Biomass carbon-based composite material prepared by Joule hot method in flash macro-quantity manner and application of biomass carbon-based composite material

Through the Joule rapid heating method combined with nitrogen source and nickel source, the problem of complex and low efficiency of the preparation steps of traditional corn straw electrocatalysts is solved, and the efficient macro preparation of biomass carbon-based materials is achieved and the efficient electrochemical reduction of CO2 is suitable for large batches. Production and resource utilization.

CN118996481APending Publication Date: 2024-11-22JIANGSU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411099101.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The preparation steps of traditional corn straw electrocatalysts are complex and inefficient, and the macro-quantitative industrial application of biomass carbon-based catalysts cannot be realized.

Method used

The biomass carbon-based composite material was prepared by using the joule rapid heating method, corn stalks were combined with nitrogen and nickel sources, and a series of processing steps such as ball milling, ultrasonic washing, calcining and joule calcining.

Benefits of technology

It realizes efficient macro-preparation of biomass carbon-based materials, with mild processing conditions, short reaction time, low energy consumption and environmentally friendly characteristics, is suitable for large-scale production, and promotes efficient electrochemical reduction and resources of CO2. utilizing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996481A_ABST
    Figure CN118996481A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass carbon-based composite material prepared by a Joule heat method in a flash macro-quantity manner and application thereof, and relates to the technical field of electro-catalytic materials. According to the method, a Joule rapid heating method is adopted, corn straw is selected as a raw material, a nitrogen source and a nickel source are introduced, the functional biomass carbon-based composite material is prepared in a flash macro-quantity mode, and the catalyst is used for the field of electrocatalytic CO2 reduction and shows excellent catalytic performance; in addition, the technology is green and environment-friendly, the raw materials used in the technology are cheap and easily available, the treatment time is short, the reaction is mild, the energy consumption is low, the method has very high application value and very good application prospect, the whole preparation process has very high yield, the operation is simple, the repeatability is good, the controllability is strong, the method is green and environment-friendly, and the method is beneficial to industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalytic materials, and in particular to a method for flash mass-production of biomass carbon-based composite materials using a Joule heat method and application thereof. Background Art

[0002] Generally speaking, the yield ratio between corn and corn stalks is about 1:0.8, which means that about 231 million tons of corn stalks can be harvested each year. Straw residues are a byproduct of agricultural resources in many regions and are widely used in many agricultural industries. However, the most common utilization method currently is to burn the straw and return it to the field. This not only has a low resource utilization rate, but also brings about a large amount of CO2 emissions, causing secondary damage to the environment.

[0003] At present, people have proposed a variety of CO2 emission reduction and utilization solutions, such as carbon capture and storage technology, electrochemical CO2 reduction technology, etc. Among these technologies, it is generally believed that the use of carbon-based materials for CO2 adsorption, conversion and storage is a promising treatment method.

[0004] Studies have found that biomass carbon-based materials co-doped with nickel and nitrogen have particularly outstanding CO2RR performance. However, there are many problems in its preparation process, which cannot avoid the problems of cumbersome operation, long preparation process, low product yield, and large batch variability, so that biomass carbon-based catalysts have not yet been widely used in the market. Therefore, to achieve the industrial application of agricultural waste, the problem of macro-quantity preparation must be solved first. In recent years, the application of methods such as laser induction, high voltage pulse and Joule rapid heating has gradually become a new idea for the research on macro-preparation of solid carbon-based materials. In recent years, the Joule rapid heating method has been considered to be an innovative and efficient method based on electric Joule heating. The target temperature can be reached in an ultra-short processing time, which can overcome the problem of uneven distribution of active sites caused by differences in thermal migration rates. Rapid reorganization of carbon structure can be achieved through instantaneous high energy and high heat, thereby realizing the functional modification and macro-preparation of biomass carbon-based materials. Summary of the invention

[0005] The purpose of the present invention is to address the defects of traditional corn straw electrocatalysts such as complex preparation steps and low efficiency, and to use the Joule rapid heating method to achieve efficient and large-scale preparation of electrocatalytic CO2 catalysts using corn straw as a precursor, thereby realizing the industrialized, kilogram-level preparation of biomass carbon-based materials.

[0006] In order to achieve the above-mentioned invention object, the present invention provides the following technical solution: a Joule heat method for flash mass production of biomass carbon-based composite materials, comprising the following preparation steps:

[0007] (1) ball milling corn stalks for 30 to 60 minutes, then crushing through a 200-mesh sieve, ultrasonically washing with deionized water, filtering, taking solids, and freeze-drying to obtain corn stalk powder;

[0008] (2) calcining the corn straw powder to obtain a corn straw carbon precursor;

[0009] (3) mixing the corn stalk carbon precursor and the alkali source uniformly, and then calcining and activating them to obtain intermediate A;

[0010] (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 24 to 48 h to obtain biomass carbon powder;

[0011] (5) mixing biomass carbon powder, dicyandiamide and nickel chloride hexahydrate to obtain a mixture;

[0012] (6) The mixture is subjected to Joule calcination to obtain a biomass carbon-based composite material.

[0013] Furthermore, in step (1), the ultrasonic rate is 21 kHz and the time is 2 to 3 hours.

[0014] Furthermore, the freeze-drying temperature in step (1) is -45°C and the time is 24 to 48 hours.

[0015] Furthermore, in step (1), the mass ratio of the corn stalks to the deionized water is 5-8:10-15.

[0016] Furthermore, the calcination conditions in step (2) are: nitrogen atmosphere, 500° C., and time 5 h.

[0017] Furthermore, the calcination conditions in step (3) are: nitrogen atmosphere, heating rate of 5°C / min, temperature of 800°C, and time of 2h.

[0018] Furthermore, the alkali source in step (3) is potassium hydroxide, and the mass ratio of the corn stalk carbon precursor to potassium hydroxide is 1:2.

[0019] Furthermore, in step (5), the mass ratio of the biomass carbon powder, dicyandiamide and nickel chloride hexahydrate is 1-5:0.28-0.56:1.18-2.37.

[0020] Furthermore, the Joule calcination temperature in step (6) is 500-1000° C. and the heating time is 1-10 s.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention adopts the Joule rapid heating method, uses corn stalks as raw materials, introduces nitrogen sources and nickel sources, realizes flash-speed large-scale preparation of biomass carbon-based composite materials, and realizes the virtuous cycle of "taking from carbon and using for carbon" of materials; in addition, the present invention has the characteristics of mild processing conditions, short reaction time, low energy consumption, and environmental friendliness, is suitable for mass production, and has certain application prospects. Through this research, not only can new ideas be provided for improving the preparation efficiency of biomass carbon-based materials, but also efficient electrochemical reduction and resource utilization of CO2 can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0023] Figure 1 The XRD pattern of the biomass carbon-based composite material prepared by the Joule heat method in Example 1-3;

[0024] Figure 2 This is the SEM image of the biomass carbon-based composite material prepared by the Joule heat method in Example 1;

[0025] Figure 3 The Faraday efficiency of CO and H2 of the biomass carbon-based composite materials prepared by the Joule heat method in Examples 1 and 4. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] (1) The corn stalks were ball-milled for 45 minutes, then crushed through a 200-mesh sieve, washed with deionized water at 21 kHz ultrasonic wave for 2.5 hours, filtered, and the solid was taken and dried at -45°C for 36 hours to obtain corn stalk powder; the mass ratio of the corn stalks to the deionized water was 7:12;

[0029] (2) calcining the corn straw powder at 500° C. in a nitrogen atmosphere for 5 h to obtain a corn straw carbon precursor;

[0030] (3) The corn straw carbon precursor and potassium hydroxide were mixed evenly, and the temperature was raised to 800° C. at 5° C. / min in a nitrogen atmosphere for calcination activation for 2 h to obtain intermediate A; the mass ratio of the corn straw carbon precursor to potassium hydroxide was 1:2;

[0031] (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 36 h to obtain biomass carbon powder;

[0032] (5) mixing biomass carbon powder, dicyandiamide and nickel chloride hexahydrate to obtain a mixture; the mass ratio of biomass carbon powder, dicyandiamide and nickel chloride hexahydrate is 1:0.28:1.18;

[0033] (6) The mixture was heated to 700° C. within 5 seconds and subjected to Joule calcination to obtain a biomass carbon-based composite material, namely Ni / NC-5-700.

[0034] Example 2

[0035] (1) The corn stalks were ball-milled for 45 minutes, then crushed through a 200-mesh sieve, washed with deionized water at 21 kHz ultrasonic wave for 2.5 hours, filtered, and the solid was taken and dried at -45°C for 36 hours to obtain corn stalk powder; the mass ratio of the corn stalks to the deionized water was 7:12;

[0036] (2) calcining the corn straw powder at 500° C. in a nitrogen atmosphere for 5 h to obtain a corn straw carbon precursor;

[0037] (3) The corn straw carbon precursor and potassium hydroxide were mixed evenly, and the temperature was raised to 800° C. at 5° C. / min in a nitrogen atmosphere for calcination activation for 2 h to obtain intermediate A; the mass ratio of the corn straw carbon precursor to potassium hydroxide was 1:2;

[0038] (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 36 h to obtain biomass carbon powder;

[0039] (5) mixing biomass carbon powder, dicyandiamide and nickel chloride hexahydrate to obtain a mixture; the mass ratio of biomass carbon powder, dicyandiamide and nickel chloride hexahydrate is 1:0.28:1.18;

[0040] (6) The mixture was heated to 800° C. within 5 seconds and subjected to Joule calcination to obtain a biomass carbon-based composite material, namely Ni / NC-5-800.

[0041] Example 3

[0042] (1) The corn stalks were ball-milled for 45 minutes, then crushed through a 200-mesh sieve, washed with deionized water at 21 kHz ultrasonic wave for 2.5 hours, filtered, and the solid was taken and dried at -45°C for 36 hours to obtain corn stalk powder; the mass ratio of the corn stalks to the deionized water was 7:12;

[0043] (2) calcining the corn straw powder at 500° C. in a nitrogen atmosphere for 5 h to obtain a corn straw carbon precursor;

[0044] (3) The corn straw carbon precursor and potassium hydroxide were mixed evenly, and the temperature was raised to 800° C. at 5° C. / min in a nitrogen atmosphere for calcination activation for 2 h to obtain intermediate A; the mass ratio of the corn straw carbon precursor to potassium hydroxide was 1:2;

[0045] (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 36 h to obtain biomass carbon powder;

[0046] (5) mixing biomass carbon powder, dicyandiamide and nickel chloride hexahydrate to obtain a mixture; the mass ratio of biomass carbon powder, dicyandiamide and nickel chloride hexahydrate is 1:0.28:1.18;

[0047] (6) The mixture was heated to 900° C. within 5 seconds and subjected to Joule calcination to obtain a biomass carbon-based composite material, namely Ni / NC-5-900.

[0048] Example 4

[0049] (1) The corn stalks were ball-milled for 45 minutes, then crushed through a 200-mesh sieve, washed with deionized water at 21 kHz ultrasonic wave for 2.5 hours, filtered, and the solid was taken and dried at -45°C for 36 hours to obtain corn stalk powder; the mass ratio of the corn stalks to the deionized water was 7:12;

[0050] (2) calcining the corn straw powder at 500° C. in a nitrogen atmosphere for 5 h to obtain a corn straw carbon precursor;

[0051] (3) The corn straw carbon precursor and potassium hydroxide were mixed evenly, and the temperature was raised to 800° C. at 5° C. / min in a nitrogen atmosphere for calcination activation for 2 h to obtain intermediate A; the mass ratio of the corn straw carbon precursor to potassium hydroxide was 1:2;

[0052] (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 36 h to obtain biomass carbon powder;

[0053] (5) mixing biomass carbon powder and dicyandiamide uniformly to obtain a mixture; the mass ratio of biomass carbon powder to dicyandiamide is 1:0.28;

[0054] (6) The mixture was heated to 800° C. within 5 seconds and subjected to Joule calcination to obtain a biomass carbon-based composite material, namely NC-5-800.

[0055] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing biomass carbon-based composite materials in large quantities by flash heating method, characterized in that: The method comprises the following preparation steps: (1) ball milling corn stalks for 30 to 60 minutes, then crushing through a 200-mesh sieve, ultrasonically washing with deionized water, filtering, taking solids, and freeze-drying to obtain corn stalk powder; (2) calcining the corn straw powder to obtain a corn straw carbon precursor; (3) mixing the corn stalk carbon precursor and the alkali source uniformly, and then calcining and activating them to obtain intermediate A; (4) Dispersing the intermediate A in a hydrochloric acid solution, acid washing for 2 h, washing with a 50 wt % ethanol aqueous solution until the pH of the washing solution is 7, and drying at 80° C. for 24 to 48 h to obtain biomass carbon powder; (5) mixing biomass carbon powder, dicyandiamide and nickel chloride hexahydrate to obtain a mixture; (6) The mixture is subjected to Joule calcination to obtain a biomass carbon-based composite material.

2. The method for preparing biomass carbon-based composite materials by Joule heat flash method in large quantities according to claim 1, characterized in that: The ultrasonic rate in step (1) is 21 kHz and the time is 2 to 3 hours.

3. The method for preparing biomass carbon-based composite materials by Joule heat flash method in large quantities according to claim 1, characterized in that: The freeze-drying temperature in step (1) is -45°C and the time is 24 to 48 hours.

4. The method of preparing biomass carbon-based composite materials by Joule heat flash method in large quantities according to claim 1, characterized in that: The mass ratio of the corn stalks to the deionized water in step (1) is 5-8:10-15.

5. The method of preparing biomass carbon-based composite materials in large quantities by Joule heat flash method according to claim 1, characterized in that: The calcination conditions in step (2) are as follows: nitrogen atmosphere, 500° C., and 5 h.

6. The method of preparing biomass carbon-based composite materials in large quantities by Joule heat flash method according to claim 1, characterized in that: The calcination conditions in step (3) are as follows: nitrogen atmosphere, heating rate of 5°C / min, temperature of 800°C, and time of 2h.

7. The method of preparing biomass carbon-based composite materials in large quantities by Joule heat flash method according to claim 1, characterized in that: The alkali source in step (3) is potassium hydroxide, and the mass ratio of the corn stalk carbon precursor to potassium hydroxide is 1:

2.

8. The method of preparing biomass carbon-based composite materials in large quantities by Joule heat flash method according to claim 1, characterized in that: The mass ratio of the biomass carbon powder, dicyandiamide and nickel chloride hexahydrate in step (5) is 1-5:0.28-0.56:1.18-2.

37.

9. The method of preparing biomass carbon-based composite materials in large quantities by Joule heat flash method according to claim 1, characterized in that: The Joule calcination temperature in step (6) is 500-1000° C. and the heating time is 1-10 s.

10. Use the biomass carbon-based composite material prepared by the preparation method according to any one of claims 1 to 9 for electrocatalytic CO2 reduction.