salt is one or more of cobalt nitrate, cobalt acetate, cobalt oxalate, copper nitrate, and nickel nitrate.
[0012] The above-mentioned method for preparing a Tween-80-assisted synthesis of a transition metal N2O decomposition catalyst with high catalytic activity, wherein the surfactant is a very low-priced food emulsifier polyoxyethylene sorbitan monooleate Tween-80, with a molecular formula of C 64 H 124 O 26 .
[0013] In the above-mentioned method for preparing a Tween-80-assisted synthesis of a transition metal N2O decomposition catalyst with high catalytic activity, the inorganic acid is one or more of nitric acid, hydrochloric acid or sulfuric acid.
[0014] The above-mentioned method for preparing a Tween-80-assisted synthesis of a transition metal N2O decomposition catalyst with high catalytic activity comprises the following steps: the reaction temperature is 65°C to 95°C, and the reaction time is 3h to 20h.
[0015] The above-mentioned method for preparing a Tween-80-assisted synthesis of a transition metal N2O decomposition catalyst with high catalytic activity, wherein the drying temperature is 90°C to 150°C and the drying time is 8h to 24h.
[0016] The above-mentioned Tween-80-assisted preparation method of a transition metal N2O decomposition catalyst with high catalytic activity comprises the following steps: the calcination temperature is 350°C to 450°C, the calcination time is 1h to 4h, the calcination platform temperature is 150°C to 250°C, and the calcination time is 0.5h to 1.5h.
[0017] The above-mentioned preparation method is used for the application of a Tween-80 assisted synthesis high catalytic activity transition metal N2O decomposition catalyst in direct catalytic decomposition of N2O.
[0018] In the above application, the activity of the catalyst for catalytic decomposition of N2O is evaluated in a normal pressure gas-solid fixed bed reactor, the raw gas introduced is one or more of N2O, O2, H2O, NO, the balance gas is Ar, and the operating temperature is 150°C to 400°C.
[0019] The beneficial effects of the present invention are:
[0020] 1. The preparation method of the present invention is a sol-gel method assisted by a polyoxyethylene nonionic surfactant. The added surfactant effectively reduces the crystal size of the catalyst, increases the specific surface area of the catalyst, and increases the number of active sites accordingly, providing a large number of active sites for the catalytic decomposition of N2O. In addition, the addition of the surfactant also changes the surface properties of the catalyst, weakens the Co-O bond, and reduces the activation energy of the reaction.
[0021] 2. The active component of the catalyst prepared by the present invention is a transition metal oxide. The added surfactant not only greatly improves the activity of the Co3O4 catalyst in catalytically decomposing N2O, but also the prepared catalyst has good tolerance to the impurity gases tested. Even in an atmosphere where 5vol%O2+100ppmv NO+2vol%H2O coexist, the catalyst can achieve a conversion rate of nearly 81% for N2O (2000ppmv) in the reaction gas at 400°C. In addition, the catalyst shows extremely superior performance in terms of oxidation resistance, and the conversion rate can still reach more than 80% at a low temperature of 300°C, providing a new idea for the elimination of N2O in actual exhaust gas environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the activity diagram of the catalysts obtained in Examples 1-6 and Comparative Examples 1 and 2 for catalytic decomposition of N2O.
[0023] Figure 2This is an activity diagram of the catalyst obtained in Example 1 for catalytic decomposition of N2O at different temperatures in the presence of impurity gases (O2, H2O, NO).
[0024] Figure 3 Graph showing the change in N2O conversion over time over the catalyst obtained in Example 1 at 350°C and 400°C when some impurity gases (O2, H2O, NO) are injected into or cut off from the feed stream of 2000 ppmv N2O / Ar.
[0025] Figure 4 This is a test chart of the stability of the catalyst obtained in Example 1 to a single impurity gas.
[0026] Figure 5 It is the XPS analysis spectrum corresponding to the Co 2p orbital of the catalyst obtained in Example 1 and Comparative Examples 1 and 2.
[0027] Figure 6 The pore size distribution diagram and N2 adsorption-desorption isotherms of the catalysts obtained in Example 1 and Comparative Examples 1 and 2 are shown. Specific implementation plan
[0028] In order to enable those skilled in the art to more fully understand the present invention, the present invention is described in more detail by the following non-limiting examples or comparative examples, but the examples or comparative examples do not limit the present invention in any way.
[0029] Example 1 Preparation of Catalyst S(1)-4TW-80-Co3O4
[0030] 4.0 g of surfactant Tween-80 (polyoxyethylene sorbitan monooleate Tween-80, molecular formula C 64 H 124 O 26 ) was completely dissolved in a beaker containing 17 mL of deionized water and 2.4 g of HNO3. 5.0 g of Co(NO3)2·6H2O was added to the mixed solution and then transferred to a 90°C water bath for heating and stirring. When the mixture was in a gel state that was difficult to stir, it was placed in a 120°C oven for drying for 12 h. The obtained dry gel was ground and calcined in a pit furnace. It was calcined at a heating rate of 5°C / min at temperature platforms of 150°C and 250°C for 1 h and 0.5 h, and then calcined at 400°C for 2 h to obtain the catalyst S(1)-4TW-80-Co3O4 (xTW-80-Co3O4), wherein x represents the amount of surfactant (x=1-6) and TW-80 represents the surfactant Tween-80.
[0031] Example 2 Preparation of Catalyst S(2)-1TW-80-Co3O4
[0032] The catalyst was prepared according to the method described in Example 1, except that 1 g of Tween-80 was used instead of 4 g of Tween-80 in Example 1, to obtain catalyst S(2)-1TW-80-Co3O4.
[0033] Example 3 Preparation of Catalyst S(3)-2TW-80-Co3O4
[0034] The catalyst was prepared according to the method described in Example 1, except that 2 g of Tween-80 was used instead of 4 g of Tween-80 in Example 1, to obtain catalyst S(3)-2TW-80-Co3O4.
[0035] Example 4 Preparation of Catalyst S(4)-3TW-80-Co3O4
[0036] The catalyst was prepared according to the method described in Example 1, except that 3 g of Tween-80 was used instead of 4 g of Tween-80 in Example 1, to obtain catalyst S(4)-3TW-80-Co3O4.
[0037] Example 5 Preparation of Catalyst S(5)-5TW-80-Co3O4
[0038] The catalyst was prepared according to the method described in Example 1, except that 5 g of Tween-80 was used instead of 4 g of Tween-80 in Example 1, to obtain catalyst S(5)-5TW-80-Co3O4.
[0039] Example 6 Preparation of Catalyst S(6)-6TW-80-Co3O4
[0040] The catalyst was prepared according to the method described in Example 1, except that 6 g of Tween-80 was used instead of 4 g of Tween-80 in Example 1, to obtain catalyst S(6)-6TW-80-Co3O4.
[0041] Comparative Example 1 Preparation of Catalyst B(1)-Co3O4(P)
[0042] First, take an appropriate amount of Co(NO3)2·6H2O and dissolve it in a certain amount of deionized water to prepare a 0.2M precursor solution for use. Subsequently, at 40°C, under continuous stirring, add 0.5M Na2CO3 precipitant dropwise to the above mixed precursor solution to make the pH value of the solution reach 9.3. After aging for 2 hours, the resulting precipitate is filtered and washed with a large amount of deionized water to clean the residual sodium ions therein, and the pH value of the filtrate reaches neutrality (pH=7) as the standard for cleaning the residual sodium ions. Finally, the resultant is placed in a supply box and dried at 110°C, and then calcined at 500°C in an air atmosphere for 3 hours. The B(1)-Co3O4(P) catalyst is obtained.
[0043] Comparative Example 2 Preparation of Catalyst B (2) -0TW-80-Co3O4
[0044] Catalyst B(2)-0TW-80-Co3O4 was prepared according to the method described in Example 1, except that no surfactant was added during the preparation process, to obtain catalyst B(2)-0TW-80-Co3O4.
[0045] Example 7 Performance Test of Catalyst
[0046] The general activity determination of the catalyst is carried out on an integral fixed bed at normal pressure. The catalyst samples of Examples 1-6 and Comparative Examples 1 and 2 are pressed into tablets using a mold, sieved, and 200 mg of a 40-60 mesh catalyst is added to a quartz tube reactor (inner diameter 4 mm). The mixed reaction gas contains 2000 ppmv of N2O, and Ar is the carrier gas. When impurity gases are introduced therein, the types of impurity gases and the corresponding contents are 5 vol.% O2, 2 vol.% H2O or 100 ppmv NO, respectively. In order to examine the effect of impurity gases on the activity of the catalyst, one or more of these impurity gases are introduced according to the circumstances, and the specific circumstances will be directly given in the corresponding charts. The total flow rate of the mixed gas is 50 mL·min -1 , and a Varian CP-3800 gas chromatograph (with an inner diameter equipped with a phase-fixed Porapak Q and a thermal conductivity detector, and high-purity Ar as the carrier gas) was used to detect the residual concentration of N2O online.
[0047] like Figure 1 As shown in the figure, the effect of the amount of surfactant Tween-80 on the catalytic N2O decomposition performance of xTW-80-Co3O4 (2000ppmv N2O / Ar, GHSV = 20 000h -1) and the effect of B(1)-Co3O4(P) of comparative example 1 prepared by precipitation method. The results show that the catalytic activity of the xTW-80-Co3O4 catalyst is greatly improved after the addition of Tween-80 during the preparation process. For example, at 350°C, the N2O conversion rate of the Co3O4(P) catalyst is only 24.3%, which is much lower than the N2O conversion rate of the xTW-80-Co3O4 catalyst (x=1~6). And as the amount of Tween-80 increases from 1.0g to 6.0g, the N2O conversion rate shows a trend of first increasing and then slightly decreasing, among which the catalytic activity of the S(1)-4TW-80-Co3O4 catalyst is the best. At 250°C, the N2O conversion rate on the 4TW-80-Co3O4 catalyst is 80%, while the conversion rate of the Co3O4(P) catalyst at the same temperature is almost 0. In addition, it is worth noting that the 0TW-80-Co3O4 catalyst prepared by the sol-gel method without adding any surfactant Tween-80 has the worst catalytic performance, with only 9.5% N2O conversion at 350°C. This means that the surfactant is the key to improving the activity.
[0048] The impurity gas tolerance of the catalyst with the best activity (the catalyst obtained in Example 1) was tested
[0049] Whether the catalyst has good resistance to impurity gases plays a decisive role in whether it can be used in actual industrial production. Therefore, the resistance of S(1)-4TW-80-Co3O4 catalyst to impurity gases (NO, O2 and H2O) discharged from nitric acid plants was evaluated. Figure 2 When no impurity gas is introduced into the system, the T 90 (the temperature at which the N2O conversion rate reaches 90%) is only 265°C; when 100 ppmv NO, 5 vol.% O2 and 2 vol.% H2O enter the reaction system, the corresponding T 90 The temperature increases at different temperatures are 307°C, 300°C, and 324°C, respectively, which means that NO, O2, and H2O all inhibit the activity of the catalyst, but the inhibitory effect is relatively limited. In addition, when all impurity gases (100 ppmv NO, 5 vol.% O2, and 2 vol.% H2O) are introduced into the reaction system, the N2O conversion rate of the catalyst S(1)-4TW-80-Co3O4 can still reach more than 80% at 350°C.
[0050] The catalyst with the best activity (catalyst obtained in Example 1) was tested for stability
[0051] Under the specified reaction conditions, the N2O conversion rate over S(1)-4TW-80-Co3O4 catalyst changes with time to determine the stability of the catalyst. The results are as follows Figure 3As shown. First, without any impurity gas introduced, the conversion rate of the catalyst at 400°C was always maintained at 100%; then 5vol.% O2 and 2vol.% H2O were introduced in sequence, and the conversion rate of the catalyst was still maintained at 100% after 7h. After 100ppmv NO was introduced, the catalyst activity began to decline and finally maintained at about 82%; then the temperature was lowered and all impurity gases were cut off, and it was found that the catalyst conversion rate at 350°C quickly rebounded to 100% and remained stable; impurity gases were introduced in sequence at 350°C again, and when only 5vol.% O2 existed, the catalyst could maintain a 100% conversion rate without falling, and after 100ppmv NO and 2vol.% H2O participated in the reaction, the catalyst activity dropped rapidly and finally stabilized at about 16%. After that, all impurity gases were cut off, and the catalytic N2O conversion rate gradually rebounded to 100% and remained stable.
[0052] The stability test of the catalyst with the best activity (the catalyst obtained in Example 1) was carried out for the impurity gas alone.
[0053] In order to further explore the sensitivity of the catalyst to various impurity gases, the stability test of the S(1)-4TW-80-Co3O4 catalyst to each impurity gas was carried out. The results are as follows: Figure 4 As shown. When only 5 vol.% O2 is present as an impurity gas, the catalyst can maintain a 100% conversion rate at 350℃ for more than 10 hours without falling back. When the temperature is reduced to 300℃, it can still maintain a high conversion rate of 82%, proving that the catalyst has excellent oxygen resistance. In addition, the stability of the catalyst after H2O and NO are introduced at 350℃ is tested. From the results, it can be seen that although the catalyst's resistance to H2O is inferior to O2, it still has a conversion rate of up to 96%, while the catalyst's resistance to NO is slightly inferior, with a conversion rate of 61%. In addition, the N2O conversion rate in the presence of NO and O2 is also tested. At 350℃, the activity is similar to that in the presence of H2O, NO and O2 at the same time, both of which are about 16%. This is because the surface active sites of the catalyst are almost occupied by nitrogen oxides at a lower reaction temperature, and the subsequent water vapor cannot continue to capture the remaining active sites. From the above phenomena, it can be seen that the S(1)-4TW-80-Co3O4 catalyst has satisfactory catalytic stability.
[0054] XPS analysis of the catalyst with the best activity (catalyst obtained in Example 1)
[0055] In order to explore the effect of the addition of surfactant on the strength of the Co-O bond on the catalyst surface, the surface properties of the catalysts B(1)-Co3O4(P) of Comparative Example 1, B(2)-0TW-80-Co3O4 of Comparative Example 2, and S(1)-4TW-80-Co3O4 of Example 1 were analyzed by XPS photoelectron spectroscopy. Figure 5 shown. Figure 5 The Co2p spectra of the three catalyst samples show that for Co-based composite oxide catalysts, the greater the degree of low shift of the binding energy corresponding to Co 2p3 / 2, the weaker the bond strength of the Co-O bond. Based on this, it can be seen that due to the addition of Tween-80, the binding energy corresponding to Co 2p3 / 2 in the S(1)-4TW-80-Co3O4 catalyst is 1.6 eV lower than the binding energy corresponding to Co 2p3 / 2 in B(1)-Co3O4(P). Therefore, it can be concluded that the surfactant in the catalyst weakens the Co-O bond in the catalyst to a large extent, promoting the reaction.
[0056] The catalyst with the best activity (the catalyst obtained in Example 1) was subjected to N2 physical adsorption and desorption analysis.
[0057] The S(1)-4TW-80-Co3O4 catalyst of Example 1, the B(1)-Co3O4(P) catalyst of Comparative Example 1, and the B(2)-0TW-80-Co3O4 catalyst of Comparative Example 2 were characterized by N2 physical adsorption and desorption. The corresponding results are listed in Tables 1 and Figure 6 From the data in Table 1, it can be seen that the specific surface area of S(1) catalyst is 33m 2 / g, and the catalyst prepared by the sol-gel method has a significantly smaller pore size. Figure 6 A is the N2 adsorption-desorption isotherm of the three catalysts. It can be seen that the curve of the S(1) catalyst in Example 1 is a typical IV type isotherm unique to mesoporous materials. Figure 6 The pore size distribution diagram of B also shows that the particle size distribution of the catalyst S(1) of Example 1 is 10-20 nm. These results indicate that the addition of the surfactant Tween-80 increases the specific surface area of the catalyst to a large extent and increases the number of surface active sites of the catalyst, which may be an important reason for the excellent catalytic performance of the catalyst.
[0058] Table 1
[0059]
Claims
1. A catalyst assisted by Tween-80 synthesis, characterized in that: The preparation method comprises the following steps: completely dissolving an appropriate amount of surfactant in water and inorganic acid, adding a transition metal salt, heating and stirring until completely dissolved, reacting, and drying and calcining when the reaction becomes a gel to obtain the target product.
2. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The transition metal salt is one or more of cobalt nitrate, cobalt acetate, cobalt oxalate, copper nitrate and nickel nitrate.
3. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The surfactant is polyoxyethylene sorbitan monooleate Tween-80, with a molecular formula of C 64 H 124 O 26 .
4. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The inorganic acid is one or more of nitric acid, hydrochloric acid or sulfuric acid.
5. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The reaction temperature is 65° C. to 95° C., and the reaction time is 3 h to 20 h.
6. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The drying temperature is 90° C. to 150° C., and the drying time is 8 h to 24 h.
7. A Tween-80 assisted synthesis catalyst according to claim 1, characterized in that: The calcination temperature is 350° C. to 450° C., the calcination time is 1 h to 4 h, the calcination platform temperature is 150° C. to 250° C., and the calcination time is 0.5 h to 1.5 h.
8. Use of the catalyst synthesized with the assistance of Tween-80 as claimed in claim 1 in catalytic decomposition of N2O.
9. The use according to claim 8, characterized in that: The method is as follows: the catalyst according to claim 1 is added into a quartz tube reactor in a normal pressure gas-solid fixed bed reactor, N2O and Ar are introduced as carrier gas, and decomposition is carried out at 150°C to 400°C.
Citation Information
Patent Citations
High stability nano gold catalyst for CO normal temperature oxidation and preparation method thereof
CN101380575A
Catalyst for cyclohexane oxidation as well as preparation method and application thereof
CN112973727A
Preparation method and application of transition metal oxide catalyst with high surface oxygen vacancy density
CN115739090A
Cobalt-based composite oxide catalyst for N2O catalytic decomposition and preparation method and application thereof
CN117531535A