Machining method for ring thin-wall part connection body
Through multiple turning and finishing combined with carburizing and quenching treatment, the deformation problem during the processing of ring-type thin-walled parts is solved, the dimension and position tolerance requirements of the parts are ensured, and the high-precision processing of the sliding ring is achieved.
Patent Information
- Application Number
- CN202411313952.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing processing methods are difficult to effectively control the deformation of ring-type thin-walled parts during processing, and cannot guarantee the final dimensional tolerance and positional requirements of the parts, especially the cylindricality of the inner hole of the sliding ring and the jumping requirements of the outer circle to the inner hole are difficult to meet. .
The process route of removing the margin by multiple turning is used, and the joint part of the soft jaw supports is fine-processed, combined with carburizing, quenching and aging treatment, gradually removes cutting stress, ensures the accuracy of the inner hole and outer circle, and is grinding. During the process, magnetic suction cups are used for cutting surface processing.
It effectively reduces deformation during processing, ensures the outer circle and inner hole dimension tolerance of sliding ring parts, cylindricality and the jumping requirements of the outer circle for the inner hole, and improves the quality and service life of the product.
Smart Images

Figure CN118951623A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mechanical processing, in particular to a processing method for a ring-like thin-walled component connection. Background Art
[0002] For thin-walled ring parts such as sliding rings, after being assembled with the flywheel flange, if they are worn during actual use, only the sliding ring needs to be replaced. Therefore, the inner diameter of the sliding ring is relatively large and it needs to have good cylindricity to facilitate assembly with the flywheel flange. The outer circle of the sliding ring needs to be equipped with a sealing ring, which plays a sealing role after assembly. Therefore, the outer circle has good runout requirements on the inner hole, and the outer circle roughness requirements are relatively high, and it needs to have good wear resistance.
[0003] The technical requirements for sliding rings in the existing processing process are: inner hole diameter φD, inner hole cylindricality requirement 0.04, outer circle outer diameter φd, outer circle to inner hole runout requirement 0.02, outer circle roughness requirement Ra0.4, outer circle carburizing hardening hardness Carburized layer depth 500HV10=δmm, width L, wall thickness 3mm~4mm, see attached for details Figure 1 To meet the technical requirements of sliding rings, the parts need to be carburized and quenched, and the inner hole and outer circle need to be ground. Because sliding rings are large thin-walled parts (inner hole diameter ≥φ145, wall thickness 3mm~4mm), and heat treatment is required, the size tolerance and position tolerance of the inner hole and outer circle are high, and deformation is easy to occur during the processing, so how to control and eliminate deformation is particularly important.
[0004] In the existing processing method, direct clamping with a fixture is used, which causes large deformation of the parts and cannot guarantee the final size and position tolerance requirements of the sliding ring; by using inner hole positioning and pressure plate pressing the end face, only the outer circle of the part can be ground, but the inner hole cannot be ground, and the requirements of the inner hole cylindricity, tolerance, etc. cannot be guaranteed, and the runout requirements of the outer circle to the inner hole cannot be guaranteed; the inner hole processing with a head support has a low material utilization rate. The above processing methods all have defects and cannot meet the use requirements of the sliding ring. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the existing defects and provide a processing method for connecting ring-like thin-walled parts, which can effectively control the deformation of the ring-like thin-walled parts during the processing, ensure the final dimensional tolerance and position requirements of the parts, and effectively solve the problems in the background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for processing a ring-like thin-walled component body, comprising the following steps:
[0007] S1: collar forging blank;
[0008] S2: Rough turning: Three jaws clamp the outer circle, flatten the end surface, and remove the end surface and inner hole allowance;
[0009] S3: Rough turning 2: Soft jaws support the inner hole and end surface processed in step S2 to be flat, and remove the outer circle, the end surface of the other end of the joint, the inner hole and the inner hole margin of the middle joint part;
[0010] S4: Carburizing treatment: Carburizing the semi-finished product as a whole to prepare for subsequent heat treatment;
[0011] S5: First semi-finishing turning: The soft jaws support the inner hole and end surface of one end of the joint body to be flat, and the end surface of the other end of the joint body and the carburized layer of the inner hole are turned off;
[0012] S6: First semi-finishing turning 2: Taking the inner hole and end face processed in step S5 as the reference, the soft clamping jaws support the inner hole, flatten the end face, and turn off the carburized layer of the other end face of the joint body, the inner hole and the middle joint body;
[0013] S7: Stress relief tempering: remove the cutting stress generated during rough turning, the first semi-finishing turning, and the stress generated during heat treatment;
[0014] S8: Second semi-finishing turning: The soft jaws support the inner hole and end face of one end of the joint body to be flat, and remove the end face, outer circle, outer groove, chamfer and inner hole margin of the other end of the joint body, to ensure that the inner hole of the middle joint body is the precision reference and has a good position with the outer circle, which is convenient for subsequent finishing;
[0015] S9: Second semi-finishing turning 2: The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S8, and remove the end face, outer circle, outer groove and chamfering allowance of the other end of the joint again;
[0016] S10: Quenching treatment: The semi-finished product is quenched as a whole, and after fine processing, the carburized layer depth δmm required by the drawing is achieved;
[0017] S11: Finish turning 1: The soft jaws support the inner hole of the middle joint part, level the inner hole end face of one end of the joint, and the parts at the other end of the joint are basically finished by turning, leaving only the outer circle and inner hole grinding allowance, and digging a groove in the inner hole;
[0018] S12: Finish turning 2: The soft jaws support the inner hole of the middle joint part, leveling the inner hole end face processed in step S11, and the other end part of the joint is basically finished by turning, leaving only the outer circle and inner hole grinding allowance, and the inner hole is grooved;
[0019] S13: Aging treatment: remove the stress generated during quenching, second semi-finishing turning and finishing turning;
[0020] S14: Grinding 1: The soft clamping claws support the inner hole of the middle joint part, level the inner hole end face of one end of the joint, clamp the other end of the joint and grind the outer circle and inner hole at one time to ensure the final technical requirements of the inner hole and outer circle;
[0021] S15: Grinding 2: The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S14, and grind the outer circle and inner hole of the other end of the joint at one time to ensure the final technical requirements of the inner hole and outer circle;
[0022] S16: Inspection;
[0023] S17: Cutting: The soft jaws support the inner hole of the middle joint part, level the end surface of the inner hole, cut the joint part, and process it into two sliding ring parts;
[0024] S18: Surface grinding: The end face of the part is adsorbed by a magnetic suction cup on the surface grinder, and the cutter cut surface is ground to ensure the width size of the two end faces of the final part and its technical requirements;
[0025] S19: Overall deburring and cleaning;
[0026] S20: Final inspection;
[0027] S21: Anti-rust treatment, packaging, and storage.
[0028] As a preferred technical solution of the present invention, the depth of the carburized layer in step S4 is 500HV10=δ1mm.
[0029] As a preferred technical solution of the present invention, the carburized hardening hardness of the outer circle after quenching in step S10 is ensured to be The depth of carburized layer is 500HV10=δ2mm.
[0030] As a preferred technical solution of the present invention, the single-side margin of the groove in step S11 is 1 to 1.5 mm.
[0031] As a preferred technical solution of the present invention, the single-side margin of the groove in step S12 is 1 to 1.5 mm.
[0032] As a preferred technical solution of the present invention, in step S17, a 0.1 mm margin is reserved on the end surface of the part where it is cut.
[0033] 1. Compared with the prior art, the present invention has the following beneficial effects: (1) The processing method of the ring-type thin-walled parts is to remove the excess by turning multiple times through reasonable arrangement of the process route, and to process the other end of the connected part with one end of the connected part processed as the reference. Before fine grinding, a fine turning process and aging treatment are arranged to reduce the grinding allowance as much as possible and minimize the stress generated during the cutting process, thereby reducing deformation; (2) The inner hole of the middle connected part is processed by fine turning, and the inner hole of the middle connected part is used as the fine reference to support the inner hole and level the end face of the inner hole to avoid deformation of the clamped parts. The outer circle and inner hole of the part are ground by clamping the middle connected part once, thereby ensuring the outer circle and inner hole size tolerance, inner hole cylindricity, outer circle to inner hole runout and other technical requirements of the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic diagram of the parts of a ring-type thin-walled sliding ring;
[0035] Figure 2 It is a process structure diagram of steps S2 and S3 of the present invention;
[0036] Figure 3 It is a process structure diagram of steps S5 and S6 of the present invention;
[0037] Figure 4 It is a process structure diagram of steps S8 and S9 of the present invention;
[0038] Figure 5 It is a process structure diagram of steps S11 and S12 of the present invention;
[0039] Figure 6 It is a process structure diagram of steps S14 and S15 of the present invention;
[0040] Figure 7 is a process structure diagram of step S17 of the present invention;
[0041] Figure 8 This is a process structure diagram of step S18 of the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] The present invention provides a technical solution: a method for processing a ring-like thin-walled part connection, comprising the following steps:
[0044] S1: collar forging blank;
[0045] S2: Rough turning (rough turning end face, inner hole, chamfering): Three-claw clamp the outer circle, flatten the end face, remove the end face and inner hole allowance, reserve 1.6mm in the outer circle diameter direction, and reserve 17.9mm in the inner hole diameter direction. Refer to the attached Figure 2 Left;
[0046] S3: Rough turning 2 (turning end face, outer circle, inner hole, chamfering): soft jaws support the inner hole and end face processed in step S2 to be flat, remove the outer circle, the other end face of the joint, the inner hole and the inner hole allowance of the middle joint part, reserve 1.6mm in the outer circle diameter direction, 17.9mm in the inner hole diameter direction, and 10mm in the inner hole diameter direction of the middle joint part, refer to the attached Figure 2 right;
[0047] S4: Carburizing treatment: Carburizing the semi-finished product as a whole to ensure that the carburizing layer depth is 500HV10=δ1mm, in preparation for subsequent heat treatment;
[0048] S5: First semi-finishing turning (first semi-finishing turning end face, inner hole, chamfer): soft jaws support the inner hole and end face of one end of the joint body to be flat, turn off the end face of the other end of the joint body and the carburized layer of the inner hole, and reserve a margin of 7.9mm in the inner hole diameter direction. Refer to the attached Figure 3 Left;
[0049] S6: First semi-finishing turning 2 (turn around and turn the end face, inner hole, chamfer for the first semi-finishing turning): Take the inner hole and end face processed in step S5 as the reference, support the inner hole with soft jaws, flatten the end face, turn off the carburized layer of the other end face, inner hole and middle part of the joint, reserve 7.9mm for the inner hole diameter direction, and 2mm for the inner hole diameter direction of the middle part, refer to the attached Figure 3 right;
[0050] S7: Stress relief tempering: remove the cutting stress generated during rough turning, the first semi-finishing turning, and the stress generated during heat treatment;
[0051] S8: Second semi-finishing turning 1 (second semi-finishing turning end face, outer circle, inner hole, outer groove, chamfer): soft clamping claws support the inner hole and end face of one end of the joint body to be flat, remove the end face, outer circle, outer groove, chamfer of the other end of the joint body and the inner hole margin in the middle of the joint body, ensure that the inner hole in the middle of the joint body is the precision reference and has a good position with the outer circle, which is convenient for subsequent finishing. Reserve 1mm margin in the outer circle diameter direction, refer to the attached Figure 4 Left;
[0052] S9: Second semi-finishing turning (turn around for the second semi-finishing turning of the end face, outer circle, outer groove, and chamfer): The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S8, and remove the end face, outer circle, outer groove and chamfer allowance of the other end of the joint again. The allowance in the outer circle and inner hole diameter direction is 1mm. Refer to the attached Figure 4 right;
[0053] S10: Quenching treatment: The semi-finished product is quenched as a whole to ensure that the carburized hardening hardness of the outer circle is The carburizing layer depth is 500HV10=δ2mm, and after fine machining, it reaches the carburizing layer depth δmm required by the drawing design;
[0054] S11: Finish turning (finish turning inner hole, inner groove, outer circle, chamfer at one end): soft jaws support the inner hole of the middle joint part, flatten the inner hole end face of one end of the joint, and basically finish turn the parts at the other end of the joint, leaving only the outer circle and inner hole grinding allowance, the outer circle and inner hole diameter direction reserved allowance are 0.6mm, the inner hole is grooved, and the single side allowance of the groove is guaranteed to be 1~1.5mm, so that the inner chamfer is formed and the cutting stress is released as much as possible at the groove, refer to the attached Figure 5 Left;
[0055] S12: Finish turning 2 (turning around to finish turning the inner hole, inner groove, outer circle, and chamfer at one end): The soft jaws support the inner hole of the middle joint part, and level the inner hole end face processed in step S11. The parts at the other end of the joint are basically finished and formed, leaving only the outer circle and inner hole grinding allowances. The reserved allowances in the outer circle and inner hole diameter direction are both 0.6mm. The inner hole is grooved to ensure that the single-side allowance of the groove is 1-1.5mm, so that the inner chamfer is formed and the cutting stress is released as much as possible at the groove. Refer to the attached Figure 5 right;
[0056] S13: Aging treatment: remove the stress generated during quenching, second semi-finishing turning and finishing turning;
[0057] S14: Grinding (grinding outer circle and inner hole): The soft clamping claws support the inner hole of the middle joint part, flatten the inner hole end face of one end of the joint, clamp the other end of the joint at one time and grind the outer circle and inner hole to ensure the final technical requirements of the inner hole and outer circle. Figure 6 Left;
[0058] S15: Grinding 2 (turning around to grind the outer circle and inner hole): The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S14, and grind the outer circle and inner hole of the other end of the joint at one time to ensure the final technical requirements of the inner hole and outer circle. Figure 6 right;
[0059] S16: Inspection;
[0060] S17: Cutting: The soft claws support the inner hole of the middle joint part, flatten the end face of the inner hole, cut the joint part, and process it into two sliding ring parts. Leave a 0.1mm margin on the end face of the cut part. Refer to the attached Figure 7 ;
[0061] S18: Grinding surface: On the surface grinder, the end face of the part is adsorbed by the magnetic suction cup, and the cutter cutting surface is ground to ensure the width size of the end face of the final part and its technical requirements. Figure 8 ;
[0062] S19: Overall deburring and cleaning;
[0063] S20: Final inspection;
[0064] S21: Anti-rust treatment, packaging, and storage.
[0065] In steps S2, S3, S5, S6, S8 and S9, the inner hole and end face of one end of the joint body are processed, and clamping is performed based on this, and the inner hole, end face and outer circle of the other end of the joint body are processed, so that the two ends of the joint body have good consistency and position accuracy. The processing allowance is gradually removed during the turning process, which greatly reduces deformation.
[0066] Steps S4 and S10 perform carburizing and quenching treatments to achieve the design requirements for the hardness of the outer surface of the sliding ring and the depth of the carburized layer.
[0067] Steps S7 and S13 reduce the stress generated during cutting and heat treatment to a minimum through stress relief tempering and aging treatment, effectively controlling deformation and preparing for fine machining on a grinding machine.
[0068] Steps S14, S15, S17, and S18 use the inner hole of the middle connecting part as the precision reference, support the inner hole of the middle connecting part, and level the end face of the inner hole at one end, clamp and finish turn and grind the parts at one time, avoid direct clamping of parts, and cut grooves on the outer circle and inner hole during finish turning, ensuring that the single-side allowance of the groove is 1 to 1.5 mm so that the cutting stress can be released as much as possible at the groove, effectively controlling deformation and well ensuring the design requirements of the sliding ring.
[0069] Among them, step S17 supports the inner hole of the middle joint part, flattens the end face of the inner hole, cuts the joint part, forms two sliding ring parts, reserves 0.1mm margin at the part incision, and performs step S18 to grind the incision plane so that the width of the two end faces of the part meets the design requirements.
[0070] The present invention solves the problem of deformation of thin-walled ring parts by gradually removing machining allowances through joint machining, eliminating stress through heat treatment, and performing fine machining on the inner hole of the intermediate joint part by clamping. The outer circle size tolerance, the runout of the outer circle to the inner hole, the outer circle roughness, the inner hole size accuracy and the cylindricity are guaranteed while controlling the deformation of the parts, thereby ensuring the final product quality of the parts.
[0071] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for processing a ring-like thin-walled part, characterized in that: The following steps are involved: S1: collar forging blank; S2: Rough turning: Three jaws clamp the outer circle, flatten the end surface, and remove the end surface and inner hole allowance; S3: Rough turning 2: Soft jaws support the inner hole and end surface processed in step S2 to be flat, and remove the outer circle, the end surface of the other end of the joint, the inner hole and the inner hole margin of the middle joint part; S4: Carburizing treatment: Carburizing the semi-finished product as a whole to prepare for subsequent heat treatment; S5: First semi-finishing turning: The soft jaws support the inner hole and end surface of one end of the joint body to be flat, and the end surface of the other end of the joint body and the carburized layer of the inner hole are turned off; S6: First semi-finishing turning 2: Taking the inner hole and end face processed in step S5 as the reference, the soft clamping jaws support the inner hole, flatten the end face, and turn off the carburized layer of the other end face of the joint body, the inner hole and the middle joint body; S7: Stress relief tempering: remove the cutting stress generated during rough turning, the first semi-finishing turning, and the stress generated during heat treatment; S8: Second semi-finishing turning: The soft jaws support the inner hole and end face of one end of the joint body to be flat, and remove the end face, outer circle, outer groove, chamfer and inner hole margin of the other end of the joint body, to ensure that the inner hole of the middle joint body is the precision reference and has a good position with the outer circle, which is convenient for subsequent finishing; S9: Second semi-finishing turning 2: The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S8, and remove the end face, outer circle, outer groove and chamfering allowance of the other end of the joint again; S10: Quenching treatment: The semi-finished product is quenched as a whole, and after fine processing, the carburized layer depth δmm required by the drawing is achieved; S11: Finish turning 1: The soft jaws support the inner hole of the middle joint part, level the inner hole end face of one end of the joint, and the parts at the other end of the joint are basically finished by turning, leaving only the outer circle and inner hole grinding allowance, and digging a groove in the inner hole; S12: Finish turning 2: The soft jaws support the inner hole of the middle joint part, leveling the inner hole end face processed in step S11, and the other end part of the joint is basically finished by turning, leaving only the outer circle and inner hole grinding allowance, and the inner hole is grooved; S13: Aging treatment: remove the stress generated during quenching, second semi-finishing turning and finishing turning; S14: Grinding 1: The soft clamping claws support the inner hole of the middle joint part, level the inner hole end face of one end of the joint, clamp the other end of the joint and grind the outer circle and inner hole at one time to ensure the final technical requirements of the inner hole and outer circle; S15: Grinding 2: The soft jaws support the inner hole of the middle joint part, level the inner hole end face processed in step S14, and grind the outer circle and inner hole of the other end of the joint at one time to ensure the final technical requirements of the inner hole and outer circle; S16: Inspection; S17: Cutting: The soft jaws support the inner hole of the middle joint part, level the end surface of the inner hole, cut the joint part, and process it into two sliding ring parts; S18: Surface grinding: The end face of the part is adsorbed by a magnetic suction cup on the surface grinder, and the cutter cut surface is ground to ensure the width size of the two end faces of the final part and its technical requirements; S19: Overall deburring and cleaning; S20: Final inspection; S21: Anti-rust treatment, packaging, and storage.
2. A method for processing a ring-like thin-walled component as claimed in claim 1, characterized in that: The depth of the carburized layer in step S4 is 500HV10=δ1mm.
3. The method for processing a ring-like thin-walled component as claimed in claim 1, characterized in that: In step S10, after quenching, the carburization hardening hardness of the outer circle is ensured to be The depth of carburized layer is 500HV10=δ2mm.
4. The method for processing a ring-like thin-walled component as claimed in claim 1, characterized in that: In the step S11, the single-side margin of the groove is 1 to 1.5 mm.
5. The method for processing a ring-like thin-walled component as claimed in claim 1, characterized in that: In step S12, the single-side margin of the groove is 1 to 1.5 mm.
6. The method for processing a ring-like thin-walled component as claimed in claim 1, characterized in that: In step S17, a 0.1 mm margin is reserved at the end surface of the part where it is cut.
Citation Information
Patent Citations
Method for machining ultrathin wall sleeve parts
CN103659158A
Processing method for preventing sawing deformation of conjoined cylindrical parts
CN109794737A
Thin-wall sleeve part processing method
CN110757105A
Machining method of hard-seal double-eccentric ball valve ball
CN111318858A
Machining process of damping bowl
CN112372255A
Cited By
Ring piece wall thickness accurate control and equal thickness turning method and tool
CN121199151A