HZSM-5 molecular sieve catalyst, preparation method thereof and reaction for catalyzing methanol to prepare propylene
By adding a binder to the HZSM-5 molecular sieve catalyst and performing specific treatments, a catalyst with uniform pore size distribution and high activity is formed, which solves the problem of easy catalyst pulverization and improves the catalyst's compressive strength and catalytic activity.
Patent Information
- Application Number
- CN202411015982.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing HZSM-5 molecular sieve catalysts are prone to pulverization in MTP reactions, affecting catalyst activity and reactor bed pressure drop, posing a safety risk.
By adding a binder to the HZSM-5 molecular sieve catalyst and controlling its mass ratio with the HZSM-5 molecular sieve to be 75-80:20-25, combined with extrusion molding, drying and calcination, a catalyst with uniform pore size distribution and high catalytic activity is formed.
It improves the catalyst's compressive strength and resistance to carbon deposition, reduces the probability of catalyst pulverization, and enhances catalytic activity and reaction efficiency.
Smart Images

Figure CN118950073A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a HZSM-5 molecular sieve catalyst and a preparation method thereof, and a reaction of catalyzing methanol to prepare propylene. Background Art
[0002] As an important basic raw material in the petrochemical industry, propylene is mainly used to produce downstream products such as polypropylene (PP), acrylic acid (AA), butanol (BA), acetone (PK), phenol (Phenol), octanol (CA), acrylonitrile (AN), propylene oxide (PO) and isopropyl alcohol (IPA).
[0003] The traditional production routes of propylene in China mainly include steam cracking and refinery gas filling, of which the former accounts for more than 60% of the propylene supply. In recent years, with the industrial production of coal chemical industry and propane dehydrogenation (PDH) and other units, my country's propylene supply situation has changed significantly. Methanol to olefins (MTO) and methanol to propylene (MTP) are important ways to obtain propylene products in the coal chemical industry. At present, both technologies have achieved industrial production. The target product of MTO technology is mainly ethylene and propylene in equal proportions, while the target product of MTP technology is mainly propylene. The MTP process of Lurgi has achieved large-scale production.
[0004] A Chinese patent with patent authorization announcement number CN107282087B discloses a high-silicon ZSM-5 molecular sieve and its preparation method and application. Specifically, it relates to a preparation method of a high-silicon ZSM-5 molecular sieve, which comprises: uniformly mixing a liquid alkaline silicon source, an aluminum source, a ZSM-5 molecular sieve seed, a template, an alkali, urea and water, and then sequentially performing aging and hydrothermal synthesis crystallization, wherein urea is added during the uniform mixing stage of the raw materials, the liquid alkaline silicon source is calculated as SiO2, and the aluminum source is calculated as Al2O3, and the mixing ratio of the raw materials satisfies: the molar ratio of the liquid alkaline silicon source, the aluminum source, the template, the alkali, the urea and the water is 1:(0.001-0.01):(0.025-0.25):(0.02-0.2):(0.3-4):(8-100), and the weight ratio of the ZSM-5 molecular sieve seed to the SiO2 in the liquid alkaline silicon source is (1-10):100. When the prepared flaky high-silicon ZSM-5 molecular sieve is used to catalyze the reaction of methanol to propylene and / or butene, the selectivity of C3 and / or C4 olefin products is improved.
[0005] The Chinese patent with the patent authorization announcement number CN109721077B discloses a flaky Fe-ZSM-5 zeolite molecular sieve and a preparation method thereof. The crystal thickness of the flaky Fe-ZSM-5 zeolite molecular sieve is 60 to 100 nm. The flaky Fe-ZSM-5 zeolite molecular sieve is obtained by adding different contents of nanocrystalline seeds and adjusting the amount of NH4F. The invention aims at the problem that the Fe-ZSM-5 zeolite molecular sieve synthesized under the OH- system has more non-framework Fe and the Fe-ZSM-5 zeolite molecular sieve synthesized under the F- system has large grains and a long crystallization time. Under the joint action of crystal seeds, NH4F and dual template agents, nano-flaky Fe-ZSM-5 zeolite molecular sieves are obtained in a very short crystallization time. This method is conducive to the diffusion of carbon deposit precursors and products in the methanol to propylene reaction, and the content of non-framework Fe is greatly reduced compared with the synthesis method of the OH- system, thereby reducing the selectivity of by-product methane during the reaction, and having a longer life and higher propylene selectivity.
[0006] The Chinese patent with the patent authorization announcement number CN106466619B discloses a catalyst for converting methanol to propylene and its preparation method. The invention mainly solves the problems of poor stability and low propylene selectivity of the existing catalyst for converting methanol to propylene. The present invention solves the problem well by adopting a technical solution of a binder-free multi-level pore ZSM-5 molecular sieve catalyst composed of 90-100% ZSM-5 molecular sieve, 0.05-3% boron or aluminum element, and 0-5% rare earth element. The catalyst can be used in the industrial production of methanol to propylene.
[0007] The Chinese patent with the patent authorization announcement number CN108046288B discloses a method for preparing a multi-level porous ZSM-5 molecular sieve for methanol to propylene, comprising: a. mixing an aluminum source, a silicon source, an alkali source, a ZSM-5 molecular sieve seed and water to form a gel; b. pre-crystallizing the gel in a reactor at 80-140° C. for 6-48 hours; c. rapidly cooling the pre-crystallized product obtained in step b, then adding an organic template, and finally heating the pre-crystallized product with the template to 100-180° C. for crystallization reaction; after the reaction is completed, the crystallized product is subjected to solid-liquid separation, washing and drying to obtain a molecular sieve raw powder; d. placing the molecular sieve raw powder obtained in step c into an ammonium salt solution for ion exchange to obtain an ammonia-type ZSM-5 molecular sieve, and then calcining to obtain an HZSM-5 molecular sieve, the obtained HZSM-5 molecular sieve having good propylene selectivity and anti-carbon deposition performance.
[0008] The above authorized patents are basically aimed at improving and optimizing the active components of MTP (i.e., ZSM-5 molecular sieve) and its preparation technology, such as improving its reaction activity by means of element modification, pore structure adjustment, morphology control or particle size reduction, but rarely involve the powdering problem that occurs in actual production.
[0009] ZSM-5 molecular sieve is the preferred active component of the MTP process. After being combined with a binder to form granules, ZSM-5 molecular sieve becomes the only MTP catalyst that can be industrially applied. However, in the actual production process, the catalyst will be pulverized after multiple reaction-regeneration operations. The reaction-regeneration operation includes heating and cooling, changing process media, high-temperature roasting and other processes. The large-scale pulverization of the catalyst will not only affect the catalyst activity and cause changes in the reaction products, but also cause an increase in the pressure drop of the reactor bed, posing a safety risk.
[0010] Therefore, it is of great significance to develop a new ZSM-5 molecular sieve catalyst for MTP reaction that can significantly increase the catalytic reaction activity and has strong resistance to carbon deposition and pulverization. Summary of the invention
[0011] The main purpose of the present invention is to provide a HZSM-5 molecular sieve catalyst and a preparation method thereof, and catalyze the reaction of preparing propylene from methanol, so as to solve the problem of easy pulverization of the HZSM-5 molecular sieve catalyst in the prior art.
[0012] In order to achieve the above-mentioned object, according to one aspect of the present invention, a HZSM-5 molecular sieve catalyst is provided, which comprises an HZSM-5 molecular sieve and a binder, wherein the binder is located between particles of the HZSM-5 molecular sieve, the mass ratio of the HZSM-5 molecular sieve to the binder is 75 to 80:20 to 25, and the compressive strength of the HZSM-5 molecular sieve catalyst is 9.5 to 12 N / mm.
[0013] Furthermore, the binder is selected from any one or more of pseudo-boehmite, SB powder and alumina; further, the binder is preferably a mixture of pseudo-boehmite and alumina, and the mass ratio of pseudo-boehmite to alumina is 3-5:7-10.
[0014] Furthermore, the amount of acid sites of the HZSM-5 molecular sieve catalyst is 0.02 to 0.03 mmol / g; and / or the specific surface area of the HZSM-5 molecular sieve catalyst is 325 to 340 m 2 / g; and / or, the porosity of the HZSM-5 molecular sieve catalyst is 45% to 55%; and / or, the average pore size of the HZSM-5 molecular sieve catalyst is 3.5 to 4.5 nm.
[0015] According to another aspect of the present invention, there is provided a method for preparing the aforementioned HZSM-5 molecular sieve catalyst, the preparation method comprising: mixing raw materials including HZSM-5 molecular sieve, a binder, a pore expanding agent, an extrusion aid, and a nitric acid aqueous solution, and then sequentially performing extrusion molding, drying treatment, and calcination treatment to obtain a HZSM-5 molecular sieve catalyst.
[0016] Furthermore, the mass ratio of the HZSM-5 molecular sieve, pore expander, extrusion aid and nitric acid aqueous solution is 75-80: 3-3.5: 2.5-3: 1.7-2.5; and / or the mass concentration of the nitric acid aqueous solution is 3.5-5wt%.
[0017] Furthermore, the silicon-aluminum ratio of the above-mentioned HZSM-5 molecular sieve is 300-500:1; and / or the particle size of the HZSM-5 molecular sieve is 250-300 mesh; and / or the particle size of the binder is 450-500 mesh, and preferably the ratio of the particle size of the binder to the particle size of the HZSM-5 molecular sieve is 46-48:26-28.
[0018] Furthermore, the pore-enlarging agent is sesbania powder, and the dynamic viscosity of the sesbania powder is 2000-3000 cP; and / or, the extrusion aid is selected from any one or more of glycerol, polyacrylamide and silicone resin; preferably, the extrusion aid is glycerol.
[0019] Furthermore, the temperature of the drying treatment is 60 to 80° C.; and / or the time of the drying treatment is 4 to 8 hours.
[0020] Furthermore, the calcination temperature is 500-550° C.; and / or the calcination time is 6-8 hours.
[0021] According to another aspect of the present invention, there is provided a reaction of preparing propylene from methanol using a catalyst, wherein the catalyst is the aforementioned HZSM-5 molecular sieve catalyst.
[0022] Applying the technical solution of the present invention, the catalyst of the present application includes HZSM-5 molecular sieve and a binder, the HZSM-5 molecular sieve has a suitable pore size and a high catalytic activity, the role of the binder is to bind the particles of the HZSM-5 molecular sieve to form a catalyst with higher catalytic activity, preferably controlling the mass ratio of the HZSM-5 molecular sieve to the binder within the above range, so that the pore size distribution of the catalyst is more uniform, on the one hand, it helps to improve the uniformity of the force of the catalyst, so that the present application has a compressive strength within the above range, thereby reducing the probability of the catalyst being crushed due to uneven force during the catalytic process; on the other hand, it helps to provide more catalytic active sites for the catalyst, thereby improving the catalytic activity of the catalyst. Therefore, the catalyst of the present application has a strong ability to resist carbon deposition and pulverization. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0024] Figure 1 The pore size distribution diagram of the HZSM-5 molecular sieve catalyst in Example 1 of the present application is shown;
[0025] Figure 2 A schematic diagram of an evaluation device for a methanol to propylene reaction catalyst of the present application is shown;
[0026] Figure 3 A schematic diagram of the packing of the HZSM-5 molecular sieve catalyst of the present application is shown.
[0027] The above drawings include the following reference numerals:
[0028] 1. Reactor; 2. Condenser; 3. Feed inlet of reactor; 4. Upper section of reactor; 5. Middle section of reactor; 6. Lower section of reactor. DETAILED DESCRIPTION
[0029] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0030] As analyzed in the background technology of this application, there is a problem in the prior art that HZSM-5 molecular sieve catalyst is prone to pulverization. In order to solve the above problem, this application provides a HZSM-5 molecular sieve catalyst and a preparation method thereof, and catalyzes the reaction of preparing propylene from methanol.
[0031] In a typical embodiment of the present application, a HZSM-5 molecular sieve catalyst is provided, which includes a HZSM-5 molecular sieve and a binder, wherein the binder is located between particles of the HZSM-5 molecular sieve, the mass ratio of the HZSM-5 molecular sieve to the binder is 75 to 80:20 to 25, and the compressive strength of the HZSM-5 molecular sieve catalyst is 9.5 to 12 N / mm.
[0032] The catalyst of the present application includes HZSM-5 molecular sieve and binder, HZSM-5 molecular sieve has suitable pore size and high catalytic activity, the role of binder is to bind particles of HZSM-5 molecular sieve to form a catalyst with higher catalytic activity, preferably controlling the mass ratio of HZSM-5 molecular sieve to binder within the above range, so that the pore size distribution of the catalyst is more uniform, on the one hand, it helps to improve the force uniformity of the catalyst, so that the present application has the above range of compressive strength, thereby reducing the probability of the catalyst being crushed due to uneven force during the catalytic process; on the other hand, it helps to provide more catalytic active sites for the catalyst, thereby improving the catalytic activity of the catalyst. Therefore, the catalyst of the present application has a strong ability to resist carbon deposition and pulverization.
[0033] In one embodiment of the present application, the above-mentioned binder is selected from any one or more of pseudo-boehmite, SB powder, and alumina; further, the binder is preferably a mixture of pseudo-boehmite and alumina, and the mass ratio of pseudo-boehmite to alumina is 3-5:7-10.
[0034] It is preferred to control the type of binder within the above range, which helps to enrich the types of raw materials for the binder. Compared with alumina, pseudo-boehmite has incomplete crystallized water molecules, and the time it takes to become peptized is shorter than that of alumina. Adding pseudo-boehmite and alumina at the same time can make the peptization time of the binder step-like, so that the catalyst can be more evenly combined during the molding process. It is preferred to control the mass ratio of pseudo-boehmite and alumina within the above range, which helps to further improve the bonding force between HZSM-5 molecular sieve particles, thereby further improving the catalyst's anti-pulverization ability.
[0035] In one embodiment of the present application, the amount of acid sites of the HZSM-5 molecular sieve catalyst is 0.02-0.03 mmol / g; and / or the specific surface area of the HZSM-5 molecular sieve catalyst is 325-340 m 2 / g; and / or, the porosity of the HZSM-5 molecular sieve catalyst is 45% to 55%; and / or, the average pore size of the HZSM-5 molecular sieve catalyst is 3.5 to 4.5 nm.
[0036] The HZSM-5 molecular sieve catalyst having the above-mentioned range of acid sites has high catalytic activity, so that the catalyst has a strong ability to resist carbon deposition. The HZSM-5 molecular sieve catalyst having the above-mentioned specific surface area, porosity and average pore size range generates less thermal stress during the catalytic process, so that the catalyst has a higher ability to resist pulverization.
[0037] In another typical embodiment of the present application, a method for preparing the aforementioned HZSM-5 molecular sieve catalyst is provided, the preparation method comprising: mixing raw materials including HZSM-5 molecular sieve, a binder, a pore expanding agent, an extrusion aid, and a nitric acid aqueous solution, and then sequentially performing extrusion molding, drying treatment, and calcination treatment to obtain a HZSM-5 molecular sieve catalyst.
[0038] The HZSM-5 molecular sieve and the binder are calcined to form a catalyst, the pore expander is used to increase the pore size of the catalyst, the extrusion aid is used to improve the efficiency of extrusion molding, the addition of nitric acid and water is to make the HZSM-5 molecular sieve, the binder, the pore expander and the extrusion aid fully contact each other, the pore expander, the extrusion aid and the nitric acid are removed during the calcination process, so the formed catalyst has a large specific surface area. The above preparation method has the advantages of simple process and low cost, and the prepared catalyst has strong resistance to carbon deposition and pulverization.
[0039] In one embodiment of the present application, the mass ratio of the above-mentioned HZSM-5 molecular sieve, pore expander, extrusion aid and nitric acid aqueous solution is 75-80:3-3.5:2.5-3:1.7-2.5; and / or, the mass concentration of the nitric acid aqueous solution is 3.5-5wt%.
[0040] Preferably, the mass ratio of HZSM-5 molecular sieve, pore expander, extrusion aid and nitric acid aqueous solution is controlled within the above range, which helps to further improve the specific surface area and pore size distribution uniformity of the catalyst, thereby further improving the catalyst's ability to resist carbon deposition and pulverization. Preferably, the concentration of nitric acid aqueous solution is controlled within the above range, which helps to further improve the mixing uniformity of HZSM-5 molecular sieve and other components.
[0041] In one embodiment of the present application, the silicon-aluminum ratio of the above-mentioned HZSM-5 molecular sieve is 300-500:1; and / or the particle size of the HZSM-5 molecular sieve is 250-300 mesh; and / or the particle size of the binder is 450-500 mesh, and preferably the ratio of the particle size of the binder to the particle size of the HZSM-5 molecular sieve is 46-48:26-28.
[0042] Preferably, the silicon-aluminum ratio of the HZSM-5 molecular sieve is controlled within the above range, which helps to make the catalyst after molding have an appropriate number and strength of acid sites, so as to facilitate the MTP reaction to have a higher propylene selectivity. Preferably, the particle size of the HZSM-5 molecular sieve and the particle size of the binder are controlled within the above range, which helps to make the binder and the HZSM-5 molecular sieve produce a synergistic effect with other components, so that the components are more closely combined, thereby improving the anti-pulverization ability of the catalyst. Preferably, the particle size of the binder and the particle size of the HZSM-5 molecular sieve are controlled within the above range, which helps to make the binder, HZSM-5 molecular sieve and pore expander evenly distributed, and the catalyst formed after calcination has a higher porosity, and the catalyst has more active sites, which can make the catalyst remove heat in time during the reaction, thereby avoiding the local heat release during the reaction cannot be diffused, resulting in the catalyst fragmentation and pulverization.
[0043] In order to further improve the specific surface area and pore size distribution uniformity of the catalyst and improve the efficiency of extrusion molding, in one embodiment of the present application, the pore expanding agent is preferably sesbania powder, and the dynamic viscosity of the sesbania powder is 2000-3000 cP; and / or, the extrusion aid is selected from any one or more of glycerol, polyacrylamide and silicone resin; preferably, the extrusion aid is glycerol.
[0044] In order to fully remove moisture, in one embodiment of the present application, the temperature of the drying treatment is preferably 60 to 80° C.; and / or the drying treatment time is 4 to 8 hours.
[0045] In order to promote the formation of the HZSM-5 catalyst, in one embodiment of the present application, it is preferred that the temperature of the calcination treatment is 500-550° C.; and / or the calcination treatment time is 6-8 hours.
[0046] In another typical embodiment of the present application, a reaction of preparing propylene from methanol using a catalyst is provided, and the catalyst is the aforementioned HZSM-5 molecular sieve catalyst.
[0047] Since the catalyst in the above-mentioned reaction of preparing propylene from methanol is the catalyst of the present application, the reaction has a higher reaction efficiency.
[0048] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0049] Example 1
[0050] Weigh 200g of HZSM-5 molecular sieve, the silicon-aluminum ratio of HZSM-5 molecular sieve is 400:1, and the particle size of HZSM-5 molecular sieve is 275 mesh. Mix HZSM-5 molecular sieve, 55g of a mixture of pseudo-boehmite and aluminum oxide, 8g of sesbania powder and 6.5g of glycerol for 30 minutes, wherein the mass ratio of pseudo-boehmite to aluminum oxide is 3:7, and the particle size of pseudo-boehmite and aluminum oxide is 470 mesh. The dynamic viscosity of sesbania powder is 3000 cP. 5 g of 5% nitric acid aqueous solution is added to the mixture and kneaded for 30 minutes. The strips are extruded by a twin-screw extruder with a 3.0 mm diameter perforated plate. The obtained strips are left standing at room temperature for 24 hours, dried at 80°C for 4 hours, and calcined at 500°C in a muffle furnace for 8 hours to obtain a HZSM-5 molecular sieve catalyst. The pore size distribution of the HZSM-5 molecular sieve catalyst is tested. The pore size distribution is as follows: Figure 1 As shown, from Figure 1 It can be seen that the pore size distribution of the HZSM-5 molecular sieve catalyst is relatively uniform. Among them, the mass ratio of HZSM-5 molecular sieve to binder is 80:22.
[0051] Example 2
[0052] The difference from Example 1 is that the mass of HZSM-5 molecular sieve is 200 g, the mass of the mixture of pseudo-boehmite and alumina is 50 g, and the HZSM-5 molecular sieve catalyst is finally obtained, wherein the mass ratio of HZSM-5 molecular sieve to binder is 80:20.
[0053] Example 3
[0054] The difference from Example 1 is that the mass of HZSM-5 molecular sieve is 187.5 g, the mass of the mixture of pseudo-boehmite and alumina is 62.5 g, and the HZSM-5 molecular sieve catalyst is finally obtained, wherein the mass ratio of HZSM-5 molecular sieve to binder is 75:25.
[0055] Example 4
[0056] The difference from Example 1 is that the mass ratio of pseudo-boehmite to alumina is 3:10, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0057] Example 5
[0058] The difference from Example 1 is that the mass ratio of pseudo-boehmite to aluminum oxide is 5:7, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0059] Example 6
[0060] The difference from Example 1 is that the mass ratio of pseudo-boehmite to alumina is 3:5, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0061] Example 7
[0062] The difference from Example 1 is that the mass ratio of HZSM-5 molecular sieve, sesbania powder, glycerol and nitric acid aqueous solution is 80:3:3:1.7, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0063] Example 8
[0064] The difference from Example 1 is that the mass ratio of HZSM-5 molecular sieve, sesbania powder, glycerol and nitric acid aqueous solution is 75:3.5:2.5:2.5, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0065] Example 9
[0066] The difference from Example 1 is that the mass ratio of HZSM-5 molecular sieve, sesbania powder, glycerol and nitric acid aqueous solution is 90:2.5:3.5:1.5, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0067] Example 10
[0068] The difference from Example 1 is that the particle size of HZSM-5 molecular sieve is 280 mesh, the particle size of the mixture of pseudo-boehmite and alumina is 460 mesh, and the particle size ratio of the mixture of pseudo-boehmite and alumina to HZSM-5 molecular sieve is 46:28, and finally HZSM-5 molecular sieve catalyst is obtained.
[0069] Embodiment 11
[0070] The difference from Example 1 is that the particle size of HZSM-5 molecular sieve is 260 mesh, the particle size of the mixture of pseudo-boehmite and alumina is 480 mesh, and the particle size ratio of the mixture of pseudo-boehmite and alumina to HZSM-5 molecular sieve is 48:26, and finally HZSM-5 molecular sieve catalyst is obtained.
[0071] Example 12
[0072] The difference from Example 1 is that the particle size of the HZSM-5 molecular sieve is 250 mesh, and the particle size of the mixture of pseudo-boehmite and alumina is 500 mesh, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0073] Embodiment 13
[0074] The difference from Example 1 is that the particle size of the HZSM-5 molecular sieve is 300 meshes, and the particle size of the mixture of pseudo-boehmite and alumina is 450 meshes, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0075] Embodiment 14
[0076] The difference from Example 1 is that the particle size of the HZSM-5 molecular sieve is 350 mesh, and the particle size of the mixture of pseudo-boehmite and alumina is 400 mesh, and finally a HZSM-5 molecular sieve catalyst is obtained.
[0077] Embodiment 15
[0078] The difference from Example 1 is that the concentration of the nitric acid aqueous solution is 3.5%, the dynamic viscosity of the sesbania powder is 2000 cP, the drying temperature is 60°C, the drying time is 8 hours, the calcination temperature is 550°C, the calcination time is 6 hours, and finally an HZSM-5 molecular sieve catalyst is obtained.
[0079] Comparative Example 1
[0080] The difference from Example 1 is that the mass of HZSM-5 molecular sieve is 200 g, the mass of the mixture of pseudo-boehmite and alumina is 41 g, and finally the HZSM-5 molecular sieve catalyst is obtained, wherein the mass ratio of HZSM-5 molecular sieve to binder is 80:16.4.
[0081] Performance Testing
[0082] The catalysts prepared in the above examples and comparative examples were tested using a methanol to propylene reaction catalyst evaluation device. The schematic diagram of the methanol to propylene reaction catalyst evaluation device is shown in FIG. Figure 2 As shown, specifically, the reaction liquid is introduced into the reactor 1 by using a feed pump, and nitrogen is introduced into the reactor at the same time, glass beads are filled in the upper section 4 of the reactor and the lower section 6 of the reactor, and the catalyst is filled in the middle section 5 of the reactor.
[0083] The schematic diagram of catalyst loading is shown in Figure 3 As shown, the distance between the feed port 1 of the reactor and the uppermost end of the middle section 5 of the reactor is 28 cm. The gaseous product after the reaction of the reaction liquid and the catalyst is condensed through the condenser 2 to obtain a liquid product, and the gaseous product is analyzed by gas chromatography. Among them, the size of the reactor 1 is: 20mm*12mm*400mm, the filling mass of the catalyst is 5g, the particle size of the catalyst is 10-20 mesh, the particle size of the glass beads is 2-3mm, and the bottom of the reactor 1 is sealed with a filter. The patrol thermocouple is inserted in the middle of the catalyst bed to detect the actual reaction temperature in real time. The feed space velocity is 1h -1, the reaction temperature is 480℃, sampling starts after 5 hours of operation, the sampling frequency is 2 hours / time, and all components are analyzed online. After the operation time reaches 24 hours, the airspeed is adjusted to 2h -1 , after the running time reaches 48h, adjust the airspeed to 3h -1 The experiment was stopped at this air velocity until the methanol conversion rate was ≤95%, which was considered as catalyst deactivation. The sampling frequency remained unchanged during the experiment. The activity and life of the catalyst were tested during the experiment. The catalyst was deactivated and unloaded for catalysis, and the powderization rate was tested.
[0084] Acid Site Test
[0085] The acidity determination was carried out on a BELCAT-II atmospheric pressure chemical adsorption instrument, with high-purity helium as the carrier gas, a flow rate of 50L / min, and a catalyst loading of 0.05g. The catalyst was activated by heating the temperature from room temperature to 550℃ at a rate of 10℃ / min, maintaining for 1h, cooling to 100℃ to adsorb ammonia to saturation, purging for 20min to remove physically adsorbed NH3, and then heating to 610℃ at a rate of 10℃ / min, and recording the desorption curve. The acidity of the catalyst sample was quantitatively measured by passing an ammonia-helium mixture through a flowmeter, detecting it with a thermal conductivity detector (TCD), and integrating the peak area to make a calibration curve of the amount of ammonia versus the peak area. The test sample adsorbed ammonia at 100℃. After the adsorption was completed, the temperature was programmed to rise to 610℃ at a rate of 10℃ / min to desorb the ammonia adsorbed by the sample, detecting it with TCD, integrating the desorption peak, and calculating the amount of desorbed ammonia based on the desorption peak area, that is, the amount of acidic sites.
[0086] The catalysts prepared in the above examples and comparative examples were tested for acid sites, compressive strength, specific surface area, porosity, pore size, pore size distribution, life and pulverization rate. The results are shown in Table 1.
[0087] Table 1
[0088]
[0089]
[0090] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0091] The catalyst of the present application includes HZSM-5 molecular sieve and binder, HZSM-5 molecular sieve has suitable pore size and high catalytic activity, the role of binder is to bind particles of HZSM-5 molecular sieve to form a catalyst with higher catalytic activity, preferably controlling the mass ratio of HZSM-5 molecular sieve to binder within the above range, so that the pore size distribution of the catalyst is more uniform, on the one hand, it helps to improve the force uniformity of the catalyst, so that the present application has the above range of compressive strength, thereby reducing the probability of the catalyst being crushed due to uneven force during the catalytic process; on the other hand, it helps to provide more catalytic active sites for the catalyst, thereby improving the catalytic activity of the catalyst. Therefore, the catalyst of the present application has a strong ability to resist carbon deposition and pulverization.
[0092] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A HZSM-5 molecular sieve catalyst, characterized in that: The HZSM-5 molecular sieve catalyst comprises an HZSM-5 molecular sieve and a binder, wherein the binder is located between particles of the HZSM-5 molecular sieve, the mass ratio of the HZSM-5 molecular sieve to the binder is 75-80:20-25, and the compressive strength of the HZSM-5 molecular sieve catalyst is 9.5-12 N / mm.
2. The HZSM-5 molecular sieve catalyst according to claim 1, characterized in that: The binder is selected from any one or more of pseudo-boehmite, SB powder and alumina; further, the binder is preferably a mixture of pseudo-boehmite and alumina, and the mass ratio of the pseudo-boehmite to the alumina is 3-5:7-10.
3. The HZSM-5 molecular sieve catalyst according to claim 1 or 2, characterized in that: The amount of acid sites of the HZSM-5 molecular sieve catalyst is 0.02 to 0.03 mmol / g; and / or the specific surface area of the HZSM-5 molecular sieve catalyst is 325 to 340 m 2 / g; and / or, the porosity of the HZSM-5 molecular sieve catalyst is 45% to 55%; and / or, the average pore size of the HZSM-5 molecular sieve catalyst is 3.5 to 4.5 nm.
4. A method for preparing the HZSM-5 molecular sieve catalyst according to any one of claims 1 to 3, characterized in that: The preparation method comprises: The raw materials including HZSM-5 molecular sieve, binder, pore expanding agent, extrusion aid and nitric acid aqueous solution are mixed and then sequentially subjected to extrusion molding, drying treatment and calcination treatment to obtain the HZSM-5 molecular sieve catalyst.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the HZSM-5 molecular sieve, the pore-enlarging agent, the extrusion aid and the nitric acid aqueous solution is 75-80: 3-3.5: 2.5-3: 1.7-2.5; and / or the mass concentration of the nitric acid aqueous solution is 3.5-5wt%.
6. The preparation method according to claim 4 or 5, characterized in that: The silicon-aluminum ratio of the HZSM-5 molecular sieve is 300-500:1; and / or the particle size of the HZSM-5 molecular sieve is 250-300 mesh; and / or the particle size of the binder is 450-500 mesh, and preferably the ratio of the particle size of the binder to the particle size of the HZSM-5 molecular sieve is 46-48:26-28.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The pore expanding agent is sesbania powder, and the dynamic viscosity of the sesbania powder is 2000-3000 cP; and / or, the extrusion aid is selected from any one or more of glycerol, polyacrylamide and silicone resin; preferably, the extrusion aid is glycerol.
8. The preparation method according to any one of claims 4 to 7, characterized in that The drying temperature is 60-80° C. and / or the drying time is 4-8 hours.
9. The preparation method according to any one of claims 4 to 8, characterized in that: The calcination temperature is 500-550° C.; and / or the calcination time is 6-8 hours.
10. A reaction of preparing propylene from methanol using a catalyst, characterized in that: The catalyst is the HZSM-5 molecular sieve catalyst according to any one of claims 1 to 3.
Citation Information
Patent Citations
Catalyst for preparing propylene from methanol or dimethyl ether and method of use thereof
CN101406846A
ZSM-5 molecular sieve catalyst for preparing propylene by conversion of methanol and preparation method thereof
CN101940942A
Molded molecular sieve catalyst and preparation method and application thereof
CN104923284A
Method used for regulating molecular sieve moulding strength and acidity
CN109896532A
Direct forming method of methanol-to-propylene catalyst
CN111921553A