Preparation method for narrow-gap laser welding joint of large-diameter thick-wall pipe with layered design

By using laser additive and cladding technology to form a layered design of 'additive-weld-clad-clad' joint in large-diameter thick-walled pipelines, the problem of performance loss of welded joints is solved, and internal corrosion resistance and external high temperature resistance are achieved The performance improvement extends the service life of oil pipelines and improves safety.

CN118951318AActive Publication Date: 2024-11-15NANJING UNIV OF AERONAUTICS & ASTRONAUTICS

Patent Information

Application Number
CN202411146888.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The chemical composition and tissue morphology of large-diameter thick-wall pipe welded joints during rapid heating, melting and cooling and solidification, resulting in performance losses, which cannot meet the complex service requirements of internal corrosion resistance and external high temperature resistance, limiting the service life and safety of petroleum pipelines. sex.

Method used

Using a layered design, a corrosion-resistant additive layer is prepared inside the pipeline through laser additive technology, and a high-temperature resistant cladding layer is prepared outside the pipeline, and it is closely combined with the weld filling layer in the middle of the pipeline to form an additive- Welding-clad' composite narrow gap laser forming joints to improve performance in different areas.

Benefits of technology

The targeted performance improvement of the laser welded joints of large-diameter thick-walled pipes is achieved, meeting the requirements of internal corrosion resistance and external high temperature resistance of the pipeline, extending service life and improving safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951318A_ABST
    Figure CN118951318A_ABST
Patent Text Reader

Abstract

The invention discloses a layered design large-diameter thick-wall pipe narrow-gap laser welding joint preparation method, which specifically designs the internal and external performances of a pipeline welding joint, prepares a corrosion-resistant additive layer in a pipeline by adopting a laser additive technology, prepares a high-temperature-resistant cladding layer outside the pipeline by adopting a laser cladding technology, and prepares a large-diameter thick-wall pipe narrow-gap laser welding joint. And the laser beams are tightly combined with a pipeline middle weld joint filling layer in sequence to form the'material adding-welding-cladding 'composite narrow-gap laser forming joint. The method comprises the following steps: 1, preparing a corrosion-resistant additive bottoming layer in the pipeline; 2, preparing a welding filling layer in the middle of the pipeline; and 3, preparing a high-temperature-resistant fusion covering surface layer outside the pipeline. According to the method, performance targeted design can be conducted on the weld joint according to the difference of service conditions of different parts of the large-diameter thick-wall pipe laser welding joint, the inherent problem of performance loss of the welding joint is solved, the service life of a petroleum pipeline is prolonged, and safety of the petroleum pipeline is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a large-diameter thick-walled pipe narrow-gap laser welding joint, and in particular to a layered design preparation method of a large-diameter thick-walled pipe narrow-gap laser welding joint with internal corrosion resistance and external high temperature resistance, which can be applied to the welding process of oil transportation pipelines and belongs to the field of corrosion and protection. Background Art

[0002] With the continuous development of modern technology, the demand for steel pipes is increasing, and large-diameter thick-walled pipes, as a high-quality and high-efficiency pipeline material, are widely used in various fields. Large-diameter thick-walled pipes have the advantages of high strength, high rigidity, wear resistance, pressure resistance, and corrosion resistance. Therefore, they are widely used in the construction of long-distance pipelines such as oil, natural gas, and chemical raw materials in the field of energy and chemical industry. The special service environment of such transportation pipelines puts forward different requirements for their internal and external performance. Since the chemical raw materials such as petroleum transported are mostly flammable, explosive, and corrosive substances, the inside of the pipeline needs to have excellent corrosion resistance. At the same time, since the transportation pipeline often needs to withstand high pressure, high temperature and other harsh environments, the outside of the pipeline needs to have good high temperature resistance. However, due to the rapid heating, melting, cooling and solidification process, the chemical composition and organizational morphology of the welding parts between the pipelines have changed, resulting in obvious performance loss at the welding joints of the pipelines, which becomes the weak performance part of the transportation pipeline, thus seriously limiting the service life and safety of the oil pipeline.

[0003] With the help of the concept of layered design, the internal and external performances of the narrow gap laser welding joints of large-diameter thick-walled pipes are designed. The laser additive technology is used to prepare the corrosion-resistant additive layer inside the pipe, and the laser cladding technology is used to prepare the high-temperature resistant cladding layer outside the pipe. These layers are tightly combined with the weld filling layer in the middle of the pipe in turn to form an "additive-welding-cladding" composite narrow gap laser formed joint, which can achieve targeted improvement of the performance of different areas of the narrow gap laser welding joints of large-diameter thick-walled pipes. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for preparing narrow gap laser welding joints of large-diameter thick-walled pipes with a layered design, in which a corrosion-resistant additive layer is prepared inside the pipe by laser additive technology, and a high-temperature resistant cladding layer is prepared outside the pipe by laser cladding technology, and the layers are tightly combined with the weld filling layer in the middle of the pipe in sequence to form an "additive-welding-cladding" composite narrow gap laser formed joint, which specifically improves the performance of different areas of narrow gap laser welding joints of large-diameter thick-walled pipes.

[0005] The present invention is achieved through the following technical solutions:

[0006] The present invention provides a method for preparing a narrow gap laser welding joint of a large-caliber thick-walled tube with a layered design, characterized in that the preparation method comprises the following steps:

[0007] (1) A laser scanner is used to collect the geometric dimensions of the stainless steel pipe groove to be welded and perform image processing to construct the corresponding stainless steel pipe groove model;

[0008] (2) determining the laser focus position based on the pipeline groove model, inputting the corrosion-resistant additive layer process parameters, completing the preparation of the corrosion-resistant additive layer, and obtaining the corresponding corrosion-resistant additive layer height;

[0009] (3) calculating the laser focus offset height of the welding filling layer based on the height of the corrosion-resistant additive base layer, completing the adjustment of the laser focus position, inputting the welding process parameters of the filling layer, completing the preparation of the welding filling layer, obtaining the corresponding weld filling layer height, calculating the total weld height, and when the total weld height is greater than the groove height, proceeding to the next step, otherwise repeating the weld filling layer welding process;

[0010] (4) calculating the laser focus offset height of the high temperature resistant molten cover layer based on the height of the weld cap layer, completing the adjustment of the laser focus position, inputting the corrosion resistant cap layer cladding process parameters, and completing the preparation of the corrosion resistant molten cover layer;

[0011] Furthermore, the size model of the corrosion-resistant additive base layer / welding filling layer / high-temperature resistant molten metal covering layer is a relationship model between the cross-sectional area, weld width and excess height of a single additive / weld / cladding layer and the wire / powder feeding speed, laser power and scanning / welding / cladding speed, and its mathematical expression formula is as follows:

[0012] S d =a1P+b1v w +c1v f

[0013] h d =a2P+b2v w +c2v f

[0014] D d =a3P+b3v w +c3v f

[0015] Among them, S d 、h d , D d ,P,v w and v fare the cross-sectional area of ​​single-pass additive / weld / cladding layer, excess height, weld width, laser power, scanning / welding / cladding speed, and wire / powder feeding speed, respectively. a1, a2, a3, b1, b2, b3, c1, c2, and c3 are constants and are related to the material;

[0016] Furthermore, the input of the process parameters of the base layer additive / filling layer welding / capping layer cladding is realized through the interrelated additive process knowledge base, welding process knowledge base and cladding process knowledge base, and a corresponding base layer / filling layer / capping layer size model is established based on the process parameters to obtain the corresponding additive / weld / cladding layer height, including:

[0017] Extracting the blunt edge and the size of the groove gap of the groove based on the established pipeline groove model, querying the laser additive process knowledge base, and obtaining the corrosion-resistant base additive process parameters;

[0018] Based on the corrosion-resistant base layer additive / filling layer welding / high-temperature-resistant cover layer cladding process parameters, a size model of the corrosion-resistant additive base layer / welding filling layer / high-temperature-resistant molten cover layer is established to obtain the height of the corrosion-resistant additive base layer / welding filling layer / high-temperature-resistant molten cover layer;

[0019] Furthermore, the height of the corrosion-resistant additive layer and the height of the laser focus offset of the welding filling layer are solved according to the following equations, and the specific equations are as follows:

[0020]

[0021] h l1 =h1

[0022] Among them, D d1 , S d1 , d, h1 and h l1 They are respectively expressed as the additive base layer melt width, the additive base layer cross-sectional area, the groove bottom width, the corrosion-resistant additive base layer height and the welding filling layer laser focus offset height;

[0023] Furthermore, the height of the welding filling layer and the height of the laser focus offset of the next welding filling layer are solved according to the following equations, and the specific equations are as follows:

[0024]

[0025] h li =h 1+i

[0026] Among them, D d1+i , D di 、h 1+i , S d1+i and h liThey are respectively represented as the molten width of the i-th welding filling layer, the molten width of the i-1-th welding filling layer, the weld height of the i-th welding filling layer, the cross-sectional area of ​​the i-th welding filling layer and the laser focus offset height of the next welding filling layer;

[0027] Furthermore, the total height of the weld is solved according to the following equation, and the specific equation is as follows:

[0028] H=∑h i i=1,2,3...,n

[0029] Where H represents the total height of the weld.

[0030] Furthermore, the total height of the weld satisfies H≥H h When the welding process of the filling layer is completed;

[0031] Furthermore, the height of the welding capping layer and the laser focus offset height of the high temperature resistant melt-covering layer are solved according to the following equations, and the specific equations are as follows:

[0032] h ln =h 1+n

[0033] Among them, h 1+n and h ln They are respectively expressed as the height of the welding cover layer and the height of the laser focus offset of the high temperature resistant melt cover layer;

[0034] Furthermore, the pipeline groove model mainly includes: groove bottom width d, groove height H h and blunt edge h0.

[0035] Furthermore, the corrosion-resistant additive base layer is mainly prepared by adding a small amount of nano-Ta particles through a laser additive process.

[0036] Furthermore, the high temperature resistant molten metal covering surface layer is mainly prepared by laser cladding TiC nanowires.

[0037] Furthermore, the corrosion-resistant additive base layer, welding filling layer, and corrosion-resistant welded covering surface layer are all simplified into a trapezoid.

[0038] The beneficial effects of the present invention are as follows: in view of the fact that the performance loss of the narrow gap laser welding joint of the large-diameter thick-walled pipe causes the weak performance part to be unable to meet the complex service requirements of the transportation pipeline that the inside needs to be corrosion-resistant and the outside needs to be high-temperature resistant, the method adopts laser additive technology to prepare a corrosion-resistant additive layer inside the pipeline, and adopts laser cladding technology to prepare a high-temperature resistant cladding layer outside the pipeline, and these are tightly combined with the middle weld filling layer of the pipeline in turn to form an "additive-welding-cladding" composite narrow gap laser formed joint, so as to achieve targeted improvement of the performance of different areas of the narrow gap laser welding joint of the large-diameter thick-walled pipe, thereby improving its service performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a flow chart of preparing the narrow gap laser welding layered design joint of large diameter thick wall pipe according to the present invention;

[0040] Figure 2 It is a schematic diagram of a layered design joint for narrow gap laser welding of a large-diameter thick-walled tube according to the present invention;

[0041] Figure 3 It is a schematic diagram of the corrosion-resistant additive base layer of the narrow gap laser welding joint of the large-diameter thick-walled tube described in the present invention;

[0042] Figure 4 It is a schematic diagram of the high temperature resistant melt covering surface layer of the narrow gap laser welding joint of the large diameter thick wall pipe described in the present invention;

[0043] In the figure, 1-pipe groove; 2-pipe I to be welded; 3-pipe II to be welded; 4-corrosion-resistant additive base layer; 5-welding filling layer; 6-welding cover layer; 7-high-temperature resistant melt cover layer; 8-nano Ta particles; 9-laser beam; 10-TiC nano welding wire. DETAILED DESCRIPTION

[0044] The present invention provides a method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design. In order to make the purpose, effect and technical solution of the present invention more distinct, the present invention is described in detail with reference to the accompanying drawings and examples. It should be understood that the specific implementation described herein is only used to explain the present invention and is not used to limit the present invention. For the convenience of description, only the parts related to the present invention are shown in the accompanying drawings instead of all structures.

[0045] The following is combined with Figure 1 , 2 , 3 and 4 are specific descriptions of a method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design according to the present invention:

[0046] Narrow gap laser welding and laser cladding experiments were conducted on large-diameter thick-walled pipes. The dimensions of the pipes I (2) and II (3) to be welded were OD: 1088mm, ID: 900mm, and L: 400mm. The experiment used an RFL-C12000XZ laser with a maximum output power of 12000W and an IPGD50 laser head to complete the narrow gap laser additive, welding, and cladding processes.

[0047] Combination Figure 1 The flowchart shown and Figure 2 The schematic diagram of the welded joint shown in the figure shows a method for preparing a narrow gap laser welded joint of a large-diameter thick-walled tube with a layered design, comprising the following steps:

[0048] (1) using a laser scanner to collect geometric dimensions of the stainless steel pipe groove (1) to be welded and performing image processing to construct a corresponding stainless steel pipe groove model;

[0049] (2) determining the laser focus position based on the pipeline groove model, inputting the corrosion-resistant additive layer process parameters, completing the preparation of the corrosion-resistant additive layer (4), and obtaining the corresponding corrosion-resistant additive layer height;

[0050] (3) calculating the laser focus offset height of the welding filling layer based on the height of the corrosion-resistant additive base layer, completing the adjustment of the laser focus position, inputting the welding process parameters of the filling layer, completing the preparation of the welding filling layer (5), obtaining the corresponding weld filling layer height, calculating the total weld height, and when the total weld height is greater than the groove height, proceeding to the next step, otherwise repeating the weld filling layer welding process;

[0051] (4) calculating the laser focus offset height of the high temperature resistant molten cover layer based on the height of the weld cap layer, completing the adjustment of the laser focus position, inputting the corrosion resistant cap layer cladding process parameters, and completing the preparation of the corrosion resistant molten cover layer (7);

[0052] Specifically, the size model of the corrosion-resistant additive base layer / welding filling layer / high-temperature resistant cladding surface layer is a relationship model between the cross-sectional area, weld width and excess height of a single-pass additive / weld / cladding layer and the wire / powder feeding speed, laser power and scanning / welding / cladding speed, and its mathematical expression formula is as follows:

[0053] S d =a1P+b1v w +c1v f

[0054] h d =a2P+b2v w +c2v f

[0055] D d =a3P+b3v w +c3v f

[0056] Among them, S d 、h d , D d ,P,v w and v f are the cross-sectional area of ​​single-pass additive / weld / cladding layer, excess height, weld width, laser power, scanning / welding / cladding speed, and wire / powder feeding speed, respectively. a1, a2, a3, b1, b2, b3, c1, c2, and c3 are constants and are related to the material;

[0057] Specifically, the input of the process parameters of the base additive / filling layer welding / capping layer cladding is realized through the interrelated additive process knowledge base, welding process knowledge base and cladding process knowledge base, and the corresponding base additive / filling layer / capping layer size model is established based on the process parameters to obtain the corresponding additive / weld / cladding layer height, including:

[0058] Extracting the blunt edge and the size of the groove gap of the groove based on the established pipeline groove model, querying the laser additive process knowledge base, and obtaining the corrosion-resistant base additive process parameters;

[0059] Based on the corrosion-resistant base layer additive / filling layer welding / high-temperature-resistant cover layer cladding process parameters, a size model of the corrosion-resistant additive base layer / welding filling layer / high-temperature-resistant molten cover layer is established to obtain the height of the corrosion-resistant additive base layer / welding filling layer / high-temperature-resistant molten cover layer;

[0060] Specifically, the height of the corrosion-resistant additive layer and the height of the laser focus offset of the welding filling layer are solved according to the following equations, and the specific equations are as follows:

[0061]

[0062] h l1 =h1

[0063] Among them, D d1 , S d1 , d, h1 and h l1 They are respectively expressed as the additive base layer melt width, the additive base layer cross-sectional area, the groove bottom width, the corrosion-resistant additive base layer height and the welding filling layer laser focus offset height;

[0064] Specifically, the height of the welding filling layer and the height of the laser focus offset of the next welding filling layer are solved according to the following equations, and the specific equations are as follows:

[0065]

[0066] h li =h 1+i

[0067] Among them, D d1+i , D di 、h 1+i , S d1+i and h li They are respectively represented as the molten width of the i-th welding filling layer, the molten width of the i-1-th welding filling layer, the weld height of the i-th welding filling layer, the cross-sectional area of ​​the i-th welding filling layer and the laser focus offset height of the next welding filling layer;

[0068] Specifically, the total height of the weld is solved according to the following equation, and the specific equation is as follows:

[0069] H=∑h i i=1,2,3...,n

[0070] Where H represents the total height of the weld.

[0071] Specifically, the total height of the weld satisfies H≥H h When the welding process of the filling layer is completed;

[0072] Specifically, the height of the welding capping layer and the laser focus offset height of the high temperature resistant melt-covering layer are solved according to the following equations, and the specific equations are as follows:

[0073] h ln =h 1+n

[0074] Among them, h 1+n and h ln They are respectively expressed as the height of the welding cover layer and the height of the laser focus offset of the high temperature resistant melt cover layer;

[0075] Specifically, the pipeline groove model mainly includes: groove bottom width d, groove height H h and blunt edge h0.

[0076] Specifically, the corrosion-resistant additive base layer (4) is mainly prepared by adding a small amount of nano-Ta particles (8) through a laser additive process, such as Figure 3 shown.

[0077] Specifically, the high temperature resistant molten cover layer (7) is mainly prepared by laser cladding TiC nanowires (10), such as Figure 4 shown.

[0078] Specifically, the corrosion-resistant additive base layer (4), the welding filling layer (5), and the corrosion-resistant melt-coated surface layer (7) are all simplified into a trapezoidal shape.

[0079] Specifically, the process parameters used in the preparation of the corrosion-resistant additive base layer of the present invention are: laser power of 8 kW, powder feeding speed of 5 m / min, and scanning speed of 0.5 m / min.

[0080] Specifically, the process parameters used in the preparation of the welding filling layer of the present invention are: laser power of 8-10kW, wire feeding speed of 9-11m / min, welding speed of 0.5-0.8m / min, and maximum depth control range of the welding filling layer of 2.0-3.0mm.

[0081] Specifically, the process parameters used for the high temperature resistant molten covering layer of the present invention are as follows: laser power is 0.4kW, wire feeding speed is 6m / min, cladding speed is 0.5m / min, and the maximum depth control range of the high temperature resistant molten covering layer is 0.5-0.8mm.

Claims

1. A method for preparing narrow gap laser welding joints of large-diameter thick-walled tubes with a layered design, characterized in that: The preparation method comprises the following steps: (1) A laser scanner is used to collect the geometric dimensions of the stainless steel pipe groove to be welded and perform image processing to construct the corresponding stainless steel pipe groove model; (2) determining the laser focus position based on the pipeline groove model, inputting the corrosion-resistant additive layer process parameters, completing the preparation of the corrosion-resistant additive layer, and obtaining the corresponding corrosion-resistant additive layer height; (3) calculating the laser focus offset height of the welding filling layer based on the height of the corrosion-resistant additive base layer, completing the adjustment of the laser focus position, inputting the filling layer welding process parameters, completing the preparation of the welding filling layer, obtaining the corresponding weld filling layer height, calculating the total weld height, and proceeding to the next step when the total weld height is greater than the groove height, otherwise repeating the weld filling layer welding process; (4) Calculating the laser focus offset height of the high-temperature resistant molten cover layer based on the weld cover layer height, completing the adjustment of the laser focus position, inputting the corrosion-resistant cover layer cladding process parameters, and completing the preparation of the corrosion-resistant molten cover layer.

2. The method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design according to claim 1 is characterized in that: The size model of the corrosion-resistant additive base layer / weld filler layer / high-temperature resistant cladding layer is a relationship model between the cross-sectional area, weld width, and excess height of a single additive pass / weld / cladding layer and the wire / powder feeding speed, laser power, and scanning / welding / cladding speed, and its mathematical expression is as follows: S d =a1P+b1v w +c1v f h d =a2P+b2v w +c2v f D d =a3P+b3v w +c3v f Among them, S d 、h d 、D d ,P,v w and v f are the cross-sectional area of ​​single-pass additive / weld / cladding layer, excess height, weld width, laser power, scanning / welding / cladding speed, and wire / powder feeding speed, respectively. a1, a2, a3, b1, b2, b3, c1, c2, and c3 are constants and are related to the material; The input of the base layer additive / filling layer welding / capping layer cladding process parameters is achieved through the interrelated additive process knowledge base, welding process knowledge base and cladding process knowledge base, and the corresponding base layer / filling layer / capping layer size model is established based on the process parameters to obtain the corresponding additive / weld / cladding layer height, including: Extracting the blunt edge and the size of the groove gap of the groove based on the established pipeline groove model, querying the laser additive process knowledge base, and obtaining the corrosion-resistant base coating additive process parameters; Establishing a size model of the corrosion-resistant additive base layer / welding filling layer / high-temperature resistant molten metal covering layer based on the corrosion-resistant base layer additive / filling layer welding / high-temperature resistant molten metal covering layer process parameters to obtain the height of the corrosion-resistant additive base layer / welding filling layer / high-temperature resistant molten metal covering layer; The height of the corrosion-resistant additive layer and the laser focus offset height of the welding filling layer are solved according to the following equations. The specific equations are as follows: h l1 =h1 Among them, D d1 、S d1 , d, h1 and h l1 They are respectively represented as the additive base layer melt width, the additive base layer cross-sectional area, the groove bottom width, the corrosion-resistant additive base layer height and the laser focus offset height of the welding filling layer; The height of the welding filling layer and the laser focus offset height of the next welding filling layer are solved according to the following equations. The specific equations are as follows: h li =h 1+i Among them, D d1+i 、D di 、h 1+i 、S d1+i and h li They are respectively represented as the melt width of the i-th welding filling layer, the melt width of the i-1-th welding filling layer, the weld height of the i-th welding filling layer, the cross-sectional area of ​​the i-th welding filling layer and the laser focus offset height of the next welding filling layer; The total height of the weld is solved according to the following equation, which is as follows: H=∑h i i=1,2,3.....,n Where H represents the total height of the weld. The total height of the weld satisfies H≥H h When the welding process of the filling layer is completed; The height of the welding cover layer and the laser focus offset height of the high-temperature resistant melt-covered cover layer are solved according to the following equations. The specific equations are as follows: h ln =h 1+n Among them, h 1+n and h ln They are respectively represented as the height of the welding cover layer and the laser focus offset height of the high temperature resistant melt cover layer.

3. The method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design according to claim 1 is characterized in that: The pipeline groove model mainly includes: groove bottom width d, groove height H h and blunt edge h0.

4. The method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design according to claim 1 is characterized in that: The corrosion-resistant additive base layer is mainly prepared by adding a small amount of nano-Ta particles through a laser additive process.

5. The method for preparing a layered design of a large-diameter, thick-walled tube narrow-gap laser welding joint according to claim 1, characterized in that: The high temperature resistant molten covering surface layer is mainly prepared by laser cladding TiC nano welding wire.

6. The method for preparing a narrow gap laser welding joint of a large-diameter thick-walled tube with a layered design according to claim 1 is characterized in that: The corrosion-resistant additive base layer, welding filling layer, and corrosion-resistant melt-coated surface layer are all simplified into trapezoidal shapes.

Citation Information

Patent Citations

  • Thick plate large groove multi-layer multi-pass welding track planning method

    CN112276390A

  • Thick plate titanium alloy narrow-gap double-laser-beam powder filling welding method

    CN112453705A

  • Welding-cladding composite weld joint of wear-resistant steel and welding method of welding-cladding composite weld joint

    CN115635253A

  • Multi-layer thick-wall component robot welding layer channel intelligent planning method

    CN117532226A

  • Dual-wavelength laser additive welding method for improving welding seam forming quality of inner runner structure

    CN118371851A

Cited By

  • Laser welding verification method and system

    CN119910300A

  • A laser welding verification method and system

    CN119910300B

  • Hydrogen embrittlement-resistant welding wire for tailor welding of ultrahigh-strength aluminum-silicon coating hot-formed steel and welding method

    CN121339759A