High-strength natural bamboo fiber bundle as well as extraction method and application thereof
Through gentle swelling treatment and delignin treatment combined with dry hydrogen bond reconstruction, the problem of poor mechanical properties of bamboo fiber bundles in traditional methods is solved, and the effective extraction and application of high-strength bamboo fiber bundles is achieved, with industrial potential.
Patent Information
- Application Number
- CN202411010471.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
When extracting bamboo fiber bundles in traditional physical or chemical methods, the bamboo fibers are incomplete in structure, poor mechanical properties, long processing time and large reagent dosage, which limits the preparation and application of high-strength bamboo fiber bundles.
The mild swelling treatment technology is used combined with delignin treatment, and the drying hydrogen bond reconstruction effect is used to improve the accessibility of bamboo, loosen the bamboo structure, reduce the damage to bamboo fibers by chemical treatment, and achieve the extraction of high-strength bamboo fiber bundles.
The extraction of high-strength bamboo fiber bundles is achieved, the natural structure is retained, the processing time is shortened, energy consumption and preparation cost is reduced, and the mechanical properties and industrial prospects of bamboo fiber bundles are improved.
Smart Images

Figure CN118952398A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-value processing and utilization of bamboo materials, and specifically relates to a high-strength bamboo fiber bundle and an extraction method and application thereof. Background Art
[0003] Natural bamboo fiber bundles have excellent mechanical properties and are called "natural glass fibers". The cell cavities of bamboo materials such as ducts, sieve tubes, and fibers are small in size and arranged in a radially non-uniform manner. The fiber cell walls are thick and have a complex structure of alternating thickness and thinness. The density of pore distribution and the diameter of pore openings are also small, which makes the overall porosity of bamboo materials small, the permeability is poor, and there are obvious heterogeneous characteristics. At present, the methods for extracting bamboo fiber bundles from bamboo materials mainly include physical methods, chemical methods, or physical and chemical combined methods. However, the traditional physical method of extracting bamboo fiber bundles is mainly through steam explosion, cracking and fiber opening, rolling and combing, etc., but the pure physical separation method requires repeated huge mechanical external forces, which destroys the natural structure of bamboo cellulose. The separation is carried out by chemical methods such as peroxy acid and alkali solution, but there are problems such as long chemical treatment time and large amount of chemical reagents, which leads to the destruction of the natural structure of the bamboo fiber bundle after treatment. Therefore, the mechanical properties of bamboo fibers prepared by the above method are poor, which limits their further processing and utilization.
[0004] The present invention firstly adopts a mild swelling treatment technology, which promotes the removal of part of lignin and hemicellulose while swelling and softening the bamboo material, loosens the dense structure inside the bamboo material, and can greatly improve the accessibility of the bamboo material while retaining the natural structure of the bamboo fiber bundle to prepare the swollen bamboo material; then the swollen bamboo material is subjected to delignification treatment to further remove the lignin and hemicellulose on the surface of the bamboo fiber bundle. Since the accessibility of the bamboo material is improved after the swelling treatment, the subsequent delignification process is short in time, and the damage to the natural structure of the bamboo fiber bundle caused by long-term chemical reagent treatment is avoided. In the process of delignification, on the one hand, the internal structure of the bamboo material is further loosened, and on the other hand, more hydroxyl groups on the surface of the bamboo fiber bundle are exposed, which provides a basis for the subsequent hydrogen bond recombination to construct a high-strength bamboo fiber bundle. Finally, the drying treatment is combined to realize the reconstruction of hydrogen bonds between and within the molecules of the bamboo fiber bundle, and the bamboo fiber bundle is given high strength while drying can continue to loosen the internal structure of the bamboo material. Therefore, only a small mechanical external force is required in the subsequent mechanical treatment (avoiding the damage to the natural structure of the bamboo fiber caused by the mechanical treatment), and the high-strength bamboo fiber bundle is obtained by efficient extraction. Summary of the invention
[0005] Purpose of the invention: The bamboo fiber bundles extracted by traditional physical or chemical methods have incomplete natural bamboo fiber bundle structures, poor mechanical properties, long processing time, and large reagent dosage, which seriously limits the preparation and application of high-strength bamboo fiber bundles. In view of the above problems, the present invention provides a method for preparing high-strength bamboo fiber bundles by combining mild swelling treatment technology with delignification treatment and drying hydrogen bond reconstruction effect. A mild swelling agent is used to improve the accessibility of bamboo materials, remove part of lignin and hemicellulose, well retain the structure of natural bamboo fiber bundles, and loosen the internal structure of bamboo materials, providing more space for subsequent delignification treatment, shortening the subsequent delignification treatment time, avoiding chemical treatment from damaging the structure of natural bamboo fiber bundles, and exposing more hydroxyl groups on the surface of bamboo fiber bundles in combination with delignification treatment, further loosening the internal structure of bamboo materials; through drying treatment, on the one hand, the hydrogen bond reconstruction within and between the cellulose chains of bamboo fiber bundles is achieved to obtain high-strength bamboo fiber bundles, and on the other hand, the internal structure of bamboo materials continues to be loosened. Finally, high-strength bamboo fiber bundles are extracted through relatively small external mechanical force (avoiding the destruction of the natural structure of bamboo fibers by mechanical treatment).
[0006] To this end, the specific technical solution adopted by the present invention is as follows:
[0007] A method for extracting high-strength bamboo fiber bundles comprises the following steps:
[0008] S1, removing the yellow and green parts of the bamboo and processing them into bamboo slices of a certain thickness;
[0009] S2, soaking the bamboo slices prepared in step S1 in a swelling agent for full swelling treatment, and then washing out the swelling agent to obtain swollen bamboo slices with a complete bamboo fiber bundle structure;
[0010] S3, soaking the swollen bamboo chips obtained in step S2 in a delignification solution until the bamboo chips are completely whitened, and then washing away the delignification solution to obtain delignified bamboo chips with a complete bamboo fiber bundle structure;
[0011] S4, drying the delignified bamboo chips obtained in step S3, and subjecting them to mechanical separation to obtain high-strength bamboo fiber bundles. The extraction rate of the high-strength bamboo fiber bundles relative to natural bamboo is 20-30%.
[0012] Furthermore, in step S1, the bamboo species of the bamboo material are bamboo of the Chinese genus Phyllostachys, Phyllostachys pubescens, Phyllostachys laurel, Phyllostachys cineraria, Phyllostachys glabra, Phyllostachys edulis, Phyllostachys pubescens, Phyllostachys rubra, Phyllostachys edulis, Phyllostachys purpurogenum, Phyllostachys nigra, Phyllostachys truncatula, Long-branched bamboo, Phyllostachys foetida, Tortoiseshell bamboo and Phyllostachys chinensis.
[0013] Furthermore, in step S1, the bamboo material may be dried or not dried, and the moisture content is 0-150%.
[0014] Furthermore, in step S1, the bamboo material is 1 year old, 2 years old, 3 years old or 4 years old.
[0015] Furthermore, in step S1, the bamboo part of the bamboo material is the green part near the bamboo, the fleshy part of the bamboo or the yellow part near the bamboo.
[0016] Furthermore, in step S1, the thickness of the bamboo material is 1-5 mm.
[0017] Furthermore, the swelling agent in step S2 is any one of water, a sulfuric acid solution with a mass fraction of 0-15wt% or a sodium hydroxide solution with a mass fraction of 0-12wt%.
[0018] Furthermore, the swelling agent in step S2 is a mixed solution composed of acidic and alkaline compounds.
[0019] Furthermore, the acidic compound is at least one of formic acid, acetic acid, lactic acid, oxalic acid, ethylene glycol, glycerol or urea.
[0020] Furthermore, the alkaline compound is at least one of choline chloride, zinc chloride, ammonium chloride, betaine or guanidine hydrochloride.
[0021] Furthermore, the molar ratio of the acidic and basic compounds in the mixed solution is 10:1-1:1.
[0022] Furthermore, the acidic compound in the mixed solution is any one of oxalic acid, lactic acid, formic acid, acetic acid, ethylene glycol, glycerol, and urea, and the alkaline compound is choline chloride.
[0023] Furthermore, in the mixed solution, the acidic compound is lactic acid, the alkaline compound is any one of choline chloride, zinc chloride, ammonium chloride, betaine, and guanidine hydrochloride, and the molar ratio of the acidic compound to the alkaline compound is 10:1.
[0024] Furthermore, in step S2, the swelling agent treatment temperature is 70-150° C., preferably 70-130° C.; the treatment time is 0.25-6 h, preferably 0.25-4 h.
[0025] Furthermore, in step S2, the solid-liquid ratio of the bamboo chips and the swelling agent is 1:5-1:15 (g / ml).
[0026] Furthermore, the water absorption weight gain rate of the swollen bamboo chips in step S2 is 160-220%, the lignin removal rate is 2-65%, and the hemicellulose removal rate is 1-55%.
[0027] Furthermore, in step S3, the delignification solution is any one of a mixed solution of acetic acid and hydrogen peroxide, a mixed solution of formic acid and hydrogen peroxide, a mixed solution of acetic acid and sodium chlorite, or a mixed solution of sodium hydroxide and sodium sulfite.
[0028] Furthermore, in the mixed solution of acetic acid and hydrogen peroxide, the volume ratio of acetic acid to hydrogen peroxide is 1:1; in the mixed solution of formic acid and hydrogen peroxide, the volume ratio of formic acid to hydrogen peroxide is 1:1; in the mixed solution of acetic acid and sodium chlorite, the concentration of sodium chlorite is 2wt%, and the pH is adjusted to 4.6 by acetic acid; in the mixed solution of sodium hydroxide and sodium sulfite, the concentrations of sodium hydroxide and sodium sulfite are 2.5M and 0.4M, respectively.
[0029] Furthermore, the solid-liquid ratio of the swollen bamboo chips to the delignified solution in step S3 is 1:5-1:15 (g / ml), the treatment time is 3-12 hours, and the treatment temperature is 50-100° C.; the removal rate of lignin in the delignified bamboo chips is 80-95%, and the removal rate of hemicellulose is 65-80%.
[0030] Furthermore, in step S4, the drying method is at least one of room temperature drying or oven drying.
[0031] Furthermore, in step S4, the mechanical separation is at least one of rubbing, rolling or combing.
[0032] According to another aspect of the present invention, a high-strength bamboo fiber bundle is provided, which is prepared by the high-strength bamboo fiber bundle extraction method.
[0033] Furthermore, the diameter of the high-strength bamboo fiber bundle is 150-350 μm, the diameter is evenly distributed along the length direction, the length is 2-30 cm, the aspect ratio is 50-2000, and the crystallinity is 50-72%.
[0034] Furthermore, the tensile stress of the high-strength bamboo fiber bundle is 1500-3500MPa, the Young's modulus is 25-70GPa, and the breaking energy is 20-95MJ / m 3 ;
[0035] Furthermore, the intramolecular hydrogen bond O(3)H...O(5) content of the high-strength bamboo fiber bundle increases by 20-30%, the O(2)H...O(6) content decreases by 25-35%, and the intermolecular hydrogen bond O(6)H...O(3') content increases by 5-15%.
[0036] According to another aspect of the present invention, an application of a high-strength bamboo fiber bundle is provided, such as the application of the high-strength bamboo fiber bundle in the fields of composite reinforcement materials, photovoltaics, energy storage, personal thermal management, and wearable smart fabrics.
[0037] Beneficial effects: Compared with the prior art, the advantages of the present invention include:
[0038] 1) The method for extracting high-strength bamboo fiber bundles of the present invention has the advantages of mild processing conditions, short processing time and small mechanical force, saves energy consumption, reduces preparation costs, and has industrial prospects.
[0039] 2) The high-strength bamboo fiber bundle extracted by the present invention retains the structure of the natural bamboo fiber bundle, has a uniform diameter distribution, and has a tensile strength of up to 3500 MPa.
[0040] 3) The bamboo fiber bundle of the present invention not only has high strength, but also has a large number of hydroxyl groups on the surface that provide a basis for subsequent functionalization, further promoting the application of bamboo fibers in the fields of composite reinforcement materials, photovoltaics, energy storage, personal thermal management, wearable smart fabrics, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a flow chart of the extraction of high-strength bamboo fiber bundles.
[0042] Figure 2 It is a diagram showing the roller separation effect of the delignified bamboo chips after drying in Comparative Example 1 and Example 9.
[0043] Figure 3 These are the mechanical properties of the high-strength bamboo fiber bundles extracted from the bamboo pieces, Comparative Example 1 and Example 9.
[0044] Figure 4 These are photographs of the winding, folding, knotting and lifting of a heavy object of the high-strength bamboo fiber bundle in Example 9.
[0045] Figure 5 It is a morphology diagram of the high-strength bamboo fiber bundle in Example 9, and its diameter and length distribution diagram.
[0046] Figure 6 It is the water absorption weight gain rate, lignin and hemicellulose content of the bamboo chips and swollen bamboo chips in Example 9.
[0047] Figure 7 1 is a scanning electron microscope photograph of the bamboo material, the swollen bamboo material and the high-strength bamboo fiber bundle in Example 9.
[0048] Figure 8 1 is a scanning electron microscope photograph of the swollen bamboo slices in Examples 1, 2, and 3.
[0049] Fig. 9These are the mechanical properties of bamboo fiber bundles extracted from 2 mm bamboo pieces in Examples 1, 2, 3, 4 and Comparative Example 1.
[0050] Fig.10 It is the phase change property of the bamboo fabric in Example 12. DETAILED DESCRIPTION
[0051] The following will be combined with the drawings, technical process steps, specific implementation conditions and materials in the invention examples to clearly and completely describe the technical solutions in the invention examples. Obviously, the described embodiments are only part of the embodiments of the invention, not all of the embodiments. Based on the embodiments of the invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the invention.
[0052] The method used in the present invention is applicable to various bamboo materials, and the bamboo materials can be derived from bamboos such as bamboos of the Chinese genus, bamboos of the moso type, bamboos of the reed type, bamboos of the laurel type, bamboos of the arrow type, bamboos of the spotted type, bamboos of the moso type, bamboos of the purple type, bamboos of the phoenix tail type, bamboos of the long branches, bamboos of the Buddha belly type, bamboos of the tortoise shell type, and bamboos of the golden jade type. The bamboo can be 1 year old, 2 years old, 3 years old, or 4 years old, etc.; the part can be near the green part of the bamboo, the fleshy part of the bamboo, or the yellow part of the bamboo, etc.; the thickness can be 1-5 mm; it can be from absolutely dry bamboo to water-saturated bamboo, and the moisture content can be 10-150%;
[0053] In the following examples, bamboo chips with a moisture content of 10-20% from the bamboo flesh of 2-year-old moso bamboo are used as raw materials to illustrate the present invention. The chemical components in the bamboo material are 37.7% cellulose, 26.2% lignin and 16.4% hemicellulose. The length is mainly limited by the length of the bamboo joints and can be 50mm, 100mm, 150mm, 200mm, 250mm and 300mm.
[0054] The unit of solid-liquid ratio used in the present invention is (g / ml). The solid-liquid ratio of bamboo material to swelling agent can be 1:5-1:15. The present invention is illustrated in the following embodiments with a solid-liquid ratio of 1:10.
[0055] The delignification solution used in the present invention can be a mixed solution of acetic acid and hydrogen peroxide, a mixed solution of formic acid and hydrogen peroxide, a mixed solution of acetic acid and sodium chlorite, or a mixed solution of sodium hydroxide and sodium sulfite, wherein acetic acid, formic acid and 30% hydrogen peroxide are commercially available reagents and are used directly. In the following examples, the present invention is described using a mixed solution of acetic acid and hydrogen peroxide as the delignification solution.
[0056] The delignified bamboo chips used in the present invention can be dried at room temperature or in an oven. In the following embodiments, the present invention is described by using the delignified bamboo chips dried in an oven.
[0057] The bamboo fiber bundle used in the present invention can be separated mechanically by rubbing, rolling or combing. In the following embodiments, the bamboo fiber bundle is extracted by rolling mechanical separation to illustrate the present invention.
[0058] Example 1
[0059] 1) Bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) were placed in deionized water at a solid-liquid ratio of 1:10 and fully mixed, and heated at 90°C for 1 hour to swell. After the reaction was completed, the bamboo chips were washed with deionized water to obtain swollen bamboo chips. The water absorption weight gain rate of the swollen bamboo chips was 166%, the lignin removal rate was 19%, and the hemicellulose removal rate was 14%.
[0060] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed. After heating at 80°C for 5 hours, the bamboo material turns white, and then the excess delignification solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 84%, and the removal rate of hemicellulose is 72%.
[0061] 3) The delignified bamboo chips were dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 250-350 μm, a length of 50 mm, a maximum tensile stress of 1512 MPa, a Young's modulus of 25 GPa, and a fracture energy of 35 MJ / m 3 According to the weight method analysis, 0.25g of high-strength bamboo fiber bundles can be extracted from 1g of natural bamboo, and the extraction rate is 25%.
[0062] Example 2
[0063] 1) sulfuric acid was prepared into a solution with a mass fraction of 2%, and bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) were placed in deionized water at a solid-liquid ratio of 1:10 and fully mixed, and heated at 90°C for 1 hour for swelling. After the reaction was completed, the bamboo chips were washed with deionized water to obtain swollen bamboo chips. The water absorption weight gain rate of the swollen bamboo chips was 172%, the lignin removal rate was 24%, and the hemicellulose removal rate was 20%.
[0064] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 5 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 82%, and the removal rate of hemicellulose is 76%.
[0065] 3) The delignified bamboo chips were dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 150-250 μm, a length of 50 mm, a maximum tensile stress of 1673 MPa, a Young's modulus of 37.7 GPa, and a fracture energy of 40.6 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 24%.
[0066] 4) The effects of different acid concentrations on the fiber strength were studied separately. As shown in the following table, it can be seen that when the acid concentration is 15%, the strength of the bamboo fiber is the lowest, indicating that high concentrations of acid have a negative effect on the strength of the bamboo fiber.
[0067] Acid concentration (wt%) Tensile stress (MPa) Young's modulus(GPa) <![CDATA[Fracture energy (MJ / m 3 )]]> 2 1673 37.7 40.6 5 1623 33.4 48.3 10 1648 31.9 42.9 15 1522 30.6 38.8
[0068] Example 3
[0069] 1) Prepare a 2% mass fraction of sodium hydroxide solution, put bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) into deionized water at a solid-liquid ratio of 1:10 and fully mix, heat and swell at 90°C for 1 hour, and wash the excess swelling solution with deionized water after the reaction is completed to obtain swollen bamboo chips. The water absorption weight gain rate of the swollen bamboo chips is 202%, the lignin removal rate is 13%, and the hemicellulose removal rate is 44%.
[0070] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3 hours until the bamboo turns white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 95%, and the removal rate of hemicellulose is 75%.
[0071] 3) The delignified bamboo chips were dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 150-200 μm, a length of 50 mm, a maximum tensile stress of 1745 MPa, a Young's modulus of 33.9 GPa, and a fracture energy of 48.1 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 21%.
[0072] 4) The effects of different alkali concentrations on the fiber strength were studied separately. As shown in the following table, it can be seen that the higher the alkali concentration, the lower the strength of the bamboo fiber. Too high an alkali concentration will destroy the natural structure of the bamboo fiber, resulting in a decrease in its strength.
[0073]
[0074] Example 4
[0075] 1) Select lactic acid as an acidic solvent and choline chloride as an alkaline solvent, and configure a mixed solution with a molar ratio of 10:1. Put bamboo chips (length 50mm, width 20mm, thickness range 1-5mm) into the configured solution according to a solid-liquid ratio of 1:10 and fully mix. In order to ensure the swelling effect, bamboo chips of different thicknesses are heated and swollen at 110°C for 1-3h. After the reaction is completed, the bamboo chips are washed with a mixed solution of ethanol and deionized water to wash the excess swelling solution, and finally washed with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 170-180%, the lignin removal rate is 10-20%, and the hemicellulose removal rate is 20-30%.
[0076] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3-5 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 85-95%, and the removal rate of hemicellulose is 70-80%.
[0077] 3) Dry the delignified bamboo chips in an oven at 60°C, and efficiently separate the bamboo fiber bundles by roller pressing, with a diameter of 200-300 μm, a length of 50 mm, a tensile stress of 2800-3300 MPa, a Young's modulus of 60-70 GPa, and a fracture energy of 70-85 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 23-28%.
[0078] 4) The relationship between bamboo material thickness and bamboo fiber bundle strength is shown in the following table. It can be seen that through the present invention, bamboo materials with a thickness of 1-5 mm can be processed and extracted to obtain high-strength bamboo cellulose, among which bamboo materials with a thickness of 2 mm have the highest tensile strength.
[0079] Bamboo thickness (mm) Tensile stress (MPa) Young's modulus(GPa) <![CDATA[Fracture energy (MJ / m 3 )]]> 1 3065 67.3 79.9 2 3291 68.7 83.8 3 3162 69.4 82.1 4 2896 61.7 76.6 5 3106 60.3 71.9
[0080] Example 5
[0081] 1) Select lactic acid as an acidic solvent and choline chloride as an alkaline solvent, and configure a mixed solution at a molar ratio of 10:1. Put bamboo chips (length 50mm, width 20mm, thickness 2mm) into the configured solution according to a solid-liquid ratio of 1:10 and fully mix them. Heat and swell them at 70-130°C for 1h. After the reaction is completed, the bamboo chips are washed with a mixed solution of ethanol and deionized water to wash the excess swelling solution, and finally washed with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 170-185%, the lignin removal rate is 10-55%, and the hemicellulose removal rate is 10-45%.
[0082] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3-5 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 80-95%, and the removal rate of hemicellulose is 65-80%.
[0083] 3) The delignified bamboo chips are dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 200-350 μm, a tensile stress of 2500-3300 MPa, a Young's modulus of 50-70 GPa, and a fracture energy of 60-85 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 20-27%.
[0084] 4) The relationship between swelling treatment temperature and bamboo fiber bundle strength is shown in the following table. It can be seen that when the treatment temperature is 110℃, the bamboo tensile strength is the highest.
[0085] Swelling treatment temperature (℃) Tensile stress (MPa) Young's modulus(GPa) <![CDATA[Fracture energy (MJ / m 3 )]]> 70 2596 52.1 62.7 90 3054 62.6 74.9 110 3291 68.7 83.8 130 2835 60.2 71.4
[0086] Example 6
[0087] 1) Select lactic acid as an acidic solvent and choline chloride as an alkaline solvent, and configure a mixed solution at a molar ratio of 10:1. Put bamboo chips (length 50mm, width 20mm, thickness 2mm) into the configured solution according to a solid-liquid ratio of 1:10 and fully mix them. Heat and swell them at 110°C for 0.25-4h. After the reaction is completed, the bamboo chips are washed with a mixed solution of ethanol and deionized water to clean the excess swelling solution, and finally washed with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 165-200%, the lignin removal rate is 1-45%, and the hemicellulose removal rate is 5-55%.
[0088] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3-5 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 80-95%, and the removal rate of hemicellulose is 65-80%.
[0089] 3) The delignified bamboo chips are dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 200-350 μm, a tensile stress of 2000-3300 MPa, a Young's modulus of 45-70 GPa, and a fracture energy of 55-85 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 21-26%.
[0090] 4) The relationship between swelling treatment time and bamboo fiber bundle strength is shown in the following table. It can be seen that when the treatment time is 1h, the bamboo tensile strength is the highest.
[0091] Swelling treatment time (h) Tensile stress (MPa) Young's modulus(GPa) <![CDATA[Fracture energy (MJ / m 3 )]]> 0.25 2510 47.4 60.8 0.5 2924 54.2 74.7 1 3291 68.7 83.8 1.5 3111 57.4 69.3 2 2979 62.7 70.5 3 2433 46.9 63.8 4 2229 48.4 58.6
[0092] From the above examples 4-6, it can be seen that, due to the synergistic effect of swelling treatment + delignification + drying hydrogen bond reconstruction effect in the present invention, it is necessary to balance the swelling effect, the delignification effect and the destruction of the natural structure of bamboo cellulose. Therefore, the strength of the bamboo fiber bundle is not in a simple linear relationship with the thickness of the bamboo material, the swelling treatment temperature and the time.
[0093] Example 7
[0094] 1) Select the acidic solvent as lactic acid and the alkaline solvent as any one of choline chloride, zinc chloride, ammonium chloride, betaine, and guanidine hydrochloride, and configure a mixed solution with a molar ratio of 10:1, put bamboo chips (length 50mm, width 20mm, thickness 2mm) into the configured solution according to the solid-liquid ratio of 1:10 and fully mix, heat and swell at 110°C for 1h, after the reaction is completed, wash the excess swelling solution with a mixed solution of ethanol and deionized water, and finally wash with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 165-210%, the lignin removal rate is 10-55%, and the hemicellulose removal rate is 20-60%.
[0095] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3-4 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 80-90%, and the removal rate of hemicellulose is 75-80%.
[0096] 3) The delignified bamboo chips are dried in an oven at 60°C, and the bamboo fiber bundles are efficiently separated by roller pressing, with a diameter of 200-300 μm, a length of 50 mm, a tensile stress of 2400-3300 MPa, a Young's modulus of 55-70 GPa, and a fracture energy of 60-85 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 22-27%.
[0097] 4) The relationship between the swelling agents prepared with different alkaline compounds and the strength of the bamboo fiber bundle is shown in the following table. It can be seen that due to the different swelling effects of different swelling agents, the strength of the extracted bamboo fiber bundle is different.
[0098] Basic compounds Tensile stress (MPa) Young's modulus(GPa) <![CDATA[Fracture energy (MJ / m 3 )]]> Choline chloride 3291 68.7 83.8 Zinc chloride 2726 62.8 70.6 Ammonium chloride 2828 59.8 68.4 Betaine 2452 54.4 64.1 Guanidine hydrochloride 2663 55.3 63.9
[0099] Example 8
[0100] 1) Select an acidic solvent such as lactic acid, formic acid, acetic acid, ethylene glycol, glycerol, or urea, and an alkaline solvent such as choline chloride, and configure a mixed solution with different acid-base molar ratios. Put bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) into the configured solution and mix them thoroughly according to a solid-liquid ratio of 1:10, heat and swell at 110°C for 1 hour, and after the reaction is completed, wash the excess swelling solution with a mixed solution of ethanol and deionized water, and finally wash with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 165-185%, the lignin removal rate is 2-35%, and the hemicellulose removal rate is 2-25%.
[0101] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3-5 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 80-90%, and the removal rate of hemicellulose is 70-80%.
[0102] 3) The delignified bamboo chips are dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 150-350 μm, a tensile stress of 2227-3300 MPa, a Young's modulus of 45-70 GPa, and a fracture energy of 60-85 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 24-27%.
[0103] 4) The relationship between the swelling agents prepared with different acidic compounds and the strength of the bamboo fiber bundle is shown in the following table. It can be seen that due to the different swelling effects of different swelling agents, the strength of the extracted bamboo fiber bundle is different.
[0104]
[0105] Example 9
[0106] 1) Select oxalic acid as an acidic solvent and choline chloride as an alkaline solvent, and prepare a mixed solution at a molar ratio of 1:1. Put bamboo chips (length 300 mm, width 20 mm, thickness 2 mm) into the prepared solution according to a solid-liquid ratio of 1:10 and mix them thoroughly. Heat and swell them at 110°C for 1 hour. After the reaction is completed, wash the excess swelling solution with a mixed solution of ethanol and deionized water, and finally wash them with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 191%, the lignin removal rate is 30%, and the hemicellulose removal rate is 23%.
[0107] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 92%, and the removal rate of hemicellulose is 88%.
[0108] 3) After the delignified bamboo chips were dried in an oven at 60°C, bamboo fiber bundles were efficiently separated by manual rubbing, with a diameter of 300-350 μm, a length of 300 mm, an aspect ratio of 1000, and a crystallinity of 72%. The maximum tensile stress was 3500 MPa, the Young's modulus was 70.0 GPa, and the fracture energy was 95.0 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 29%.
[0109] Example 10
[0110] On the basis of Example 9, the effect of the drying method on the high-strength bamboo fiber bundle was also investigated: the delignified bamboo pieces in step 2) were replaced with ethanol, dried at room temperature, and then efficiently separated by manual rubbing to obtain bamboo fiber bundles with a diameter of 250-350 μm, a length of 300 mm, a maximum tensile stress of 3379 MPa, a Young's modulus of 66.8 GPa, and a fracture energy of 84.1 MJ / m 3 This shows that the high-strength bamboo fiber bundle can be efficiently extracted by drying at room temperature. The extraction rate of the high-strength bamboo fiber bundle relative to the natural bamboo material is 27%.
[0111] On the basis of Example 9, the effect of mechanical treatment method on high-strength bamboo fiber bundles was also investigated. The delignified bamboo chips in step 2) were dried in an oven at 60°C, and then rolled 20 times to obtain bamboo fiber bundles with high efficiency separation. The bamboo fiber bundles had a diameter of 300-350 μm, a length of 50 mm, a maximum tensile stress of 3382 MPa, a Young's modulus of 69.1 GPa, and a fracture energy of 94.4 MJ / m 3 This shows that the high-strength bamboo fiber bundle can be efficiently extracted by roller separation in the present invention. The extraction rate of the high-strength bamboo fiber bundle relative to the natural bamboo material is 30%.
[0112] Embodiment 11
[0113] 1) Select oxalic acid as an acidic solvent and choline chloride as an alkaline solvent, and prepare a mixed solution at a molar ratio of 1:1. Put bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) into the prepared solution according to a solid-liquid ratio of 1:10 and fully mix them. Heat and swell them at 110°C for 1 hour. After the reaction is completed, wash the excess swelling solution with a mixed solution of ethanol and deionized water, and finally wash them with deionized water to obtain swollen bamboo chips. The volume ratio of ethanol to deionized water is preferably 7:3-10:0. The water absorption weight gain rate of the swollen bamboo chips is 191%, the lignin removal rate is 30%, and the hemicellulose removal rate is 23%.
[0114] The following 2)-5) are treated with different delignification solutions to study the promoting effect of swelling treatment on the delignification effect.
[0115] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 92%, and the removal rate of hemicellulose is 88%.
[0116] 3) A mixed solution of formic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 50°C for 12 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 94%, and the removal rate of hemicellulose is 86%.
[0117] 4) Prepare a sodium chlorite solution with a concentration of 2wt%, adjust the pH to 4.6 with acetic acid to obtain a mixed solution, immerse the swollen bamboo chips in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mix, heat the delignified bamboo chips at 80°C for 6 hours until the bamboo turns white, then wash the excess delignified solution with a mixed solution of ethanol and deionized water, and finally wash with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 89%, and the removal rate of hemicellulose is 87%.
[0118] 5) Prepare a mixed solution of 2.5M sodium hydroxide and 0.4M sodium sulfite, immerse the swollen bamboo chips in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mix, heat the delignified bamboo chips at 100°C for 5 hours until the bamboo turns white, then wash the excess delignified solution with a mixed solution of ethanol and deionized water, and finally wash with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 94%, and the removal rate of hemicellulose is 90%.
[0119] 6) After drying the above four delignified bamboo chips in an oven at 60°C, bamboo fiber bundles were efficiently separated by manual rubbing, with a diameter of 250-350 μm, a length of 50 mm, an aspect ratio of 50-2000, a crystallinity of 50-70%, a maximum tensile stress of 3000-3500 MPa, a Young's modulus of 65-75 GPa, and a fracture energy of 85-95 MJ / m 3 The extraction rate of high-strength bamboo fiber bundles relative to natural bamboo is 26-29%. The intramolecular hydrogen bond O(3)H...O(5) content of high-strength bamboo fiber bundles increased by 20-30%, the O(2)H...O(6) content decreased by 25-35%, and the intermolecular hydrogen bond O(6)H...O(3') content increased by 5-15%.
[0120] It can be seen that the present invention can extract high-strength bamboo fiber bundles from natural bamboo materials by combining swelling treatment with different delignification treatments. The hydrogen bond reconstruction of the bamboo fiber bundle after drying is one of the important reasons for its high strength.
[0121] Example 12
[0122] A preparation method of bamboo phase change fabric
[0123] 1) The bamboo fiber bundle extracted in Example 9 was placed in pyrrole for vacuum impregnation, and then a mixed solution of ferric chloride and 0.3M hydrochloric acid solution with a mass ratio of 1:9 was added to the reaction solution, and the mixture was reacted at 4° C. for 24 hours. After the reaction was completed, the excess reaction solution was washed with 0.05M hydrochloric acid solution, and finally washed with deionized water and dried to obtain a polypyrrole bamboo fiber bundle.
[0124] 2) placing the polypyrrole bamboo fiber bundle in molten polyethylene glycol for vacuum impregnation, taking it out and cooling it to obtain the polypyrrole / polyethylene glycol bamboo fiber bundle.
[0125] 3) A layer of polyvinylidene fluoride is coated on the surface of the polypyrrole / polyethylene glycol bamboo fiber bundle, and then the bamboo phase change fiber is obtained after drying.
[0126] 4) Weaving bamboo phase change fibers to obtain polypyrrole bamboo phase change fabrics.
[0127] 5) Select the bamboo fiber bundle extracted from Example 9 and weave it to obtain bamboo fabric
[0128] 6) The bamboo fiber bundle extracted in Example 9 was selected and placed in molten polyethylene glycol for vacuum impregnation, and a layer of polyvinylidene fluoride was coated on the surface. After drying, bamboo phase change fibers were obtained, and bamboo phase change fabrics were woven.
[0129] Comparative Example 1
[0130] 1) Take bamboo chips (length 50 mm, width 20 mm, thickness 2 mm), prepare a mixed solution of acetic acid and hydrogen peroxide in a volume ratio of 1:1, immerse the bamboo chips in the prepared mixed solution in a solid-liquid ratio of 1:10 and fully mix, heat delignify at 80°C for 16 hours until the bamboo turns white, then wash the excess delignify solution with a mixed solution of ethanol and deionized water, and finally wash with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 95%, and the removal rate of hemicellulose is 85%.
[0131] 2) The delignified bamboo chips were dried in an oven at 60°C. Compared with Example 9 in which the bamboo fiber bundles were separated by rolling 20 times, the bamboo fiber bundles in this example could not be effectively separated by rolling 40 times. This shows that in the present invention, bamboo fibers cannot be separated from bamboo chips that have not been subjected to swelling treatment. This shows that swelling treatment plays a key role in the efficient extraction of high-strength bamboo fiber bundles in the present invention. Subsequently, bamboo fibers can be separated by increasing the mechanical treatment force, but the separation effect is not good. The diameter is 300-400μm, the tensile stress is 672MPa, the Young's modulus is 14.4GPa, and the fracture energy is 16.8MJ / m 3. The extraction rate of bamboo fiber bundles relative to natural bamboo is 12%. The hydrogen bond content of the bamboo fiber bundles extracted from Comparative Example 1 and Example 9 was tested respectively and is shown in the following table. Among them, the content of intramolecular hydrogen bonds O(3)H...O(5) increased by 24%, the content of O(2)H...O(6) decreased by 30%, and the content of intermolecular hydrogen bonds O(6)H...O(3') increased by 7%, which shows that the hydrogen bonds of the bamboo fiber bundles treated with swelling of the present invention have been reconstructed, the content of intermolecular hydrogen bonds has increased, and the intramolecular hydrogen bonds have changed from one type to two types of combined action, which confirms that the present invention has endowed the bamboo fiber bundles with higher mechanical properties through hydrogen bond reconstruction.
[0132]
[0133] Comparative Example 2
[0134] 1) sulfuric acid was prepared into a mixed solution with a mass fraction of 20%, and bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) were placed in deionized water and fully mixed at a solid-liquid ratio of 1:10, and heated at 90°C for 1 hour for swelling. After the reaction was completed, the bamboo chips were washed with deionized water to obtain swollen bamboo chips. The water absorption weight gain rate of the swollen bamboo chips was 186%, the lignin removal rate was 21%, and the hemicellulose removal rate was 28%.
[0135] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 4 hours until the bamboo turns white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 84%, and the removal rate of hemicellulose is 79%.
[0136] 3) The delignified bamboo chips were dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 200-250 μm, a tensile stress of 567 MPa, a Young's modulus of 12.5 GPa, and a fracture energy of 15.8 MJ / m 3 The extraction rate of bamboo fiber bundles relative to natural bamboo is 17%. Due to the high acid concentration, the natural structure of bamboo fiber bundles is destroyed and partially chemically degraded, resulting in a decrease in its mechanical properties and a lower extraction rate.
[0137] Comparative Example 3
[0138] 1) Sodium hydroxide was prepared into a mixed solution with a mass fraction of 20%, and bamboo chips (length 50 mm, width 20 mm, thickness 2 mm) were placed in deionized water and fully mixed at a solid-liquid ratio of 1:10, and heated and swollen at 90°C for 1 hour. After the reaction was completed, the bamboo chips were washed with deionized water to obtain swollen bamboo chips. The water absorption weight gain rate of the swollen bamboo chips was 237%, the lignin removal rate was 27%, and the hemicellulose removal rate was 52%.
[0139] 2) A mixed solution of acetic acid and hydrogen peroxide is prepared in a volume ratio of 1:1, and the swollen bamboo chips are immersed in the prepared mixed solution at a solid-liquid ratio of 1:10 and fully mixed, and the delignified bamboo chips are heated at 80°C for 3 hours until the bamboo becomes white, and then the excess delignified solution is washed with a mixed solution of ethanol and deionized water, and finally washed with deionized water to obtain delignified bamboo chips. The volume ratio of ethanol to deionized water is preferably 1:1. The removal rate of lignin in the delignified bamboo chips is 92%, and the removal rate of hemicellulose is 88%.
[0140] 3) The delignified bamboo chips were dried in an oven at 60°C and efficiently separated by roller pressing to obtain bamboo fiber bundles with a diameter of 150-200 μm, a tensile stress of 626 MPa, a Young's modulus of 10.2 GPa, and a fracture energy of 17.7 MJ / m 3 The extraction rate of bamboo fiber bundles relative to natural bamboo is 15%. Due to the high alkali concentration, the bamboo fiber bundles are structurally destroyed and partially chemically degraded, resulting in a decrease in its mechanical properties and a lower extraction rate.
[0141] The delignified bamboo chips obtained in Comparative Example 1 and Example 9 were dried and rolled to separate the Figure 2 As shown in the figure, the delignified bamboo chips of Example 9 can be rolled 20 times to effectively separate the bamboo fiber bundles. However, the delignified bamboo chips of Comparative Example 1 cannot be effectively separated from the bamboo fiber bundles after being rolled 40 times.
[0142] The mechanical properties of the bamboo fiber bundles extracted from natural bamboo pieces, Comparative Example 1 and Example 9 are as follows: Figure 3 As shown. The tensile stress of the bamboo fiber bundle of Example 9 is 3500MPa, which is 28.2 times the tensile stress of the bamboo sheet (124MPa) and 5.2 times the tensile stress of the comparative example 1 (672MPa), showing excellent tensile properties. And the Young's modulus and breaking energy of the bamboo fiber bundle of Example 9 also reached 70.0GPa and 95.0MJ / m-3, which are 12.3 times and 69.3 times of the bamboo sheet (5.71GPa and 1.37MJ / m-3), and 4.9 times and 5.7 times of the comparative example 1 (14.41GPa and 16.75MJ / m-3), and also have excellent rigidity and toughness.
[0143] The flexibility of the high-strength bamboo fiber bundle extracted in Example 9 is as follows Figure 4 This shows that the bamboo fiber bundle extracted by the present invention has excellent flexibility when being wound, folded, and knotted, and a single bamboo fiber bundle can lift a weight of 2.5 kg.
[0144] The size uniformity of the high-strength bamboo fiber bundle extracted in Example 9 is as follows Figure 5 This shows that the length of the bamboo fiber bundle can reach 30cm, and the diameter can maintain excellent uniformity, and its diameter observed from both ends and the middle is about 330 microns.
[0145] The water absorption weight gain rate, lignin and hemicellulose content of the bamboo chips and swollen bamboo chips in Example 9 are as follows: Figure 6 This indicates that the swelling treatment opens the natural anti-dissociation physical barrier on the bamboo surface and removes non-fixed substances such as lignin and hemicellulose, which improves the accessibility of the bamboo and is conducive to the entry and treatment of the delignification solution.
[0146] The scanning electron microscope photos of the bamboo chips, swollen bamboo chips and high-strength bamboo fiber bundles in Example 9 are as follows: Figure 7 This indicates that after the swelling agent treatment, the cell wall of the bamboo material becomes thinner and the cell corners are opened, which is conducive to the subsequent delignification treatment. And after delignification and drying, the vascular bundle and vessel structure of the high-strength bamboo fiber bundle are complete, with a diameter of about 330μm.
[0147] Scanning electron microscopy of the swollen bamboo pieces obtained in Examples 1, 2 and 3 shows Figure 8 After treatment with water and acidic solvents as swelling agents, the cell corners are opened to a certain extent, and the cell walls of thin-walled cells become thinner; while after treatment with alkaline solvents as swelling agents, the structure of thin-walled cells is destroyed, which is conducive to their removal.
[0148] The mechanical properties of the bamboo fiber bundles extracted from the 2 mm bamboo pieces in Examples 1, 2, 3, 4 and Comparative Example 1 are as follows: Fig. 9 The mechanical properties of the bamboo fiber bundle extracted in Example 4 are significantly better than those in Examples 1, 2, 3 and Comparative Example 1.
[0149] The phase change properties of the bamboo fabric obtained in Example 12 are as follows: Fig.10 This shows that the bamboo phase change fabrics after functionalization of bamboo fiber bundles have excellent phase change properties.
Claims
1. A method for extracting high-strength bamboo fiber bundles, characterized in that: The following steps are involved: S1, removing the yellow and green parts of the bamboo and processing them into bamboo slices with a thickness of 1-5 mm; S2, soaking the bamboo slices prepared in step S1 in a swelling agent to fully swell the bamboo slices, so as to obtain swollen bamboo slices with a complete bamboo fiber bundle structure; S3, soaking the swollen bamboo chips obtained in step S2 in a delignification solution to obtain delignified bamboo chips with a complete bamboo fiber bundle structure; S4, drying the delignified bamboo chips obtained in step S3, and then subjecting them to mechanical separation to extract high-strength bamboo fiber bundles; the drying method is room temperature drying or oven drying; the mechanical separation method is at least one of rubbing, rolling or combing. The extraction rate of the high-strength bamboo fiber bundle relative to natural bamboo is 20-30%.
2. The method for extracting high-strength bamboo fiber bundles according to claim 1, characterized in that: The swelling agent in step S2 is any one of water, a sulfuric acid solution with a mass fraction of 0-15wt% or a sodium hydroxide solution with a mass fraction of 0-12wt%.
3. The method for extracting high-strength bamboo fiber bundles according to claim 1, characterized in that: The swelling agent in step S2 is a mixed solution composed of acidic and alkaline compounds; the acidic compound is at least one of formic acid, acetic acid, lactic acid, oxalic acid, ethylene glycol, glycerol or urea; the alkaline compound is at least one of choline chloride, zinc chloride, ammonium chloride, betaine or guanidine hydrochloride; the molar ratio of the acidic and alkaline compounds in the mixed solution is 10:1-1:
1.
4. A method for extracting high-strength bamboo fiber bundles according to any one of claims 1 to 3, characterized in that: The swelling treatment time of step S2 is 0.25-4h, the swelling treatment temperature is 70-130°C, and the solid-liquid ratio of the bamboo slices to the swelling liquid is 1:5-1:15 (g / ml).
5. The method for extracting high-strength bamboo fiber bundles according to claim 1, characterized in that: The water absorption weight gain rate of the swollen bamboo chips in step S2 is 160-220%, the lignin removal rate is 2-65%, and the hemicellulose removal rate is 1-55%.
6. The method for extracting high-strength bamboo fiber bundles according to claim 1, characterized in that: The delignification solution described in step S3 is any one of a mixed solution of acetic acid and hydrogen peroxide, a mixed solution of formic acid and hydrogen peroxide, a mixed solution of acetic acid and sodium chlorite, or a mixed solution of sodium hydroxide and sodium sulfite; the solid-liquid ratio of the swollen bamboo chips to the delignification solution is 1:5-1:15 (g / ml), the treatment time is 3-12h, and the treatment temperature is 50-100°C; the removal rate of lignin in the delignified bamboo chips is 80-95%, and the removal rate of hemicellulose is 70-85%.
7. A high-strength bamboo fiber bundle, characterized in that: The high-strength bamboo fiber bundle is extracted by the preparation method of any one of claims 1 to 6.
8. The high-strength bamboo fiber bundle according to claim 7, characterized in that: The high-strength bamboo fiber bundle has a diameter of 150-350 μm, is evenly distributed along the length direction, has a length of 20-300 mm, an aspect ratio of 50-2000, and a crystallinity of 50-70%.
9. The high-strength bamboo fiber bundle according to claim 7, characterized in that: The tensile stress of the high-strength bamboo fiber bundle is 1500-3500MPa, the Young's modulus is 25-70GPa, and the breaking energy is 35-95MJ / m 3 .
10. Application of high-strength bamboo fiber bundles, application of the high-strength bamboo fiber bundles as described in any one of claims 7 to 9 in the fields of composite reinforcement materials, photovoltaics, energy storage, personal thermal management, and wearable smart fabrics.
Citation Information
Patent Citations
Bamboo fiber dissolving pulp and production technology thereof
CN102978993A
TiO2 / polypyrrole / lignocellulose composite material capable of releasing negative oxygen ions and preparation method thereof
CN110724391A
Preparation method of wall-broken separated bunchy bamboo fibers
CN112976195A
Method for preparing environment-friendly biological board by taking waste rubber wood as raw material