Powder alloy Damascus steel and preparation process thereof
Through hot rolling process and partition layer technology, the problems of low production efficiency and high cost of Damascus steel are solved, and the production of high strength, high hardness and beautiful Damascus steel is achieved, which improves production efficiency and reduces costs.
Patent Information
- Application Number
- CN202411064982.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
The existing Damascus steel production process has problems of low production efficiency and high production costs, especially when using powder alloy technology, 3D models and thermal isostatic pressing processes need to be designed, resulting in unsatisfactory efficiency and cost.
Damascus steel is produced through hot rolling process by using alloy powder, and the partition plate of the partition layer and alloy powder of different thicknesses are laminated, combined with hot rolling composite and torsion processes to form high-strength, high hardness and beautiful Damascus pattern.
The production of Damascus steel with high strength, high hardness and beautifulness has been achieved, avoiding stratification, improving production efficiency and reducing costs.
Smart Images

Figure CN118951024A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a powder alloy Damascus steel and a preparation process thereof. Background Art
[0002] Powder alloy materials have unique chemical compositions and physical and mechanical properties that cannot be obtained by traditional melting and casting processes, such as controllable porosity, uniform material structure, no macroscopic segregation, and one-time molding, which make powder alloy materials have excellent properties such as high strength, high hardness, high wear resistance, and high corrosion resistance. Powder alloy technology can easily achieve various types of composites and give full play to the characteristics of each component material. It is a low-cost process technology for producing high-performance metal-based composite materials.
[0003] Damascus steel was once the king of cold weapons. Traditional Damascus steel is made of two or more steels that are repeatedly stacked and forged. It has excellent toughness, high strength and high wear resistance. After grinding and etching, the surface presents a beautiful Damascus pattern.
[0004] The use of powder alloy technology and high-performance powder alloy materials to prepare new powder alloy Damascus steel can obtain composite materials with better performance. In the patent CN114833340A, a 3D model needs to be designed according to the texture requirements of Damascus steel, and then a binder injection molding process is performed to obtain a blank, and finally a hot isostatic pressing process is used for molding, which has problems such as low production efficiency and high production cost.
[0005] The present invention adopts the hot rolling process to produce powder alloy Damascus steel, which has the advantages of high production efficiency and low production cost, and has positive significance for promoting the development of my country's high-performance composite materials industry. Summary of the invention
[0006] In view of the above problems, the present invention provides a powder alloy Damascus steel and a preparation process thereof. The alloy powder is used as a raw material and Damascus steel is produced through a hot rolling process. The material can have the advantages of both Damascus steel and powder alloy steel, and has the advantages of high strength, high hardness and high toughness.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A powder alloy Damascus steel is formed by assembling and hot-rolling two or more alloy powders with different components, wherein there is a separation layer between the different alloy powders. The alloy powders contain the following components: C: 0.5-2.0%, Cr: 13-20%, Mo: 2-5%, V: 0.5-5%, and Co: 0-2%.
[0009] Furthermore, the separation layer is a separation plate selected from 3Cr13, 4Cr13, 5Cr15 stainless steel, and its alloy composition is similar to that of a powder in contact with it, or its corrosion resistance is similar to that of a powder in contact with it.
[0010] Furthermore, the thickness of the separation layer is less than or equal to the thickness of the thinnest layer of adjacent powders.
[0011] Preferably, the thickness of the separation layer is less than or equal to 1 / 2 of the thickness of the thinnest layer of adjacent powders.
[0012] Furthermore, the layer thickness ratio of the two adjacent powders is 1:1-5, and the thickness ratios of the powders at different positions may be the same or different.
[0013] A preparation process of powder alloy Damascus steel comprises the following steps:
[0014] S1, cleaning of the partition plate surface: using physical or chemical methods to remove oil, oxides and impurities on the partition plate surface;
[0015] S2, blank assembly: put the cleaned separator and the prepared alloy powder into a clean package box in sequence, one layer of separator and one layer of alloy powder, with separators placed between different alloy powders, and finally cover with the package cover plate;
[0016] S3, powder pre-pressing: the package box is placed in a pressure device for 20-90 minutes, and the unit pressure is 10-100MPa to press the powder to obtain a composite blank;
[0017] S4, vacuum packaging: the composite blank is sent into the vacuum packaging equipment, the air in the package box is removed by vacuuming, and then the package box is sealed and welded;
[0018] S5, hot rolling: heating the composite blank after the treatment in step S4 to 1000-1150°C, keeping the temperature for 2-4 hours and then hot rolling, the starting rolling temperature is 980-1100°C, and the total deformation of hot rolling is greater than 85%;
[0019] S6, slitting: slitting the hot-rolled billet into a size that meets the subsequent processing, and the shape is a rod-shaped or strip-shaped intermediate billet;
[0020] S7, twisting: heating the rod-shaped or strip-shaped intermediate billet to 900-1100°C and twisting it on a twisting device to obtain a rod;
[0021] S8, machining: turning, milling or grinding the bar obtained after twisting to remove surface oxide scale and impurities, and processing to the required size and specifications;
[0022] S9, etching treatment: soak the machined rod with a smooth surface in an acidic solvent for 2-30 minutes to obtain powder alloy Damascus steel, wherein the acidic solution is a mixed acid of sulfuric acid and hydrochloric acid, with a sulfuric acid concentration of 10% and a hydrochloric acid concentration of 3-10%.
[0023] Furthermore, the blank assembly in step S2 can be 5 layers, 9 layers or more layers, the alloy powder can also be two or more components, and its partition plate can be one or more materials; the alloy powder is not in contact with the sleeve, and the bottom layer and the top layer in the sleeve are both partition plates; the sleeve box material is selected from 5-20mm carbon steel or low alloy steel material.
[0024] Furthermore, the heating method in step S5 is staged heating. The first stage is rapid heating from room temperature to 750-800°C, with a heating rate of 100-150°C / h, and keeping warm for 2-4h. The second stage is continuing to heat to 1000-1150°C, with a heating rate of 50-80°C / h.
[0025] Furthermore, in step S5, the hot rolling adopts alternating flat rolling and vertical rolling for the first 10 passes, and the cross-sectional deformation of the 10 passes is greater than 30%, and the hot rolling speed of the first 10 passes is 10-60 m / min.
[0026] Furthermore, in step S7, the pitch of the bar after twisting is less than 4 cm, and the number of twisting turns per meter of the bar is greater than 25 turns.
[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) the present invention uses alloy powder as raw material and produces Damascus steel through hot rolling process, so that the material has the advantages of both Damascus steel and powder alloy steel, and has the advantages of high strength, high hardness and high toughness;
[0028] (2) The present invention uses different alloy powders to stack different thicknesses, and after hot rolling, compounding and twisting, a rich and beautiful Damascus pattern can be obtained;
[0029] (3) In the present invention, a partition plate with a similar composition or corrosion resistance to a powder material is placed between different powder layers, so that the pattern after etching is more distinct, and the junction will not be blurred in color or have a clear transition zone;
[0030] (4) The partition layer used in the production of powder alloy Damascus steel of the present invention is made of stainless steel. During hot rolling, due to the presence of non-metallic inclusions (mainly sulfides, oxides and silicates), it is pressed into thin sheets and delamination occurs. Delamination greatly deteriorates the tensile performance of the steel along the thickness direction, making it more likely to crack or break during hot rolling, affecting the processing performance. Moreover, for materials such as Damascus steel that focus on appearance and texture, delamination will destroy its unique pattern, affecting its appearance and commercial value. Therefore, segmented heating is used before hot rolling to ensure that the steel billet is heated evenly before hot rolling, reduce internal stress and uneven distribution of inclusions, and clean the surface of the steel billet before hot rolling to remove surface inclusions and oxide scale. During hot rolling, the rolling speed is appropriately controlled to avoid uneven deformation of inclusions caused by excessively fast rolling speed, thereby avoiding delamination. The present invention adopts hot rolling process to produce powder alloy Damascus steel, which has the advantages of high production efficiency and low production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The cross-sectional structure diagram of the powder alloy Damascus steel composite billet, wherein 1 is the jacket steel plate, 2 is the alloy powder 2, 3 is the separation layer, 4 is the alloy powder 1, and 5 is the welding point;
[0032] Figure 2 This is a physical picture of the powder alloy Damascus steel produced in Example 1;
[0033] Figure 3 This is a physical picture of the powder alloy Damascus steel produced in Example 2. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the technical solution, the present invention is described in detail below in conjunction with embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.
[0035] Embodiment 1:
[0036] A preparation process of M390+8Cr13MoV powder alloy Damascus steel comprises the following steps:
[0037] 1. Surface cleaning of the raw materials of the separation layer steel plate: 3Cr13 steel plate is selected as the separation layer, and ultrasonic cleaning is used to remove oil and impurities on the surface of 3Cr13 stainless steel;
[0038] 2. Billet assembly: Put the cleaned partition plate and the prepared alloy powder into a clean bag box in turn, put a piece of 3Cr13 stainless steel at the bottom of the bag box, and then put the plates into the bag box in the order of a layer of M390 powder, 3Cr13 stainless steel, a layer of 8Cr13MoV powder, and a layer of 3Cr13 stainless steel. The thickness of 3Cr13 stainless steel is 1mm, the thickness of M390 powder is 5mm, and the thickness of 8Cr13MoV powder is 5mm. The two powders are paved 25 layers each, with a total thickness of 301mm. After filling, cover the upper end cover of the bag. The bag box is welded with 15mm thick Q235 low carbon steel. The five sides of the bag are welded with gas shielded welding, and the upper end opening is reserved for filling raw materials;
[0039] 3. Powder pre-pressing: put the package box as a whole into the pressure equipment, and apply pressure to the powder through the end cover plate, with a unit pressure of 40MPa, press for 40min, and press the powder to obtain the composite blank;
[0040] 4. Vacuum packaging: send the composite blank into the vacuum equipment, and remove the air in the package box by vacuuming, with a vacuum degree of 10Pa. Then use an electron beam welder to weld the end cover plate for sealing;
[0041] 5. Hot rolling: the vacuum-encapsulated powder alloy composite billet is heated to 1100°C, kept warm for 3 hours, and then hot rolled. The starting rolling temperature is 1050°C. The billet is hot rolled into a plate with a thickness of 15 mm. The total reduction of hot rolling is 95%. The heating method is segmented heating. The first stage is to quickly heat from room temperature to 780°C at a heating rate of 120°C / h and keep warm for 3 hours. The second stage is to continue to heat to 1100°C at a heating rate of 55°C / h. The hot rolling adopts the first 10 passes of alternating flat rolling and vertical rolling, and the cross-sectional deformation of 10 passes is 52%. The hot rolling speed of the first 10 passes is 35m / min.
[0042] 6. Cutting: Cut the hot-rolled billet into 15*15*1000mm rod-shaped materials;
[0043] 7. Twisting: Heat the rod-shaped intermediate billet to 1000°C and twist it on a twisting device for 32 turns;
[0044] 8. Machining: The twisted bar is turned to remove surface oxide scale and impurities, and processed to the required size and specifications;
[0045] 9. Etching treatment: The rod material with a smooth surface after machining is placed in a mixed acid solution of 10% H2SO4 + 10% HCl and soaked for 5 minutes to obtain powder alloy Damascus steel.
[0046] Embodiment 2:
[0047] A preparation process of 10Cr15CoMoV+6Cr13 powder alloy Damascus steel comprises the following steps:
[0048] 1. Surface cleaning of the raw materials of the separation layer steel plate: 3Cr13 steel plate is selected as the separation layer, and ultrasonic cleaning is used to remove oil and impurities on the surface of 3Cr13 stainless steel;
[0049] 2. Assembly of blanks: put the cleaned partition plate and the prepared alloy powder into a clean bag box in sequence, put a piece of 3Cr13 stainless steel at the bottom of the bag box, and then put the plates into the bag box in the order of a layer of 10Cr15CoMoV powder, 3Cr13 stainless steel, a layer of 6Cr13 powder, and a layer of 3Cr13 stainless steel. The thickness of 3Cr13 stainless steel is 1mm, the thickness of each layer of 5 layers of 10Cr15CoMoV powder in the lower and upper layers is 6mm, the thickness of each layer of 5 layers of 6Cr13 powder in the lower and upper layers is 4mm, the thickness of each layer of 10 layers of 10Cr15CoMoV powder in the middle is 3mm, the thickness of each layer of 10 layers of 6Cr13 powder in the middle is 6mm, and the total thickness is 231mm. After filling, cover the upper end cover of the bag, and lay 20 layers of each of the two powders. The bag box is welded with 10mm thick Q355 low alloy, and the 5 surfaces of the bag are welded with gas shielded welding, and the upper end face opening is reserved for filling raw materials;
[0050] 3. Powder pre-pressing: put the package box as a whole into the pressure equipment, and apply pressure to the powder through the end cover plate, with a unit pressure of 50MPa, press for 30 minutes, and press the powder to obtain the composite blank;
[0051] 4. Vacuum packaging: send the composite blank into the vacuum equipment, and remove the air in the package box by vacuuming, with a vacuum degree of 10Pa. Then use an electron beam welder to weld the end cover plate for sealing;
[0052] 5. Hot rolling: the vacuum-encapsulated powder alloy composite billet is heated to 1100°C, kept warm for 3 hours, and then hot rolled. The starting rolling temperature is 1050°C. The billet is hot rolled into a plate with a thickness of 12 mm. The total hot rolling reduction is 94.8%. The heating method is segmented heating. The first stage is rapid heating from room temperature to 800°C, the heating rate is 150°C / h, and the temperature is kept for 4 hours. The second stage is to continue heating to 1100°C, the heating rate is 50°C / h, and the hot rolling adopts the first 10 passes of flat rolling and vertical rolling alternately, and the cross-sectional deformation of 10 passes is 48%. The hot rolling speed of the first 10 passes is 40m / min;
[0053] 6. Cutting: Cut the hot-rolled billet into 12*12*1000mm rod-shaped materials;
[0054] 7. Twisting: Heat the rod-shaped intermediate billet to 1100°C and twist it on a twisting device for 40 turns;
[0055] 8. Machining: The twisted bar is turned to remove surface oxide scale and impurities, and processed to the required size and specifications;
[0056] 9. Etching treatment: The rod material with a smooth surface after machining is immersed in a mixed acid solution of 10% H2SO4 + 5% HCl for 8 minutes to obtain powder alloy Damascus steel.
[0057] Embodiment 3:
[0058] A preparation process of 12Cr15Mo4V+8Cr15 powder alloy Damascus steel comprises the following steps:
[0059] 1. Surface cleaning of the raw materials of the separation layer steel plate: 5Cr15 steel plate is selected as the separation layer, and ultrasonic cleaning is used to remove oil and impurities on the surface of 5Cr15 stainless steel;
[0060] 2. Billet assembly: put the cleaned partition plate and the prepared alloy powder into a clean bag box in turn, put a piece of 5Cr15 stainless steel at the bottom of the bag box, and then put the plates into the bag box in the order of a layer of 12Cr15Mo4V powder, 5Cr15 stainless steel, a layer of 8Cr15 powder, and a layer of 5Cr15 stainless steel. The thickness of 5Cr15 stainless steel is 1mm, the thickness of each layer of 10 layers of 12Cr15Mo4V powder in the lower and upper layers is 6mm, the thickness of each layer of 10 layers of 8Cr15 powder in the lower and upper layers is 3mm, the thickness of each layer of 10 layers of 10Cr15CoMoV powder in the middle is 10mm, the thickness of each layer of 10 layers of 8Cr15 powder in the middle is 3mm, and the total thickness is 371mm. After filling, cover the upper end cover of the bag, and lay 30 layers of each of the two powders. The bag box is welded with 13mm thick Q355 low alloy, and the 5 surfaces of the bag are welded with gas shielded welding, and the upper end opening is reserved for filling raw materials;
[0061] 3. Powder pre-pressing: put the package box as a whole into the pressure equipment, and apply pressure to the powder through the end cover plate, with a unit pressure of 60MPa, press for 20min, and press the powder to obtain the composite blank;
[0062] 4. Vacuum packaging: send the composite blank into the vacuum equipment, and remove the air in the package box by vacuuming, with a vacuum degree of 10Pa. Then use an electron beam welder to weld the end cover plate for sealing;
[0063] 5. Hot rolling: the vacuum-encapsulated powder alloy composite billet is heated to 1150°C, kept warm for 2 hours, and then hot rolled. The starting rolling temperature is 1100°C. The billet is hot rolled into a plate with a thickness of 20 mm. The total hot rolling reduction is 94.1%. The heating method is segmented heating. The first stage is to quickly heat from room temperature to 750°C at a heating rate of 100°C / h and keep warm for 4 hours. The second stage is to continue to heat to 1150°C at a heating rate of 80°C / h. The hot rolling adopts the first 10 passes of alternating flat rolling and vertical rolling, and the cross-sectional deformation of the 10 passes is 40%. The hot rolling speed of the first 10 passes is 28m / min;
[0064] 6. Cutting: Cut the hot-rolled billet into 20*20*1000mm rod-shaped materials;
[0065] 7. Twisting: Heat the rod-shaped intermediate billet to 1050°C and twist it on a twisting device for 48 turns;
[0066] 8. Machining: The twisted bar is turned to remove surface oxide scale and impurities, and processed to the required size and specifications;
[0067] 9. Etching treatment: The rod material with a smooth surface after machining is placed in a mixed acid solution of 10% H2SO4 + 5% HCl and soaked for 10 minutes to obtain powder alloy Damascus steel.
[0068] Comparative Example 1:
[0069] The difference between this comparative example and Example 1 is that during hot rolling in step 3, the heating method is direct heating, which is heated to 1100° C. at a uniform speed, and the remaining process steps are the same as those in Example 1.
[0070] Comparative Example 2:
[0071] The difference between this comparative example and Example 1 is that the selected separation layer is a pure iron plate, and the remaining process steps are the same as those in Example 1.
[0072] Comparative Example 3:
[0073] The difference between this comparative example and Example 1 is that the separation layer is made of nickel plate material, and during hot rolling in step 3, the heating method is direct heating, which is heated to 1100° C. at a uniform speed, and the remaining process steps are the same as those in Example 1.
[0074] Performance testing:
[0075] The powder alloy Damascus steel prepared in Examples 1-3 and Comparative Examples 1-3 was quenched at 1000°C and tempered at 200°C. The room temperature hardness was tested using a Rockwell hardness tester, the tensile test was performed using a universal material testing machine, the impact toughness test was performed using a Charpy impact test method, and the metallographic structure was observed using an optical microscope and a scanning electron microscope. The test results are shown in Table 1.
[0076] Table 1
[0077]
[0078]
[0079] It should be noted that, in this article, the terms: include, contain and any other variants are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. Specific examples are used in this article to illustrate the principle and implementation of the technical solution of the present invention. The above examples are only used to help understand the method of the present invention and its core idea. The above is only a preferred implementation of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements, modifications or changes can be made, and the above technical features can also be combined in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the concept and technical solution of the present invention to other occasions without improvement, should be regarded as the protection scope of the present invention.
Claims
1. A powder alloy Damascus steel, It is characterized in that It is formed by assembling and hot-rolling two or more alloy powders with different components, with separation layers between different alloy powders. The components of the alloy powders include: C: 0.5-2.0%, Cr: 13-20%, Mo: 2-5%, V: 0.5-5%, Co: 0-2%.
2. The powder alloy Damascus steel according to claim 1, It is characterized in that The partition layer is a partition plate selected from 3Cr13, 4Cr13, 5Cr15 stainless steel, and its alloy composition is similar to that of a powder in contact with it, or its corrosion resistance is similar to that of a powder in contact with it.
3. The powder alloy Damascus steel according to claim 1, It is characterized in that The thickness of the separation layer is less than or equal to the thickness of the thinnest layer of adjacent powders.
4. The powder alloy Damascus steel according to claim 1, It is characterized in that The thickness of the separation layer is less than or equal to 1 / 2 of the thickness of the thinnest layer of adjacent powders.
5. The powder alloy Damascus steel according to claim 1, It is characterized in that The layer thickness ratio of the two adjacent powders is 1:1-5, and the thickness ratios of the powders at different positions can be the same or different.
6. A process for preparing powder alloy Damascus steel, It is characterized in that The following steps are involved: S1, cleaning of the partition plate surface: using physical or chemical methods to remove oil, oxides and impurities on the partition plate surface; S2, blank assembly: put the cleaned separator and the prepared alloy powder into a clean package box in sequence, one layer of separator and one layer of alloy powder, with separators placed between different alloy powders, and finally cover with the package cover plate; S3, powder pre-pressing: the package box is placed in a pressure device for 20-90 minutes, and the unit pressure is 10-100MPa to press the powder to obtain a composite blank; S4, vacuum packaging: the composite blank is sent into the vacuum packaging equipment, the air in the package box is removed by vacuuming, and then the package box is sealed and welded; S5, hot rolling: heating the composite blank after the treatment in step S4 to 1000-1150°C, keeping the temperature for 2-4 hours and then hot rolling, the starting rolling temperature is 980-1100°C, and the total deformation of hot rolling is greater than 85%; S6, slitting: slitting the hot-rolled billet into a size that meets the subsequent processing, and the shape is a rod-shaped or strip-shaped intermediate billet; S7, twisting: heating the rod-shaped or strip-shaped intermediate billet to 900-1100°C and twisting it on a twisting device to obtain a rod; S8, machining: turning, milling or grinding the bar obtained after twisting to remove surface oxide scale and impurities, and processing to the required size and specifications; S9, etching treatment: soak the machined rod with a smooth surface in an acidic solvent for 2-30 minutes to obtain powder alloy Damascus steel, wherein the acidic solution is a mixed acid of sulfuric acid and hydrochloric acid, with a sulfuric acid concentration of 10% and a hydrochloric acid concentration of 3-10%.
7. A process for preparing powder alloy Damascus steel according to claim 6, It is characterized in that The blank assembly in step S2 can be 5 layers, 9 layers or more layers, the alloy powder can also be two or more components, and the partition plate can be made of one or more materials; the alloy powder is not in contact with the sheath, and the bottom layer and the top layer in the sheath are both partition plates; the sheath box material is selected from 5-20mm carbon steel or low alloy steel.
8. A process for preparing powder alloy Damascus steel according to claim 6, It is characterized in that The heating method in step S5 is staged heating. The first stage is rapid heating from room temperature to 750-800°C at a heating rate of 100-150°C / h and keeping warm for 2-4h. The second stage is continued heating to 1000-1150°C at a heating rate of 50-80°C / h.
9. The process for preparing powder alloy Damascus steel according to claim 6, It is characterized in that In step S5, the hot rolling adopts alternating flat rolling and vertical rolling for the first 10 passes, and the cross-sectional deformation of the 10 passes is greater than 30%, and the hot rolling speed of the first 10 passes is 10-60 m / min.
10. The process for preparing powder alloy Damascus steel according to claim 6, It is characterized in that In step S7, the pitch of the bar after twisting is less than 4 cm, and the number of twisting turns per meter of the bar is greater than 25 turns.