High-performance Al-Si-Mg aluminum alloy welding wire and preparation method thereof

By using high-performance Al-Si-Mg aluminum alloy wire and combined with specific process processing, the problems of insufficient thermal cracking tendency and mechanical properties in aluminum alloy welding are solved, and the high strength and fatigue resistance of the welded joints are improved.

CN118951480APending Publication Date: 2024-11-15WEIQIAO LIGHTWEIGHT RESEARCH CENTER AT SOOCHOW
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411278806.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing aluminum alloy wires have problems of thermal cracking tendency and insufficient mechanical properties during welding, especially when welding 6XXX series and 7XXX series aluminum alloys, it is difficult to meet the welding manufacturing needs of high-end equipment.

Method used

High-performance Al-Si-Mg aluminum alloy wire is used, and its chemical composition includes Si 2.7-9.4%, Mg 1.5-2.1%, Cu 0.05-0.95%, Mn 0.01-1.25%, Zn 0.01-0.5%, Ti 0.001-0.5 %, Sr 0.001 to 0.1%, welding wire with excellent performance is prepared by specific smelting and processing processes such as homogenization annealing, hot extrusion, skinning and multi-pass drawing.

Benefits of technology

The strength and mechanical properties of the welds are improved and the tendency of thermal cracking is reduced. The welded joints after welding can be heat treated and strengthened to obtain better mechanical properties. The average hardness value of the welds is not less than 80HV.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951480A_ABST
    Figure CN118951480A_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance Al-Si-Mg aluminum alloy welding wire and a preparation method thereof.The high-performance Al-Si-Mg aluminum alloy welding wire is prepared from, by mass, 2.7%-9.4% of Si, 1.5%-2.1% of Mg, 0.05%-0.95% of Cu, 0.01%-1.25% of Mn, 0.01%-0.5% of Zn, 0.001%-0.5% of Ti, 0.001%-0.1% of Sr and the balance Fe. 0.15%, and the balance being Al and inevitable impurity elements. According to the high-performance Al-Si-Mg aluminum alloy welding wire, the welding seam strength can be improved, and the overall mechanical property of a welding product is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material welding, and in particular relates to a high-performance Al-Si-Mg aluminum alloy welding wire and a preparation method thereof. Background Art

[0002] With the development of welding technology and the increasing demand for high-strength and tough materials in the industrial field, high-strength aluminum alloys have been widely used in welding products in industries such as automobiles, ships, and aerospace. As the main connection method for aluminum alloy components, fusion welding requires the selection of appropriate welding wire components to ensure that the welded joint has sufficient strength, ductility and other properties to meet the service requirements of aluminum alloy structures, and to minimize welding defects such as pores and thermal cracks.

[0003] At present, the most widely used aluminum alloy welding wires are 5XXX series aluminum alloy welding wires, such as ER5356, ER5183, etc., and 4XXX series aluminum alloy welding wires, such as ER4043, ER4047, etc. The 5XXX series aluminum alloy welding wires have higher strength themselves, but they also have a higher tendency to thermal cracking when welding 6XXX series aluminum alloys and 7XXX series aluminum alloys. The 4XXX series aluminum alloy welding wires have a low melting point, a small solidification range, and good fluidity. They can provide low-melting point eutectics during the welding process, thereby minimizing the tendency to thermal cracking and improving the shear strength of the fillet weld. However, there are no strengthening elements in the composition of the ER4043 and ER4047 welding wires. The mechanical properties of the welded joints strongly depend on the composition of the diluted base material, and the weld becomes the weak point in the mechanical properties of the entire component.

[0004] The chemical composition of the welding wire will have a great influence on the organization and performance of the welded joint. Thanks to the fast cooling rate of welding, the weld as a cast metal organization can dissolve more solute elements and has fine grains. Therefore, the optimization of welding wire alloy mainly adopts multi-component composite microalloying to improve the mechanical properties of the welded joint. Patents CN201510882922.4 and CN201810532500.8 add Cu elements to the welding wire to strengthen the welding wire / weld through its solid solution strengthening effect. Patents CN202110629191.8 and CN202010483321.7 respectively improve the strength and toughness of the welding wire / weld by refining the welding wire / weld grains with microalloying elements such as Mn / Zr and Sr / Ti. However, the strengthening effect of this type of welding wire is limited. Patents CN201910414172.6, CN 201711273943.1, CN201910672080.8, and CN201910576688.0 etc. enhance the performance of welding wire / weld by adding ceramic particles such as Al2O3 or TiB2 to welding wire and utilizing the dispersion strengthening effect of ceramic particles. Although such welding wire has good strengthening effect, ceramic particles are prone to agglomeration, making it difficult to prepare welding wire with uniform distribution.

[0005] Mg has a high solubility in aluminum alloys. Adding a small amount of Mg to aluminum-silicon alloys can greatly improve their yield strength and tensile strength. Patent CN 202310445098.0 and Patent CN 202111402791.7 both add trace amounts of Mg to ER4043 to combine it with Si to form a Mg2Si phase, strengthening the weld through dispersion strengthening. However, these welding wires contribute little to improving the performance of welded joints and cannot meet the welding manufacturing needs of high-end equipment.

[0006] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0007] The object of the present invention is to provide a high-performance Al-Si-Mg aluminum alloy welding wire and a preparation method thereof, wherein the welding wire can increase the weld strength and improve the overall mechanical properties of the welded product.

[0008] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0009] A high-performance Al-Si-Mg aluminum alloy welding wire has the following chemical compositions by mass percentage: Si 2.7-9.4%, Mg 1.5-2.1%, Cu 0.05-0.95%, Mn 0.01-1.25%, Zn 0.01-0.5%, Ti 0.001-0.5%, Sr 0.001-0.1%, Fe<0.15%, and the remainder is Al and unavoidable impurity elements.

[0010] In one or more embodiments of the present invention, the alloy structure of the aluminum alloy welding wire includes an α-Al matrix, a eutectic Si phase, an α-AlFeMnSi phase, a π-AlFeMgSi phase, a Mg2Si phase and a Q-AlCuMgSi phase.

[0011] Another specific embodiment of the present invention provides a technical solution as follows:

[0012] A method for preparing a high-performance Al-Si-Mg aluminum alloy welding wire comprises the following steps:

[0013] Step 1, weighing pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys according to the chemical composition of the welding wire, heating and melting them in a smelting furnace, and casting them after stirring, slagging, degassing and refining to obtain ingots;

[0014] Step 2, subjecting the ingot to homogenization annealing treatment;

[0015] Step 3, preheating the ingot at 500-530° C. for 10-30 min, and extruding at 480-500° C. after preheating to obtain a wire with a diameter of 6-9.5 mm;

[0016] Step 4: Strip the wire;

[0017] Step 5, drawing the wire obtained in step 4 for multiple times, and performing annealing treatment during the drawing process to obtain welding wire;

[0018] Step 6: Perform a final scraping process on the welding wire obtained in step 5 to obtain a high-performance Al-Si-Mg aluminum alloy welding wire.

[0019] In one or more embodiments of the present invention, in step 1, stirring, slagging, degassing and refining are performed at 720-750°C.

[0020] In one or more embodiments of the present invention, in step 2, the temperature of the homogenization annealing treatment is 500-540° C., and the holding time is 1-8 hours.

[0021] In one or more embodiments of the present invention, in step 3, the extrusion ratio of hot extrusion is 45-90.

[0022] In one or more embodiments of the present invention, in step 4, the wire stripping treatment has a diameter reduction of 0.3 to 0.8 mm.

[0023] In one or more embodiments of the present invention, in step 5, the wire is drawn 7 to 19 times, with a diameter reduction of 10 to 20% in each time, and the annealing temperature during the drawing process is 300 to 450° C., the holding time is 0.5 to 3 h, and the cooling rate is ≤30° C. / h.

[0024] In one or more embodiments of the present invention, in step 6, after the final scraping process, the diameter of the high-performance Al-Si-Mg aluminum alloy welding wire obtained is 0.8 to 3.2 mm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The welding wire of the present invention is based on the hypoeutectic Al-Si alloy, which has good fluidity after melting and is not easy to produce crystallization cracks. Compared with Al-Mg welding wire, Al-Si welding wire requires less heat input during welding, and the softening effect of the heat-affected zone caused by welding high-strength heat-treatable alloys is lower.

[0027] 2. A certain proportion of Mg element is added to the welding wire of the present invention, which can ensure that there is enough Mg element dissolved in the Al matrix during welding to improve the strength of the weld; at the same time, it can avoid the performance degradation caused by the reduction of Mg dissolved in the weld due to the burning of Mg element during welding. In addition to the Mg dissolved in the weld, some Mg elements combine with Si to form Mg2Si phase to further improve the hardness of the weld. After adding the Mg element, the work hardening effect of the alloy causes cyclic slip resistance at the crack tip, hindering the expansion of the crack, and a large number of slip systems are activated. The solute Mg can transform the crack movement into a non-localized mode, resulting in a longer crack path before the final failure and a longer fatigue life.

[0028] 3. A certain proportion of Cu element is added to the welding wire of the present invention, which plays a role of solid solution strengthening in the weld and does not precipitate a large amount of Q phase and θ phase at the grain boundary, thereby reducing the corrosion resistance of the weld.

[0029] 4. A certain amount of Mn element is added to the welding wire of the present invention. When the Mg element in the weld reaches the solid solubility limit, the Mn element can further improve the weld performance through solid solution strengthening, and the Mn element has a high boiling point and is not easily burned during welding. Among them, the Al6Mn phase can dissolve the impurity Fe to form the Al6(Mn,Fe) phase, reducing the adverse effect of Fe on the ductility of the welding wire. Moreover, after homogenization treatment, the fine-sized Al6Mn phase is dispersed, which can prevent grain boundary migration, thereby refining the grain size. In addition, a certain Mn content can prevent mold sticking during the welding wire casting process.

[0030] 5. A trace amount of Zn element is added to the welding wire of the present invention, which is solid-dissolved in the aluminum matrix and can improve the solid-solution strengthening effect of the weld joint.

[0031] 6. Adding a trace amount of aluminum-titanium-carbon-boron refiner to the welding wire of the present invention can refine the grains of the welding wire, increase the ductility of the welding wire alloy, and ensure that the welding wire has sufficient elongation during the processing and deformation process.

[0032] 7. The addition of a trace amount of Sr in the welding wire of the present invention can modify the Al-Si alloy, spheroidize the needle-shaped eutectic Si, and improve the mechanical properties of the welding wire alloy.

[0033] In summary, compared with the existing ER4043 welding wire and ER5183 welding wire, the present invention takes hypoeutectic Al-Si alloy as the component basis, and adds Mg element, Cu element, Mn element, Zn element and Sr element, so that the prepared welding wire has excellent performance, and the welded joint after welding with the welding wire can be heat treated and strengthened, and more excellent mechanical properties can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 This is a physical picture of the high performance Al-Si-Mg alloy welding wire in Example 1 of the present invention.

[0036] Figure 2 The macroscopic morphology of the weld using the high performance Al-Si-Mg alloy welding wire in Example 1 of the present invention;

[0037] Figure 3 The macroscopic morphology of the weld using the high performance Al-Si-Mg alloy welding wire in Example 2 of the present invention;

[0038] Figure 4 The macroscopic morphology of the weld using the high performance Al-Si-Mg alloy welding wire in Example 3 of the present invention;

[0039] Figure 5 This is a backscattering structure diagram of the weld center using a high-performance Al-Si-Mg alloy welding wire in Example 1 of the present invention;

[0040] Figure 6 This is a backscattering structure diagram of the weld center using a high-performance Al-Si-Mg alloy welding wire in Example 2 of the present invention;

[0041] Figure 7 This is a backscattering structure diagram of the weld center using a high-performance Al-Si-Mg alloy welding wire in Example 3 of the present invention;

[0042] Figure 8 This is the microhardness distribution diagram of the welded joints of Examples 1-3 of the present invention at half the thickness of the plate;

[0043] Fig. 9 The engineering stress-strain curves of the welded joints of Examples 1-3 of the present invention;

[0044] Fig.10 This is the fracture macroscopic morphology of the tensile specimen of the welded joint of Examples 1-3 of the present invention;

[0045] Fig.11 The as-cast structure diagram of the ingot obtained in step (1) of Example 1 of the present invention;

[0046] Fig.12 The as-cast structure diagram of the ingot obtained in step (1) of Example 2 of the present invention;

[0047] Fig.13 The as-cast structure diagram of the ingot obtained in step (1) of Example 3 of the present invention;

[0048] Fig.14 This is a microhardness distribution diagram of the welded joint at half the thickness of the plate in Comparative Example 1 of the present invention;

[0049] Fig.15 This is the microhardness distribution diagram of the weld joint along half of the plate thickness in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0050] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0051] A specific embodiment of the present invention provides a high-performance Al-Si-Mg aluminum alloy welding wire. The chemical composition of the welding wire is as follows, by mass percentage: Si 2.7-9.4%, Mg 1.5-2.1%, Cu 0.05-0.95%, Mn 0.01-1.25%, Zn 0.01-0.5%, Ti 0.001-0.5%, Sr 0.001-0.1%, Fe<0.15%, and the remainder is Al and unavoidable impurity elements.

[0052] Specifically, the alloy structure of the aluminum alloy welding wire includes an α-Al matrix, a eutectic Si phase, an α-AlFeMnSi phase, a π-AlFeMgSi phase, a Mg2Si phase and a Q-AlCuMgSi phase, and the average hardness value of the weld after welding using the aluminum alloy welding wire of the present invention is not less than 80HV. Specifically, the present invention is based on the hypoeutectic Al-Si alloy, and by adding 1.5 to 2.1wt% of magnesium elements, it is ensured that there is enough Mg element dissolved in the Al matrix during welding, thereby improving the strength of the weld, and at the same time, it can avoid the reduction of the solid solution amount of Mg in the weld due to the burning of the Mg element, which causes the performance to decrease. The addition amount of the Mg element will affect the performance of the weld. If the addition amount is lower than the ratio disclosed in the present invention, the strength of the weld cannot be effectively improved, and if the addition amount is too high, the excessive Mg element will cause the volume fraction of the intermetallic compound Mg2Si phase in the weld to increase, the phase density will increase and connect, and finally cause the weld to brittle fracture.

[0053] In addition, a certain proportion of Cu, Mn, Zn and Sr elements are combined to further improve the weld strength and the overall mechanical properties of the welded product, so that the average hardness value of the weld after welding is not less than 80HV.

[0054] Another embodiment of the present invention provides a method for preparing a high-performance Al-Si-Mg aluminum alloy welding wire, comprising steps 1-6.

[0055] Step 1, weighing pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys according to the chemical composition of the welding wire, heating and melting them in a smelting furnace, and casting them after stirring, slagging, degassing and refining to obtain ingots.

[0056] Specifically, stirring, slagging, degassing and refining are carried out at 720-750° C., and casting is performed to obtain an ingot with a diameter of 90 mm.

[0057] Step 2: subjecting the ingot to homogenization annealing treatment.

[0058] Specifically, the temperature of the homogenization annealing treatment is 500-540° C., and the holding time is 1-8 hours. The homogenization annealing treatment of the ingot can improve the element segregation in the microstructure of the ingot and improve the uniformity of the element distribution of the alloy.

[0059] Step 3, preheating the ingot at 500-530° C. for 10-30 min, and extruding at 480-500° C. after preheating to obtain a wire with a diameter of 6-9.5 mm.

[0060] Specifically, preheating the ingot within a certain temperature range can reduce the temperature difference between the inside and the surface of the ingot, reduce thermal stress, avoid cracks during the extrusion process, and also help improve the plasticity of the alloy. Hot extrusion at a certain temperature can improve the microstructure of the aluminum alloy, improve the mechanical properties of the material, and achieve a larger deformation under lower stress, thereby improving production efficiency.

[0061] Step 4: peel the wire.

[0062] Specifically, the wire is peeled to remove the coarse-grained layer on the wire surface, and the diameter reduction of the wire peeling treatment is 0.3-0.8 mm. The coarse-grained layer is a layer of material with relatively coarse grains on the surface of the wire, which will reduce the toughness of the welded joint and affect the microstructure of the weld. Removing the coarse-grained layer on the wire surface with a certain diameter reduction can effectively ensure the welding performance of the welding wire.

[0063] Step 5, drawing the wire obtained in step 4 for multiple times, and performing annealing treatment during the drawing process to obtain welding wire.

[0064] Specifically, the wire is drawn for 7 to 19 times, with a diameter reduction of 10 to 20% in each time. The temperature of the annealing treatment during the drawing process is 300 to 450°C, the holding time is 0.5 to 3 hours, and the cooling rate is ≤30°C / h. Drawing the welding wire through multiple passes to gradually reduce the diameter of the welding wire, combined with annealing treatment, can improve the plasticity of the welding wire, promote grain refinement, and improve the strength and toughness of the welding wire.

[0065] Step 6, performing a final scraping process on the welding wire obtained in step 5 to obtain a high-performance Al-Si-Mg aluminum alloy welding wire.

[0066] Specifically, after the final scraping treatment, the diameter of the high-performance Al-Si-Mg aluminum alloy welding wire obtained is 0.8 to 3.2 mm. The final scraping treatment of the welding wire can remove the oxide film and impurities on the surface of the welding wire, thereby reducing the generation of pores and slag inclusions during welding and improving the strength and density of the weld.

[0067] The present invention is further described in detail below in conjunction with specific embodiments.

[0068] Example 1

[0069] High performance Al-Si-Mg aluminum alloy welding wire, its chemical composition by mass percentage is: Si 4.1%, Mg2.1%, Cu 0.4%, Mn 0.4%, Zn 0.05%, Ti 0.01%, Sr 0.03%, Fe<0.15%, the balance is Al and unavoidable impurity elements.

[0070] Follow the steps below to prepare high performance Al-Si-Mg aluminum alloy welding wire:

[0071] (1) According to the chemical composition of the welding wire, pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys were weighed and added into a crucible of a smelting furnace in sequence for heating and melting, stirred, slag-stripped, degassed and refined at 720° C., and then cast to obtain an ingot with a diameter of 90 mm.

[0072] (2) The ingot is subjected to homogenization annealing treatment at a temperature of 540° C. and a holding time of 8 h.

[0073] (3) The ingot obtained in step (2) was placed in a resistance heating furnace for preheating at 530° C. for 10 min. The ingot was then extruded at 500° C. with an extrusion ratio of 89.75 to obtain a wire with a diameter of 9.5 mm.

[0074] (4) The wire is peeled and the diameter reduction is 0.6 mm.

[0075] (5) The wire obtained in step (4) is drawn 14 times, with a diameter reduction of 13% in each time. During the drawing process, annealing treatment is performed at a temperature of 420° C., a holding time of 2 h, and a cooling rate of 20° C. / h, and welding wire is obtained after completion.

[0076] (6) The welding wire obtained in step (5) is subjected to a final scraping treatment to obtain a high-performance Al-Si-Mg aluminum alloy welding wire with a diameter of 1.2 mm.

[0077] A 3mm thick Al-Mg-Si-Cu alloy profile in T6 heat treatment state was selected as the welding base material for welding test. The specific composition of the Al-Mg-Si-Cu alloy profile is shown in Table 1:

[0078] Table 1 Chemical composition of Al-Mg-Si-Cu alloy (wt.%)

[0079] Si Mg Cu Cr Mn Ti Fe Zn Al 0.9-1.2 0.8-1.0 0.3-0.65 0.2-0.3 0.55-0.7 0.03 ≤0.15 <0.05 margin

[0080] The surface oxide scales of two Al-Mg-Si-Cu test plates were removed, and CMT+MIX Synchropulse butt welding was performed using the prepared high-performance Al-Si-Mg aluminum alloy welding wire with a diameter of 1.2 mm. The welding process parameters were: wire feeding speed 4.5 m / min, welding current 100 A, welding voltage 16.9 V, and welding speed 8 mm / s.

[0081] Example 2

[0082] High performance Al-Si-Mg aluminum alloy welding wire, its chemical composition by mass percentage is: Si 5.6%, Mg 1.5%, Cu 0.24%, Mn 0.06%, Zn 0.1%, Ti 0.01%, Sr 0.03%, Fe<0.15%, the balance is Al and unavoidable impurity elements.

[0083] Follow the steps below to prepare high performance Al-Si-Mg aluminum alloy welding wire:

[0084] (1) According to the chemical composition of the welding wire, pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys were weighed and added into a crucible of a smelting furnace in sequence for heating and melting, stirred, slag-stripped, degassed and refined at 720° C., and then cast to obtain an ingot with a diameter of 90 mm.

[0085] (2) The ingot is subjected to homogenization annealing treatment at a temperature of 520° C. and a holding time of 6 h.

[0086] (3) The ingot obtained in step (2) was placed in a resistance heating furnace for preheating at 520° C. for 10 min. The ingot was then extruded at 500° C. at an extrusion ratio of 56.25 to obtain a wire with a diameter of 6 mm.

[0087] (4) The wire is peeled and the diameter reduction is 0.4 mm.

[0088] (5) The wire obtained in step (4) is drawn for 7 times, with a diameter reduction of 18% in each time. During the drawing process, an annealing treatment is performed at a temperature of 400° C., a holding time of 1 h, and a cooling rate of 20° C. / h. After the annealing treatment, a welding wire is obtained.

[0089] (6) The welding wire obtained in step (5) is subjected to a final scraping treatment to obtain a high-performance Al-Si-Mg aluminum alloy welding wire with a diameter of 1.2 mm.

[0090] For the welding test of the high performance Al-Si-Mg aluminum alloy welding wire in this embodiment, the welding base material and welding process used are the same as those in Example 1.

[0091] Example 3

[0092] High performance Al-Si-Mg aluminum alloy welding wire, its chemical composition according to mass percentage is: Si 9%, Mg 1.9%, Cu 0.1%, Mn 0.2%, Zn 0.3%, Ti 0.01%, Sr 0.03%, Fe<0.15%, the balance is Al and unavoidable impurity elements.

[0093] Follow the steps below to prepare high performance Al-Si-Mg aluminum alloy welding wire:

[0094] (1) According to the chemical composition of the welding wire, pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys were weighed and added into a crucible of a smelting furnace in sequence for heating and melting, stirred, slag-stripped, degassed and refined at 750° C., and then cast to obtain an ingot with a diameter of 90 mm.

[0095] (2) The ingot is subjected to homogenization annealing treatment at a temperature of 530° C. and a holding time of 8 h.

[0096] (3) The ingot obtained in step (2) was placed in a resistance heating furnace for preheating at 520° C. for 10 min. The ingot was then extruded at 500° C. with an extrusion ratio of 89.75 to obtain a wire with a diameter of 9.5 mm.

[0097] (4) The wire is peeled and the diameter reduction is 0.5 mm.

[0098] (5) The wire obtained in step (4) is drawn 12 times, with a diameter reduction of 15% in each time. During the drawing process, an annealing treatment is performed at a temperature of 400° C., a holding time of 1 h, and a cooling rate of 20° C. / h. After the annealing treatment, a welding wire is obtained.

[0099] (6) The welding wire obtained in step (5) is subjected to a final scraping treatment to obtain a high-performance Al-Si-Mg aluminum alloy welding wire with a diameter of 1.2 mm.

[0100] For the welding test of the high performance Al-Si-Mg aluminum alloy welding wire in this embodiment, the welding base material and welding process used are the same as those in Example 1.

[0101] Comparative Example 1

[0102] The ER4043 welding wire with a diameter of 1.2 mm produced by Lincoln Company of the United States was selected as the comparative example, and its specific chemical composition is shown in Table 2:

[0103] Table 2 Chemical composition of ER4043 welding wire (wt.%)

[0104] Si Mg Fe Mn Cr Cu Ti Zn Al 5.0 <0.1 0.2 <0.1 <0.1 <0.1 <0.1 <0.1 margin

[0105] The Al-Mg-Si-Cu alloy profile with a thickness of 2.3 mm and a T6 heat treatment state was selected as the welding base material for welding test. The specific composition of the Al-Mg-Si-Cu alloy profile is shown in Table 1. The surface oxide scale of the two Al-Mg-Si-Cu test plates was removed and CMT+MIX Synchropulse butt welding was performed using ER4043 welding wire. The welding process parameters were: wire feeding speed 4.0 m / min, welding current 65 A, welding voltage 15.6 V, and welding speed 10 mm / s.

[0106] Comparative Example 2

[0107] The ER5183 welding wire with a diameter of 1.2 mm produced by Lincoln Company of the United States was selected as the comparative example, and its specific chemical composition is shown in Table 3:

[0108] Table 3 Chemical composition of ER5183 welding wire (wt.%)

[0109] Si Mg Fe Mn Cr Cu Ti Zn Al <0.4 5 <0.4 0.5-1.0 <0.1 <0.1 <0.15 0.25 margin

[0110] The Al-Mg-Si-Cu alloy profile with a thickness of 2 mm and a T5 heat treatment state was selected as the welding base material for welding test. The specific composition of the Al-Mg-Si-Cu alloy profile is shown in Table 1. The surface oxide scale of the two Al-Mg-Si-Cu test plates was removed and CMT+MIX Synchropulse butt welding was performed using ER5183 welding wire. The welding process parameters were: wire feeding speed 4.5 m / min, welding current 100 A, welding voltage 16.9 V, and welding speed 10 mm / s.

[0111] The tensile properties of the welded joints in each embodiment and each comparative example were tested, and the results are shown in Table 4:

[0112] Table 4 Tensile properties of welded joints

[0113] sample Yield strength (MPa) Tensile strength(MPa) Elongation after break (%) Fracture location Example 1 159.0 254.9 6.3 Heat affected zone Example 2 161.2 250.1 5.5 Heat affected zone Example 3 164.2 255.8 5.8 Heat affected zone Comparative Example 1 120.0 244.0 6.7 Weld Comparative Example 2 141.4 231.3 6.8 Weld

[0114] Depend on Figure 2-Figure 4 It can be seen that the weld formed by using the high performance Al-Si-Mg alloy welding wire of the present invention is good without obvious welding defects. Figure 5-Figure 7 The microstructure of the center of the weld shows that the weld structure is composed of α-Al matrix + eutectic Si, and there is also a bright white Fe-containing phase at the grain boundary, as well as a small amount of strip-shaped black Mg2Si phase. It can be seen that after the Mg content in the welding wire is burned by welding, the Mg content provided to the weld has reached its solid solubility limit.

[0115] The microhardness of the welded joints in Examples 1-3 was measured along the half of the plate thickness, and the obtained microhardness distribution is as follows: Figure 8 As shown, in the welded joints of Examples 1-3, the average hardness of the welds is 86.3HV, 87.3HV and 90.7HV respectively, all of which are higher than the hardness of the over-aging zone in the heat-affected zone (~70HV). At this time, the heat-affected zone becomes the lowest point in the performance of the welded joint. Fig.14 and Fig.15 In Comparative Example 1 and Comparative Example 2, ER4043 welding wire and ER5183 welding wire were used to weld 2-2.3 mm thick Al-Si-Mg-Cu alloy respectively. The lowest hardness points of the two welded joints were the welds, and the average hardnesses of the welds were 71.2 HV and 60.8 HV respectively, which were lower than the average hardness of the welds in Examples 1-3.

[0116] Fig. 9 : is the room temperature tensile engineering stress-strain curve of the welded joints of Examples 1-3. It can be seen from the figure that since the average hardness of the welds in Examples 1-3 is higher than the hardness of the over-aging zone in the heat-affected zone, the tensile specimens all broke in the heat-affected zone. Fig.10As shown. In Comparative Examples 1 and 2, the average hardness of the weld is the lowest point of the entire weld joint, and the tensile specimens all break at the weld.

[0117] Figure 11-13 This is the cast structure diagram of the ingot in Example 1-3. It can be seen from the figure that the microstructure of the ingot contains α-Al matrix, eutectic Si phase, α-AlFeMnSi phase, π-AlFeMgSi phase, Mg2Si phase and Q-AlCuMgSi phase.

[0118] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0119] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A high performance Al-Si-Mg aluminum alloy welding wire, characterized in that: According to mass percentage, the chemical composition of the welding wire is: Si 2.7-9.4%, Mg 1.5-2.1%, Cu 0.05-0.95%, Mn 0.01-1.25%, Zn 0.01-0.5%, Ti 0.001-0.5%, Sr 0.001-0.1%, Fe<0.15%, and the balance is Al and unavoidable impurity elements.

2. The high performance Al-Si-Mg aluminum alloy welding wire according to claim 1, characterized in that: The alloy structure of the aluminum alloy welding wire includes an α-Al matrix, a eutectic Si phase, an α-AlFeMnSi phase, a π-AlFeMgSi phase, a Mg2Si phase and a Q-AlCuMgSi phase.

3. A method for preparing the high performance Al-Si-Mg aluminum alloy welding wire according to any one of claims 1 to 2, characterized in that: The steps include: Step 1, weighing pure aluminum ingots, pure copper ingots, quick-dissolving silicon, pure zinc ingots, pure magnesium ingots, aluminum-manganese master alloys, aluminum-strontium master alloys and aluminum-titanium-carbon-boron master alloys according to the chemical composition of the welding wire, heating and melting them in a smelting furnace, and casting them after stirring, slagging, degassing and refining to obtain ingots; Step 2, subjecting the ingot to homogenization annealing treatment; Step 3, preheating the ingot at 500-530° C. for 10-30 min, and extruding at 480-500° C. after preheating to obtain a wire with a diameter of 6-9.5 mm; Step 4: Strip the wire; Step 5, drawing the wire obtained in step 4 for multiple times, and performing annealing treatment during the drawing process to obtain welding wire; Step 6: Perform a final scraping process on the welding wire obtained in step 5 to obtain a high-performance Al-Si-Mg aluminum alloy welding wire.

4. The method for preparing the high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 1, stirring, slagging, degassing and refining are carried out at 720-750°C.

5. The method for preparing the high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 2, the temperature of the homogenization annealing treatment is 500-540° C., and the holding time is 1-8 hours.

6. The method for preparing a high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 3, the extrusion ratio of hot extrusion is 45-90.

7. The method for preparing a high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 4, the wire stripping treatment has a diameter reduction of 0.3 to 0.8 mm.

8. The method for preparing a high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 5, the wire is drawn for 7 to 19 times, with a diameter reduction of 10 to 20% in each time. The annealing temperature during the drawing process is 300 to 450° C., the holding time is 0.5 to 3 hours, and the cooling rate is ≤30° C. / h.

9. The method for preparing a high performance Al-Si-Mg aluminum alloy welding wire according to claim 3, characterized in that: In step 6, after the final scraping process, the diameter of the high-performance Al-Si-Mg aluminum alloy welding wire obtained is 0.8 to 3.2 mm.

Citation Information

Cited By

  • Welding material, welding material, application and preparation method

    CN119457563A

  • Welding materials, welding consumables, applications and preparation methods

    CN119457563B

  • Filling material for 6XXX series aluminum alloy and welding process of filling material