Machining process for long hollow shaft in complex shape

A multi-step processing technology for hollow motor shafts addresses inefficiencies in existing methods by employing warm forging and precision machining to produce complex-shaped shafts with high precision and quality, reducing material consumption and processing time.

CN119057400APending Publication Date: 2024-12-03TIANJIN PACIFIC DRIVELINE TECH LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411392253.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing methods for processing hollow motor shafts are inefficient, material-intensive, costly, and unsuitable for complex structures, particularly for long shafts with large diameter changes and shrinkage at both ends.

Method used

A multi-step processing technology involving warm forging, residual heat treatment, laser welding, and precision machining, including steps like finish turning, high-frequency quenching, magnetic particle inspection, and ultrasonic flaw detection, to produce hollow shafts with complex shapes, ensuring high precision and quality.

Benefits of technology

The method enables the production of hollow shafts with complex shapes, saving materials, reducing processing time, and achieving high dimensional accuracy, with precise welding and detection methods ensuring quality and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057400A_ABST
    Figure CN119057400A_ABST
Patent Text Reader

Abstract

The invention discloses a machining technology for a long hollow shaft in a complex shape. The machining technology comprises the following steps that firstly, materials are prepared; secondly, warm forging forming is conducted; 3, waste heat treatment; fourthly, finish turning is conducted on the right end piece; fifthly, finish turning is conducted on the left end piece; sixthly, a spline is flexibly pulled; 7, high-frequency quenching and tempering are conducted; step 8, magnetic powder inspection; step 9, cleaning; tenthly, a spline is subjected to hard pulling; eleventhly, ultrasonic cleaning is conducted on the sub-parts; 12, press fitting is conducted; 13, laser welding is conducted; step 14, ultrasonic flaw detection; (15) finish turning of the assembly; sixthly, milling is conducted; seventeenthly, laser marking is conducted; eighteenthly, grinding is conducted; nineteenthly, dynamic balancing is conducted; step 20, sorting and inspecting; 21, ultrasonic cleaning of a finished product; and step 22, packaging. And (23) warehousing. The machining method has the beneficial effects that the machined workpiece is high in size precision, and the machining method can be used for producing thin-walled motor shafts with two necked ends, large diameter difference and other complex appearances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of motor shaft processing in the field of new energy vehicles, and in particular to a processing technology for a long hollow shaft with a complex shape. Background Art

[0002] With the development of new energy vehicles, the hollowing of motor shafts is beneficial to saving raw materials and increasing the heat dissipation area. The hollowing of motor shafts has become an inevitable trend. The processing methods of motor shafts with different structures are different. The current production methods of hollow motor shafts mainly include three methods: hollowing out solid shafts, welding, and one-piece molding.

[0003] Solid shaft hollowing processing is suitable for short shafts with simple structures, but it consumes a lot of materials, has high costs, and has a long processing cycle. Friction welding processing is relatively complex, and it is difficult to control the runout. One-piece molding requires that the mandrel size is similar to the inner cavity size of the finished product. It is not suitable for processing workpieces with complex inner cavity structures, large diameter changes, and shrinkage at both ends.

[0004] In view of the above situation, it is necessary to improve the existing hollow shaft processing method so that it can adapt to the current needs of using hollow shafts. Summary of the invention

[0005] To achieve the above-mentioned purpose, the technical solution of the present invention is a processing technology of a long hollow shaft with a complex shape, comprising the following steps:

[0006] Step 1: Prepare the ingredients;

[0007] Step 2: Warm forging;

[0008] Step 3: Residual heat treatment;

[0009] Step 4: Finish turning the right end piece;

[0010] Step 5: Finish turning of the left end piece;

[0011] Step 6: Soft pull spline;

[0012] Step 7: high frequency quenching and tempering;

[0013] Step 8: Magnetic particle inspection;

[0014] Step 9: Cleaning;

[0015] Step 10: Hard pull the spline;

[0016] Step 11: Ultrasonic cleaning of sub-parts;

[0017] Step 12: Pressing;

[0018] Step 13: Laser welding;

[0019] Step 14: Ultrasonic flaw detection;

[0020] Step 15: Component finishing;

[0021] Step 16: Milling;

[0022] Step 17: Laser marking;

[0023] Step 18: Grinding;

[0024] Step 19: Dynamic balancing;

[0025] Step 20: Sorting inspection;

[0026] Step 21: ultrasonic cleaning of finished product;

[0027] Step 22: Packaging;

[0028] Step 23: Storage.

[0029] To further supplement the technical solution, the step 1 material preparation includes three processes: blanking, chamfering and shot blasting; the step 2 warm forging adopts multi-station forging, and the workpiece is forged into a hollow shaft through forward extrusion, upsetting, reverse extrusion and punching, retaining the shape of the product structure as much as possible; the step 3 residual heat treatment is operated online with the warm forging equipment, and the normalizing effect is achieved by controlling the furnace entry temperature, isothermal furnace temperature and holding time of the forging. After the residual heat treatment, the oxide scale of the forging is thin, and the shot blasting process can also be cancelled.

[0030] To further supplement the technical solution, in step 4, the finishing turning of the right end piece is to complete the two processes of turning the inner hole and the outer circle, and the dimensional tolerance band of the welding surface is controlled within 0.016mm; in step 5, the finishing turning of the left end piece is to complete the two processes of turning the inner hole and the outer circle, and the dimensional tolerance band of the welding surface is controlled within 0.016mm.

[0031] To further supplement the technical solution, in steps six to nine, soft spline drawing, high-frequency quenching and tempering, and magnetic particle inspection are produced in a connected line; in step seven, high-frequency quenching and tempering, the hardness of the quenching area is required to be 58-63HRC, and the quenching and tempering interval time is ≤30min; in step eight, magnetic particle inspection is performed on 100% of the quenching area; in step nine, there is no cleanliness requirement for cleaning, and it is mainly for cleaning magnetic powder.

[0032] As a further supplement to the technical solution, the step 10 of hard drawing the splines is to improve the spline tooth profile accuracy.

[0033] To further supplement the technical solution, the ultrasonic cleaning of the sub-parts in step eleven must ensure the cleanliness requirements, metal particle grade F, non-metal particle grade G, total mass ≤ 4 mg, and single fibers and fluff are allowed.

[0034] To further supplement the technical solution, the press-fitting in step twelve is achieved by a press-fitting machine, which controls the press-fitting into place by displacement, and there is an interference fit between the left end piece and the right end piece. The laser welding in step thirteen must first be performed by half-power welding to ensure that the weld offset is qualified, and then by full-power welding to ensure that the weld depth is qualified; the ultrasonic flaw detection in step fourteen is used to check the weld position to ensure the quality of the workpiece.

[0035] To further supplement the technical solution, the step fifteen component finishing turning is divided into two sequences, firstly, processing multiple diameter sections on the outer circle, and then double-head turning to process various grooves; the step sixteen milling is to process various asymmetric keyways and oil holes on the outer circle; the step seventeen laser marking is used for internal traceability; the step eighteen grinding various key dimensions to ensure the dimensional accuracy of the workpiece, requiring the tolerance range to be ≤0.013mm.

[0036] To further supplement the technical solution, the dynamic balancing requirement of step nineteen is ≤300mg; the selection inspection of step twentieth is to conduct 100% inspection on all key dimensions through the final inspection machine; the finished product ultrasonic cleaning of step twenty-one is to clean and oil all qualified parts, and the cleanliness requirement is the same as that of sub-parts, and the anti-rust oil in the cavity must be blown clean.

[0037] To further supplement the technical solution, in step 22, the workpiece shape must be scanned and confirmed before packaging, and a box code is generated after the box is full, and the information is archived; and in step 23, the qualified parts are put into storage.

[0038] The beneficial effects are as follows: 1. The present invention designs a multi-station warm forging process, and forges the workpiece to retain the product structure through forward extrusion, upsetting, reverse extrusion and punching, which can be used to produce forgings with complex inner cavity structures, and the forging excess is uniform, which saves raw materials and is also conducive to improving the subsequent machining cycle;

[0039] 2. The present invention can be used to process thin-walled parts by precision turning the left and right forgings, and ensure that the dimensional tolerance of the welding surface is ≤0.016mm. Through soft drawing, high-frequency quenching and tempering, magnetic particle flaw detection and hard drawing splines, it can be used to process shafts with high-precision splines. Magnetic particle flaw detection can be used to detect spline defects;

[0040] 3. The present invention combines the left and right end pieces by laser welding, and the weld has a small heat-affected zone, high precision and beautiful appearance. After the hollow shaft is welded, the weld quality needs to be ultrasonically tested to ensure that the product welding quality is qualified;

[0041] 4. The present invention uses fine turning of the welded components to process the shafts with shrinkage at both ends, large diameter differences, and various grooves. Milling can be used to process various asymmetric keyways and oil holes, and grinding can be used to improve the dimensional accuracy of key parts to ensure that the tolerance range is ≤0.013mm;

[0042] 5. The present invention detects the dynamic balance of the workpiece after the keyway is machined by dynamic balancing, and ensures the cleanliness of the workpiece by ultrasonic cleaning;

[0043] 6. The present invention can be used to trace the processing information of a single workpiece by laser marking on the workpiece;

[0044] The present invention combines forging, machining, heat treatment, welding and multiple detection methods. The processed workpiece has high dimensional accuracy and can be used to produce motor shafts with complex appearances such as thin walls, necked ends, large diameter differences, hollow inner cavities, multiple grooves, oil holes, splines, and external keyways. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a processing flow chart of the present invention;

[0046] Figure 2 is a top view of a finished product of the present invention;

[0047] Figure 3 It is a sectional view of a finished product of the present invention. DETAILED DESCRIPTION

[0048] In order to make the technical solution more clear to those skilled in the art, Figure 1-3 The technical solution of the present invention is described in detail:

[0049] First of all, the original intention of the design of the present invention is explained. The hollowing of motor shafts has become an inevitable trend. The processing methods of motor shafts with different structures are different. The current production methods of hollow motor shafts mainly include three methods: solid shaft hollowing, welding, and one-piece molding. The solid shaft hollowing process is suitable for short shafts with simple structures, but it consumes a lot of materials, has high costs, and has a long processing cycle. The friction welding process is relatively complicated and it is difficult to control the runout. One-piece molding requires that the core shaft size is similar to the inner cavity size of the finished product, which is not suitable for processing workpieces with complex inner cavity structures, large diameter changes, and shrinkage at both ends. Therefore, the present invention designs a processing technology for long hollow shafts with complex shapes.

[0050] This embodiment takes the motor shaft in a certain automobile transmission as an example to illustrate the processing technology of the long hollow shaft with complex shape in the present invention. The raw material is C45E, which includes 8 outer diameters, 8 inner diameters, 2 annular grooves, 7 oil holes, and 2 asymmetric external key grooves.

[0051] The present invention will be described in detail below in conjunction with the accompanying drawings. Figure 1-Figure 3 As shown, a processing technology for a long hollow shaft with a complex shape includes the following steps:

[0052] Step 1: Material preparation, including three processes: cutting, chamfering and shot blasting.

[0053] Step 2: Warm forging; process the left and right end pieces, use multi-station forging, and forge the workpieces to retain the product structure through forward extrusion, upsetting, reverse extrusion and punching. It can be used to produce forgings with complex inner cavity structures, and the forging excess is uniform, which saves raw materials and is also conducive to improving the subsequent machining cycle.

[0054] Step 3: Residual heat treatment; it is operated in conjunction with the warm forging equipment. By controlling the temperature of the forging entering the furnace, the temperature of the isothermal furnace and the holding time, the normalizing effect is achieved. After the residual heat treatment, the oxide scale of the forging is thin, and the shot blasting process can also be eliminated.

[0055] Step 4: Finish turning the right end piece; perform two-pass finish turning on the right end piece, turning the inner hole and outer circle, and control the size tolerance band of the welding surface within 0.016mm. The size of the welding surface is a negative tolerance, with an inner diameter of 5 (-0.016~0)mm.

[0056] Step 5: Finish turning the left end piece; perform two-pass finish turning on the left end piece, turning the inner hole and outer circle, and control the dimensional tolerance band of the welding surface within 0.016mm. The size of the welding surface is a positive tolerance, with an inner diameter of 4 (0~+0.016)mm.

[0057] Step 6: Soft pull spline,

[0058] Step 7: High frequency quenching and tempering, the hardness of the quenching area is required to be 58-63HRC, and the quenching and tempering interval time is ≤30min.

[0059] Step 8: Magnetic particle inspection should be performed on 100% of the quenching area.

[0060] Step 9: Clean the magnetic powder, no cleanliness requirement;

[0061] In steps six to nine, soft spline drawing, high-frequency quenching and tempering, and magnetic particle inspection are produced in a connected line to reduce the flow of workpieces between processes and save time. In step seven, high-frequency quenching and tempering, the hardness of the quenching area is required to be 58-63HRC, and the interval time between quenching and tempering is ≤30min to avoid cracks caused by untimely stress relief. In step eight, magnetic particle inspection must conduct 100% inspection of the quenching area. In step nine, there is no cleanliness requirement, and the main purpose is to clean the magnetic powder.

[0062] Step 10: Hard drawing the spline improves the spline tooth profile accuracy and ensures the reliability and durability of the workpiece.

[0063] Step 11: To ensure the cleanliness requirements, metal particles are graded F, non-metal particles are graded G, the total mass is ≤4mg, and individual fibers and fluff are allowed.

[0064] Step 12: The press machine controls the press-fitting into place through displacement, and there is an interference fit between the left end piece and the right end piece.

[0065] Step 13: Laser welding should first be performed by half-power welding to ensure that the weld offset is qualified, and then by full-power welding to ensure that the weld depth is qualified.

[0066] Step 14: Ultrasonic testing is used to inspect the weld position to ensure the quality of the workpiece.

[0067] Step 15: The component finishing is divided into two steps. First, the 8 outer diameters on the outer circle are processed, and then double-end turning is used to process the inner diameter and 2 grooves.

[0068] Step 16: Milling to produce 2 asymmetric keyways and 7 oil holes on the outer circle;

[0069] Step 17: Laser marking for internal traceability;

[0070] Step 18: Grind various key dimensions to ensure the dimensional accuracy of the workpiece. The required tolerance range is 2 (+0.01~+0.0023) mm for outer diameter, 4 (0~+0.013) mm for outer diameter, 5 (+0.022~+0.035) mm for outer diameter, and 6 (+0.012~+0.025) mm for outer diameter.

[0071] Step 19: Dynamic balance requirement is ≤300mg.

[0072] Step 20: Sorting inspection is to use the final inspection machine to check all key dimensions.

[0073] Step 21: Finished product ultrasonic cleaning is to clean and oil all qualified parts. The cleanliness requirements are the same as those of sub-parts, and the anti-rust oil in the cavity must be blown clean.

[0074] Step 22: Before packaging, the workpiece shape must be scanned and confirmed. When the box is full, a box code is generated and the information is archived.

[0075] Step 23: Put qualified parts into storage.

[0076] By fine turning the left and right end pieces, it can be used to process thin-walled parts and ensure that the dimensional tolerance of the welding surface is ≤0.016mm. Through soft drawing, high-frequency quenching and tempering, magnetic particle inspection and hard drawing splines, it can be used to process shafts with high-precision splines. Magnetic particle inspection can be used to detect spline defects.

[0077] The left and right end pieces are joined together by laser welding, and the weld has a small heat-affected zone, high precision, and beautiful appearance. After the hollow shaft is welded, the weld quality needs to be ultrasonically checked to ensure that the product welding quality is qualified.

[0078] Through fine turning of welded components, it is used to process shafts with shrinkage at both ends, large diameter differences, and various grooves. Milling can be used to process various keyways, and grinding can be used to improve the dimensional accuracy of key parts to ensure a tolerance range of ≤0.013mm.

[0079] The dynamic balance of the workpiece after keyway machining is tested by dynamic balancing, and the cleanliness of the workpiece is ensured by ultrasonic cleaning.

[0080] Laser marking on the workpiece can be used to trace the processing information of a single workpiece.

[0081] This technical solution combines forging, machining, heat treatment, welding and multiple testing methods. The processed workpiece has high dimensional accuracy and can be used to produce motor shafts with complex appearance such as thin walls, necked ends, large diameter differences, hollow inner cavities, multiple grooves, oil holes, splines, and external keyways.

[0082] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A processing technology for long hollow shafts with complex shapes. It is characterized in that The following steps are involved: Step 1: Prepare the ingredients; Step 2: Warm forging; Step 3: Residual heat treatment; Step 4: Finish turning the right end piece; Step 5: Finish turning of the left end piece; Step 6: Soft pull spline; Step 7: high frequency quenching and tempering; Step 8: Magnetic particle inspection; Step 9: Cleaning; Step 10: Hard pull the spline; Step 11: Ultrasonic cleaning of sub-parts; Step 12: Pressing; Step 13: Laser welding; Step 14: Ultrasonic flaw detection; Step 15: Component finishing; Step 16: Milling; Step 17: Laser marking; Step 18: Grinding; Step 19: Dynamic balancing; Step 20: Sorting inspection; Step 21: ultrasonic cleaning of finished product; Step 22: Packaging; Step 23: Storage.

2. A process for processing a long hollow shaft of complex shape according to claim 1, It is characterized in that The step 1 material preparation includes three processes: blanking, chamfering and shot blasting; the step 2 warm forging adopts multi-station forging, and the workpiece is forged into a hollow shaft through forward extrusion, upsetting, reverse extrusion and punching, and the shape of the product structure is retained as much as possible; the step 3 residual heat treatment is operated online with the warm forging equipment, and the normalizing effect is achieved by controlling the furnace entry temperature, isothermal furnace temperature and holding time of the forging. After the residual heat treatment, the oxide scale of the forging is thin, and the shot blasting process can also be eliminated.

3. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that In step 4, the finishing turning of the right end piece is to complete the two processes of turning the inner hole and the outer circle, and the dimensional tolerance band of the welding surface is controlled within 0.016mm; in step 5, the finishing turning of the left end piece is to complete the two processes of turning the inner hole and the outer circle, and the dimensional tolerance band of the welding surface is controlled within 0.016mm.

4. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that In the steps six to nine, soft spline drawing, high-frequency quenching and tempering, and magnetic particle inspection are produced in a connected line; in the step seven, high-frequency quenching and tempering, the hardness of the quenching area is required to be 58-63HRC, and the quenching and tempering interval time is ≤30min; in the step eight, magnetic particle inspection is performed on 100% of the quenching area; in the step nine, there is no cleanliness requirement for cleaning, and it is mainly for cleaning magnetic powder.

5. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that The step 10 of hard drawing the spline is to improve the spline tooth profile accuracy.

6. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that In step 11, the ultrasonic cleaning of the sub-parts must ensure the cleanliness requirements, metal particle grade F, non-metal particle grade G, total mass ≤ 4 mg, and single fibers and fluff are allowed.

7. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that The press-fitting in step 12 is realized by a press-fitting machine, which controls the press-fitting into place by displacement, and there is an interference fit between the left end piece and the right end piece. The laser welding in step 13 must first be performed by half-power welding to ensure that the weld offset is qualified, and then by full-power welding to ensure that the weld depth is qualified; the ultrasonic flaw detection in step 14 checks the weld position to ensure the quality of the workpiece.

8. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that The component finishing turning in step 15 is divided into two sequences, firstly, processing multiple diameter sections on the outer circle, and then double-head turning to process various grooves; the milling in step 16 is to process various asymmetric keyways and oil holes on the outer circle; the laser marking in step 17 is used for internal traceability; the various key dimensions in step 18 are ground to ensure the dimensional accuracy of the workpiece, requiring the tolerance range to be ≤0.013mm.

9. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that The dynamic balance requirement of step 19 is ≤300mg; the selection inspection of step 20 is to conduct 100% inspection on all key dimensions through the final inspection machine; the finished product ultrasonic cleaning of step 21 is to clean and oil all qualified parts, and the cleanliness requirement is the same as that of sub-parts, and the anti-rust oil in the cavity must be blown clean.

10. The processing technology of a long hollow shaft with a complex shape according to claim 1, It is characterized in that In step 22, the workpieces must be scanned and confirmed before packaging, and a box code is generated after the box is full, and the information is archived; in step 23, qualified parts are put into storage.

Citation Information

Cited By

  • High-speed motor rotating shaft giving consideration to dynamic balance and wear resistance and machining method of high-speed motor rotating shaft

    CN121223440A