Atomic vapor chamber manufacturing method and atomic vapor chamber
By assembling atomic vapor chambers under vacuum conditions using micro-nano fabrication technology and laser bonding process, the problem of controlling the shape and size of the internal cavity of the gas chamber body has been solved, realizing the requirements for high-precision quantum instrument integration and miniaturization.
Patent Information
- Application Number
- CN202410995592.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
Existing methods for manufacturing atomic vapor chambers make it difficult to precisely control the shape and size of the chamber's internal cavity, thus failing to meet the requirements for integration and miniaturization of chip-level quantum instruments.
The components of the gas chamber body are manufactured using micro-nano fabrication technology, laser-induced etching and machining technology, and assembled under vacuum conditions using laser bonding technology to ensure the regularity of the inner cavity shape and dimensional accuracy, thereby achieving the purity of the alkali metal atomic environment.
It achieves a regular internal cavity shape, high dimensional accuracy, and excellent sealing performance, providing a stable alkali metal atomic environment, making it suitable for the integration and miniaturization of high-precision quantum instruments.
Smart Images

Figure CN118954423A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of quantum instruments, and in particular to an atomic vapor chamber manufacturing method and an atomic vapor chamber. Background Art
[0002] Atomic vapor cells are key components of quantum instruments such as atomic clocks, atomic magnetometers, and atomic gyroscopes. These quantum instruments achieve high-precision time measurement, magnetic field detection, and inertial navigation by utilizing the unique physical properties of alkali metal atoms, such as the hyperfine atomic energy level transitions caused by the hyperfine structure of the quantum state.
[0003] In order to meet the high-precision requirements of quantum instruments, the manufacture of atomic vapor cells must follow strict technical specifications to ensure that alkali metal atoms move under almost no interference conditions, thereby achieving high-precision measurement and sensing functions. These technical specifications include using a light-transmitting material that allows lasers or other light sources to penetrate the gas cell body, ensuring that the gas cell body has good airtightness so that the gas cell cavity can maintain a high vacuum state, ensuring that the gas cell body has a regular inner cavity to facilitate precise manipulation and observation of alkali metal atoms, and ensuring that the gas cell cavity can withstand temperature and pressure changes during operation.
[0004] At present, there are two main methods for manufacturing glass-based gas chamber bodies: bubble blowing and laser firing. The bubble blowing method is to heat the glass tube in a vacuum inert atmosphere, blow it into a hollow bubble-shaped cavity and then seal it. The laser firing method is to use a laser to fire a hollow glass tube in an inert atmosphere.
[0005] The atomic vapor chamber is a container used to precisely manipulate and observe alkali metal atoms. The regularity of its inner cavity shape and the precise controllability of its size are very important. However, both of the above-mentioned two manufacturing methods have the problem of difficulty in precisely controlling the shape and size of the inner cavity of the chamber body, which is not conducive to the precise manipulation and observation of alkali metal atoms and cannot meet the requirements of chip-level quantum instrument integration and miniaturization. Summary of the invention
[0006] In view of this, the purpose of an embodiment of the present invention is to provide an atomic vapor chamber manufacturing method and an atomic vapor chamber, by adopting micro-nano processing technology to accurately manufacture the inner cavity structure and the peripheral cavity of the gas chamber body, so as to solve the technical problem that it is difficult to achieve precise control of the inner cavity shape and size of the gas chamber body in the existing atomic vapor chamber manufacturing method.
[0007] In order to achieve the above purpose, the technical solutions adopted in the embodiments of the present invention are as follows:
[0008] An embodiment of the present invention provides a method for manufacturing an atomic vapor chamber, the method comprising the following steps:
[0009] Laser-induced etching technology is used to process a prefabricated through hole in the air chamber cavity on a cubic glass substrate to obtain a square barrel-shaped air chamber matrix;
[0010] Through mechanical processing technology, two glass substrates for sealing are processed into a first air chamber sealing plate and a second air chamber sealing plate; wherein the first air chamber sealing plate is used to seal one open end of the square barrel-shaped air chamber base, and the second air chamber sealing plate is used to seal the other open end;
[0011] Using a laser bonding process, the first air chamber cover plate is used to seal one end opening of the square barrel-shaped air chamber base to obtain a semi-closed square barrel-shaped air chamber base;
[0012] The semi-enclosed square barrel-shaped gas chamber substrate is moved into a vacuum chamber, a predetermined amount of alkali metal or alkali metal azide is added into the inner cavity thereof under vacuum conditions, and then a predetermined amount of inert gas is injected, and then the opening of the semi-enclosed square barrel-shaped gas chamber substrate is covered with the second gas chamber sealing plate to obtain a gas chamber body precursor structure to be bonded and sealed;
[0013] In the vacuum chamber, the gas chamber body precursor structure is fixed and sealed in a transparent vacuum mold box, and then the transparent vacuum mold box is moved into the operating chamber of the laser equipment;
[0014] The laser bonding process is adopted to bond the second gas chamber cover plate to the semi-enclosed square barrel-shaped gas chamber substrate through the transparent vacuum mold box to obtain an atomic vapor chamber.
[0015] Optionally, the material of the glass substrate used to make the square barrel-shaped air chamber base, the first air chamber covering plate, and the second air chamber covering plate is one of borosilicate glass and quartz glass.
[0016] Optionally, the steps of using laser induced etching technology to process a prefabricated through hole in the inner cavity of the air chamber on a cubic glass substrate to obtain a square barrel-shaped air chamber matrix are specifically as follows:
[0017] Using a laser device to irradiate a predetermined area of the cubic glass substrate from top to bottom, so as to form a modified area of a predetermined pattern on the cubic glass substrate;
[0018] The cubic glass substrate with the predetermined area modified is placed in the etching tank of the etching equipment, and the etching is performed for a predetermined time using a corrosive liquid to form a prefabricated through hole in the inner cavity of the air chamber that passes through the upper and lower parts on the cubic glass substrate to obtain the square barrel-shaped air chamber matrix.
[0019] Optionally, the cross-sectional shape of the prefabricated through hole in the inner cavity of the air chamber is one of a circle, a rectangle and a regular polygon.
[0020] Optionally, after the step of obtaining the square barrel-shaped air chamber matrix, the method further includes polishing the prefabricated through hole in the air chamber inner cavity of the square barrel-shaped air chamber matrix through a polishing process to control the inner wall surface roughness Ra value of the prefabricated through hole in the air chamber inner cavity to be less than or equal to 0.2 μm.
[0021] Optionally, in the step of polishing the prefabricated through hole in the inner cavity of the air chamber of the square barrel-shaped air chamber substrate by a polishing process and controlling the inner wall surface roughness Ra value of the prefabricated through hole in the inner cavity of the air chamber to be less than or equal to 0.2μm, the step also includes controlling the hole wall thickness of the prefabricated through hole in the inner cavity of the air chamber to be greater than or equal to 0.5mm.
[0022] Optionally, after the step of processing two glass substrates for sealing into a first air chamber sealing plate and a second air chamber sealing plate, the step further includes polishing the surfaces of the first air chamber sealing plate and the second air chamber sealing plate to control the surface roughness Ra value of the first air chamber sealing plate and the second air chamber sealing plate to be less than 0.2 μm.
[0023] In a second aspect, an atomic vapor chamber is also provided in an embodiment of the present invention. The atomic vapor chamber is manufactured by the aforementioned atomic vapor chamber manufacturing method.
[0024] Based on the above technical scheme, the atomic vapor chamber manufacturing method and the atomic vapor chamber in the embodiment of the present invention use laser induced etching technology and mechanical processing technology with micron-level processing accuracy to shape the components used to make the gas chamber body with micron-level precision; then the components are assembled through a laser bonding process with an alignment accuracy of less than 10 microns to obtain a gas chamber body with a highly regular inner cavity structure and a dimensional accuracy controlled at least at the micron level; wherein the addition of alkali metals and the injection of inert gases, as well as the final laser bonding and sealing of the gas chamber body are completed under vacuum conditions.
[0025] Compared with the traditional bubble blowing or laser burning method that relies on the operator's experience and skills, the atomic vapor chamber manufacturing method in the embodiment of the present invention adopts a highly controllable component processing and assembly process, and realizes the addition of alkali metals and the injection of inert gas under vacuum conditions, as well as the final laser bonding and sealing of the gas chamber body. The obtained atomic vapor chamber not only has a regular inner cavity shape and a dimensional accuracy controlled at least at the micron level, but also has excellent sealing performance, and can provide a pure alkali metal atomic environment for precise measurement based on atomic energy level transitions.
[0026] Therefore, the method for making an atomic vapor chamber in the embodiment of the present invention not only solves the technical problem that the shape and size of the inner cavity of the gas chamber body in the prior art are difficult to accurately control, but also has significant advantages in terms of sealing performance and long-term stability, as well as the purity of the alkali metal atomic environment. The atomic vapor chamber prepared by this method is very suitable for the integration and miniaturization requirements of chip-level quantum instruments, and has broad application prospects in the fields of high-precision quantum instruments such as atomic clocks, atomic magnetometers, and atomic gyroscopes. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 A schematic flow chart of a method for manufacturing an atomic vapor chamber in an embodiment of the present invention is shown;
[0029] Figure 2 A schematic structural diagram of an atomic vapor chamber in an embodiment of the present invention is shown.
[0030] The corresponding relationship between the reference numerals and component names in the figures is as follows:
[0031] An air chamber body 100 , an inner cavity 110 of the air chamber body, a square barrel-shaped air chamber base 120 , a first air chamber sealing plate 130 , and a second air chamber sealing plate 140 . DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with practical applications and with reference to the drawings of the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The atomic vapor chamber prepared by the atomic vapor chamber manufacturing method in the embodiment of the present invention is used to manufacture quantum instruments such as atomic clocks, atomic magnetometers, atomic gyroscopes, etc.
[0034] The existing atomic vapor chamber manufacturing method has the technical problem of difficulty in accurately controlling the shape and size of the inner cavity of the chamber body, which is not conducive to the precise manipulation and observation of alkali metal atoms and cannot meet the requirements of chip-level quantum instrument integration and miniaturization.
[0035] After in-depth research, the inventors found that the reason why it is difficult to accurately control the inner cavity shape and size of the gas chamber body in the existing atomic vapor chamber manufacturing method is not because the inner cavity of the gas chamber body is an internal structure and cannot be accurately processed, but because the traditional bubble blowing method and laser burning method are one-piece molding methods and mainly rely on the operator's experience and skills to control the processing accuracy.
[0036] The inventors further discovered that if the air chamber body is constructed of components, then by precisely controlling the shape and size of each component, a structure of the air chamber body with a regular inner cavity shape and high dimensional control accuracy can be obtained.
[0037] In the process of implementing the technical solution in the embodiment of the present invention, the inventors found that the laser induced etching technology can produce through holes with regular shapes and micron-level precision. If the through holes formed by the laser induced etching technology are used as the main structure of the inner cavity of the air chamber body, then two cover plates are used to seal the through holes, and an inner cavity structure with regular shapes and high dimensional control precision can be obtained. The inventors further found that the alignment accuracy of the bonding process is less than 10 microns, which can achieve high-precision and high-sealing assembly of components.
[0038] Based on the above understanding, the inventor provides a method for manufacturing an atomic vapor chamber and an atomic vapor chamber. The manufacturing method uses a laser induced etching technology with micron-level processing accuracy combined with a mechanical processing technology to manufacture a micron-level high-precision component with a fixed shape for constituting the gas chamber body, and uses a laser bonding process with an alignment accuracy of less than 10 microns to assemble the components, and realizes the addition of alkali metals or alkali metal azides and the injection of inert gas under vacuum conditions. The bonding and sealing of the gas chamber body is finally achieved under vacuum conditions to obtain an atomic vapor chamber with a regular inner cavity shape, high dimensional control accuracy, excellent sealing performance and long-term stability. The atomic vapor chamber can provide a stable and pure alkali metal atomic environment to support precise measurements based on atomic energy level transitions.
[0039] The technical solution of the present invention will be described below in conjunction with the accompanying drawings and embodiments.
[0040] Figure 1 A schematic flow chart of a method for manufacturing an atomic vapor chamber in an embodiment of the present invention is shown.
[0041] Now refer to Figure 1 As shown, an embodiment of the present invention provides a method for manufacturing an atomic vapor chamber, and the manufacturing method includes the following steps:
[0042] S110, using laser induced etching technology, a prefabricated through hole in the air chamber cavity is processed on a cubic glass substrate to obtain a square barrel-shaped air chamber base;
[0043] Before laser induced etching of a cubic glass substrate, it is usually necessary to pre-treat it. The pre-treating process can be:
[0044] A cubic glass substrate is selected and cleaned using an appropriate chemical solvent or physical method to remove impurities and stains attached to the surface; then the cleaned cubic glass substrate is inspected for air tightness to ensure that it meets the requirements.
[0045] In the embodiment of the present invention, the material of the cubic glass substrate used to make the square barrel-shaped gas chamber base is one of borosilicate glass and quartz glass.
[0046] Borosilicate glass and quartz glass have unique physical and chemical properties, such as low thermal expansion coefficient, which can maintain stable shape and size under extreme temperature conditions, and are suitable for high-precision quantum instrument manufacturing.
[0047] Borosilicate glass material has a lower thermal expansion coefficient than ordinary glass, good chemical stability and mechanical strength, and is available at a lower cost;
[0048] Quartz glass material has a low thermal expansion coefficient and high dimensional stability under temperature changes. At the same time, it also has excellent heat resistance and chemical corrosion resistance, and can withstand severe thermal shock without performance degradation, ensuring that the gas chamber body made of it can maintain dimensional stability and performance consistency under various environmental conditions. Glass substrates made of quartz glass are suitable for manufacturing atomic vapor chambers for quantum instruments with extremely high precision requirements.
[0049] In a possible implementation manner, the steps of using laser induced etching technology to process a prefabricated through hole in the inner cavity of the air chamber on a cubic glass substrate to obtain a square barrel-shaped air chamber substrate are specifically as follows:
[0050] Using a laser device to irradiate a predetermined area of the cubic glass substrate from top to bottom, so as to form a modified area of a predetermined pattern on the cubic glass substrate;
[0051] The cubic glass substrate with the predetermined area modified is placed in the etching tank of the etching equipment, and the etching is performed for a predetermined time using a corrosive liquid to form a prefabricated through hole in the inner cavity of the air chamber that passes through the upper and lower parts on the cubic glass substrate to obtain the square barrel-shaped air chamber matrix.
[0052] Accordingly, the specific implementation process of step S110 may be:
[0053] The cubic glass substrate that has passed the airtightness inspection is set at the processing position of the stage used by the laser equipment.
[0054] The pre-designed photolithography pattern of the prefabricated through hole in the inner cavity of the air chamber is imported into the control system of the laser equipment, and the scanning path is planned; the laser equipment is started, and the predetermined area of the cubic glass substrate is scanned and irradiated from top to bottom according to the preset parameters, including laser power, pulse frequency, and scanning irradiation time, to form a modified area of the predetermined pattern thereon.
[0055] The cubic glass substrate with the predetermined area modified is placed in the etching tank of the etching equipment, and the cubic glass substrate is etched for a predetermined time under the action of the corrosive liquid to form a prefabricated through hole in the inner cavity of the air chamber that passes through from top to bottom on the cubic glass substrate to obtain the square barrel-shaped air chamber matrix.
[0056] After the laser induced etching is completed, the square barrel-shaped gas chamber substrate is usually cleaned to remove impurities or residual corrosive liquid attached to the surface.
[0057] In the embodiment of the present invention, the cross-sectional shape of the prefabricated through hole in the inner cavity of the air chamber can be one of a circle, a rectangle, and a regular polygon.
[0058] The prefabricated through hole in the inner cavity of the air chamber with a circular cross-section is geometrically symmetrical, has uniform light distribution, and is easy to manufacture and process.
[0059] The prefabricated through hole in the inner cavity of the air chamber with a rectangular cross-section shape can provide a larger opening area, and the inner cavity of the air chamber body formed by the prefabricated through hole can easily achieve light control in a specific direction.
[0060] The prefabricated through hole in the inner cavity of the air chamber with a regular polygonal cross-section shape shows good balance in structure and function, and the inner cavity of the air chamber body formed thereby can achieve more uniform light distribution and control.
[0061] The air chamber inner cavity prefabricated through hole with a square cross-section shape has the characteristics of the air chamber inner cavity prefabricated through hole with a rectangular cross-section shape and the air chamber inner cavity prefabricated through hole with a regular polygonal cross-section shape, and has consistent symmetry, which can ensure the uniformity and consistency of the light path, and is conducive to the precise control of the light path in a specific direction. The inner cavity of the air chamber body formed by it can better meet the strict requirements of the atomic energy level light path for light diffusion, scattering and refraction. At the same time, the manufacturing process of the air chamber inner cavity prefabricated through hole with a square cross-section shape is relatively simple, and it is easy to achieve high-precision replication and mass production.
[0062] In order to ensure that the air chamber body assembled using the square barrel-shaped air chamber matrix has good optical properties, in a possible implementation, after the step of obtaining the square barrel-shaped air chamber matrix, it also includes polishing the prefabricated through hole in the inner cavity of the air chamber of the square barrel-shaped air chamber matrix through a polishing process, and controlling the inner wall surface roughness Ra value of the prefabricated through hole in the inner cavity of the air chamber to be less than or equal to 0.2μm.
[0063] For example, the polishing process may be mechanical polishing, chemical polishing or laser polishing. The surface roughness may be measured using a surface roughness measuring instrument, such as an atomic force microscope or a white light interferometer.
[0064] The inner wall surface roughness Ra value of the prefabricated through hole in the inner cavity of the air chamber is controlled to be less than or equal to 0.2 μm, and further, the inner wall surface roughness Ra value of the air chamber body composed of the square barrel-shaped air chamber matrix is controlled to be less than 0.2 μm.
[0065] If the surface roughness Ra value of the inner wall of the gas chamber body is no more than 0.2 μm, then its inner wall becomes a more uniform and consistent optical interface, which helps to reduce the diffusion and scattering of light in the gas chamber body, improve the clarity and stability of the optical path, and enhance the optical performance of the gas chamber body, thereby enabling the quantum instrument using the gas chamber body to achieve high-precision optical measurement.
[0066] In order to ensure that the air chamber body formed by the square barrel-shaped air chamber matrix has sufficient mechanical strength and heat shock resistance, in a possible implementation manner, in the step of polishing the air chamber inner cavity prefabricated through hole of the square barrel-shaped air chamber matrix through a polishing process, and controlling the inner wall surface roughness Ra value of the air chamber inner cavity prefabricated through hole to be less than or equal to 0.2μm, it also includes controlling the hole wall thickness of the air chamber inner cavity prefabricated through hole to be greater than or equal to 0.5mm.
[0067] The hole wall thickness of the prefabricated through hole in the inner cavity of the air chamber is controlled to be greater than or equal to 0.5 mm, and further, the wall thickness of the air chamber body formed by the square barrel-shaped air chamber matrix is greater than or equal to 0.5 mm. In practical applications, the hole wall thickness of the prefabricated through hole in the inner cavity of the air chamber is preferably about 1 mm. The hole wall thickness of the prefabricated through hole in the inner cavity of the air chamber can be specifically detected by ultrasonic measurement or other non-destructive detection technology to ensure that the wall thickness is within the specified range.
[0068] The wall thickness of the gas chamber body directly affects its ability to withstand pressure and temperature. A gas chamber body with a wall thickness of less than 0.5 mm is prone to failure under high pressure or high temperature environments; a gas chamber body with a wall thickness greater than or equal to 0.5 mm can provide the necessary mechanical strength and thermal stability to withstand the pressure and temperature during operation. A gas chamber body with a wall thickness of about 1 mm can better meet the needs of chip-level quantum instrument integration and miniaturization, and also has sufficient mechanical strength and thermal shock resistance to ensure that it can withstand the required pressure and temperature during operation.
[0069] In the embodiment of the present invention, the processing accuracy of the laser equipment is at the micron level. The prefabricated through holes in the inner cavity of the square barrel-shaped air chamber substrate obtained in step S110 have regular shapes, and the dimensional accuracy can be controlled at microns or below.
[0070] S120, processing two glass substrates for sealing into a first air chamber sealing plate and a second air chamber sealing plate by mechanical processing technology; wherein the first air chamber sealing plate is used to seal one open end of the square barrel-shaped air chamber base, and the second air chamber sealing plate is used to seal the other open end;
[0071] The specific implementation process of step S120 may be:
[0072] According to the structural size of the prefabricated through hole in the inner cavity of the air chamber, a glass substrate for sealing is selected. Usually, the thickness of the glass substrate for sealing is smaller than the thickness of the cubic glass substrate used to make the square barrel-shaped air chamber base.
[0073] The glass substrate for the cover is placed on a machining device such as a CNC milling machine or a laser cutting machine;
[0074] The mechanical processing equipment is started to process the glass substrate for sealing. After the glass substrate of the predetermined shape and size is obtained, the first air chamber sealing plate and the second air chamber sealing plate are obtained; wherein, the first air chamber sealing plate is used to seal one open end of the square barrel-shaped air chamber substrate, and the second air chamber sealing plate is used to seal the other open end; during the processing, it is necessary to ensure that the size and shape of the first air chamber sealing plate and the second air chamber sealing plate can completely cover the prefabricated through hole of the inner cavity of the air chamber.
[0075] The first air chamber cover plate and the second air chamber cover plate obtained by mechanical processing are cleaned to remove debris or impurities attached to the surface. Then, the sealing performance of the cleaned first air chamber cover plate and the second air chamber cover plate is tested to ensure that they meet the requirements.
[0076] In the embodiment of the present invention, the material of the glass substrate used to make the first gas chamber covering plate and the second gas chamber covering plate is one of borosilicate glass and quartz glass.
[0077] For the convenience and simplicity of description, the selection of borosilicate glass and quartz glass materials can refer to the relevant instructions in step S110, which will not be repeated here.
[0078] In order to make the first air chamber covering plate and the second air chamber covering plate serving as optical windows have good light transmittance, in a possible implementation manner, after the step of processing the two glass substrates for covering into the first air chamber covering plate and the second air chamber covering plate, the surface of the first air chamber covering plate and the second air chamber covering plate is polished to control the surface roughness Ra value of the first air chamber covering plate and the second air chamber covering plate to be less than 0.2 μm.
[0079] The process of polishing the surface of the first air chamber cover plate and the second air chamber cover plate may specifically be:
[0080] First, the first air chamber cover plate and the second air chamber cover plate are cleaned to remove dust, grease and processing residues remaining on the surface;
[0081] Next, according to the material properties of the first air chamber cover plate and the second air chamber cover plate, an appropriate polishing liquid and a polishing pad are selected;
[0082] Then, the first air chamber cover plate and the second air chamber cover plate are installed in a polishing machine, and polished based on the set rotation speed, pressure and polishing time to ensure that the material is removed evenly and the surface is smooth during the polishing process.
[0083] The surface roughness after polishing is detected using a surface roughness measuring instrument, such as an atomic force microscope or a white light interferometer. When the surface roughness Ra value is controlled to be less than 0.2 μm, the polishing process is completed.
[0084] Controlling the surface roughness Ra value of the first air chamber cover plate and the second air chamber cover plate to less than 0.2μm and enhancing their light transmittance can reduce the diffusion and scattering of light when it is incident, improve the transmittance of light, and improve the stability and reliability of the optical path transmission of the laser or other light source in the inner cavity of the air chamber body, so as to meet the high standard requirements of the atomic energy level optical path for light quality. In the range of surface roughness Ra value less than 0.2μm, 0.02~0.16μm is the preferred range. The surface roughness Ra value of 0.02~0.16μm can enhance the light transmittance of the first air chamber cover plate and the second air chamber cover plate as optical windows, and greatly reduce the volume of the air chamber body while ensuring the optical performance.
[0085] S130, using a laser bonding process to seal one end opening of the square barrel-shaped air chamber base with the first air chamber cover plate to obtain a semi-closed square barrel-shaped air chamber base;
[0086] The specific implementation process of step S130 may be:
[0087] Marking alignment points on the first air chamber cover plate and the square barrel-shaped air chamber substrate that have been cleaned;
[0088] Based on the marked alignment points, a precise alignment system, such as an optical alignment system, is used to align the first gas chamber cover plate and the square barrel-shaped gas chamber substrate. The alignment accuracy of the alignment system used in the existing bonding process is less than 10 microns.
[0089] The laser bonding equipment is used to emit a laser beam to scan the bonding area of the two materials, so that the materials are partially melted and bonded together to obtain the semi-enclosed square barrel-shaped air chamber matrix. In the laser bonding process, it is necessary to accurately control the laser parameters, such as laser energy and scanning speed.
[0090] After the bonding is completed, the semi-enclosed square barrel-shaped air chamber substrate needs to be cleaned.
[0091] Through step S130, the first air chamber covering plate is assembled with the square barrel-shaped air chamber base in a highly airtight manner, so that one end opening of the square barrel-shaped air chamber base is sealed with the first air chamber covering plate in a highly airtight manner to obtain a semi-closed square barrel-shaped air chamber base.
[0092] S140, moving the semi-enclosed square barrel-shaped gas chamber substrate into a vacuum chamber, adding a predetermined amount of alkali metal or alkali metal azide into its inner cavity under vacuum conditions, then injecting a predetermined amount of inert gas, and then covering the opening of the semi-enclosed square barrel-shaped gas chamber substrate with the second gas chamber sealing plate to obtain a gas chamber body precursor structure to be bonded and sealed;
[0093] The specific implementation process of step S140 may be:
[0094] The cleaned semi-enclosed square barrel-shaped air chamber base and the second air chamber cover plate are moved into the vacuum chamber and stably placed; at the same time, a transparent vacuum mold box is also moved in, and the inner cavity of the transparent vacuum mold box can fix the combination of the square barrel-shaped air chamber base and the second air chamber cover plate;
[0095] Start the vacuum pump and gradually reduce the pressure in the vacuum chamber until the predetermined vacuum degree is reached;
[0096] Under vacuum conditions, a predetermined amount of alkali metal or alkali metal azide is added into the inner cavity of the semi-enclosed square barrel-shaped gas chamber substrate through a suitable special feeding device;
[0097] Using an inert gas injection system or device, inject a predetermined amount of inert gas, such as argon or nitrogen, into the inner cavity of the semi-enclosed square barrel-shaped gas chamber substrate into which a predetermined amount of alkali metal or alkali metal azide is added;
[0098] Align the second air chamber cover plate with the opening of the square barrel-shaped air chamber base, cover it carefully, and ensure good sealing to form the air chamber body precursor structure to be bonded and sealed.
[0099] In the embodiment of the present invention, for example, the alkali metal azide can be sodium azide (NaN 3 ), potassium azide (KN 3 ), rubidium azide (RbN 3), cesium azide (CsN 3 ).
[0100] S150, in the vacuum chamber, fixing and sealing the gas chamber body precursor structure in a transparent vacuum mold box, and then moving the transparent vacuum mold box into the operating chamber of the laser equipment;
[0101] The specific implementation process of step S150 may be:
[0102] The air chamber body precursor structure is fixed and sealed in a transparent vacuum mold box, and then the lid of the transparent vacuum mold box is closed and sealed using a sealing device;
[0103] Open the vacuum chamber, take out the sealed transparent vacuum mold box from the vacuum chamber, and clean it;
[0104] Move the transparent vacuum mold box into the operating chamber of the laser equipment, making sure it is firmly placed.
[0105] S160, using a laser bonding process, through the transparent vacuum mold box, the second gas chamber cover plate is bonded to the semi-enclosed square barrel-shaped gas chamber substrate to obtain an atomic vapor chamber.
[0106] The specific implementation process of step S160 may be:
[0107] Check the settings and parameters of the laser equipment to ensure they meet the process requirements;
[0108] The laser device is started to emit a laser beam, which penetrates the transparent vacuum mold box and scans and irradiates the bonding area between the second gas chamber cover plate and the semi-enclosed square barrel-shaped gas chamber substrate, so that the materials are partially melted and bonded together to obtain an atomic vapor chamber. In the laser bonding process, it is necessary to accurately control laser parameters such as laser energy and scanning speed.
[0109] In the embodiment of the present invention, the addition of alkali metal or alkali metal azide and the precise control of inert gas injection are sequentially implemented under vacuum conditions through steps S140, S150, and S160, so as to realize the transfer of the precursor structure of the gas chamber body to be bonded and sealed, realize the final laser bonding and sealing of the gas chamber body, and obtain an atomic vapor chamber with good airtightness and a pure alkali metal atomic environment. The atomic vapor chamber can meet the strict requirements of the atomic energy level optical path for light diffusion, scattering and refraction, is conducive to the precise control and observation of alkali metal atoms, and is very suitable for the integration and miniaturization requirements of chip-level quantum instruments.
[0110] It can be seen that the atomic vapor chamber manufacturing method in the embodiment of the present invention uses laser induced etching technology and mechanical processing technology with micron-level processing accuracy to shape the components used to manufacture the gas chamber body with micron-level precision; then the components are assembled through a laser bonding process with an alignment accuracy of less than 10 microns to obtain a gas chamber body with a highly regular inner cavity structure and a dimensional accuracy controlled at least in the micron level; wherein, the addition of alkali metals and the injection of inert gases, as well as the final laser bonding and sealing of the gas chamber body are completed under vacuum conditions.
[0111] Compared with the traditional bubble blowing or laser burning method that relies on the operator's experience and skills, the atomic vapor chamber manufacturing method in the embodiment of the present invention adopts a highly controllable component processing and assembly process, and realizes the addition of alkali metals and the injection of inert gas under vacuum conditions, as well as the final laser bonding and sealing of the gas chamber body. The obtained atomic vapor chamber not only has a regular inner cavity shape and a dimensional accuracy controlled at least at the micron level, but also has excellent sealing performance, and can provide a pure alkali metal atomic environment for precise measurement based on atomic energy level transitions.
[0112] Therefore, the method for making an atomic vapor chamber in the embodiment of the present invention not only solves the technical problem that the shape and size of the inner cavity of the gas chamber body in the prior art are difficult to accurately control, but also has significant advantages in terms of sealing performance and long-term stability, as well as the purity of the alkali metal atomic environment. The atomic vapor chamber prepared by this method is very suitable for the integration and miniaturization requirements of chip-level quantum instruments, and has broad application prospects in the fields of high-precision quantum instruments such as atomic clocks, atomic magnetometers, and atomic gyroscopes.
[0113] Figure 2 A schematic structural diagram of an atomic vapor chamber in an embodiment of the present invention is shown.
[0114] Now refer to Figure 2 As shown, an atomic vapor chamber is also provided in an embodiment of the present invention. The atomic vapor chamber is manufactured by the aforementioned atomic vapor chamber manufacturing method.
[0115] The atomic vapor chamber comprises a chamber body 100 and an alkali metal or alkali metal azide and an inert gas filled in an inner cavity 110 of the chamber body; the chamber body 100 comprises:
[0116] A hollow square barrel-shaped air chamber base 120;
[0117] A first air chamber cover plate 130, used for sealing an opening at one end of the square barrel-shaped air chamber base 120;
[0118] The second air chamber cover plate 140 is used to seal the other end opening of the square barrel-shaped air chamber base 120 .
[0119] The alkali atomic vapor cell in the embodiment of the present invention is used to manufacture quantum instruments such as atomic clocks, atomic magnetometers, atomic gyroscopes, etc.
[0120] It should be understood that the atomic vapor chamber in the atomic vapor chamber embodiment of the present invention is an atomic vapor chamber prepared by the manufacturing method in the aforementioned atomic vapor chamber manufacturing method embodiment of the present invention. For the convenience and brevity of description, the atomic vapor chamber manufacturing method and material selection in the atomic vapor chamber embodiment of the present invention can refer to the relevant description in the manufacturing method embodiment, and will not be repeated here.
Claims
1. A method for manufacturing an atomic vapor chamber, characterized in that: The production method comprises the following steps: Laser-induced etching technology is used to process a prefabricated through hole in the air chamber cavity on a cubic glass substrate to obtain a square barrel-shaped air chamber matrix; Through mechanical processing technology, two glass substrates for sealing are processed into a first air chamber sealing plate and a second air chamber sealing plate; wherein the first air chamber sealing plate is used to seal one open end of the square barrel-shaped air chamber base, and the second air chamber sealing plate is used to seal the other open end; Using a laser bonding process, the first air chamber cover plate is used to seal one end opening of the square barrel-shaped air chamber base to obtain a semi-closed square barrel-shaped air chamber base; The semi-enclosed square barrel-shaped gas chamber substrate is moved into a vacuum chamber, a predetermined amount of alkali metal or alkali metal azide is added into the inner cavity thereof under vacuum conditions, and then a predetermined amount of inert gas is injected, and then the opening of the semi-enclosed square barrel-shaped gas chamber substrate is covered with the second gas chamber sealing plate to obtain a gas chamber body precursor structure to be bonded and sealed; In the vacuum chamber, the gas chamber body precursor structure is fixed and sealed in a transparent vacuum mold box, and then the transparent vacuum mold box is moved into the operating chamber of the laser equipment; The laser bonding process is adopted to bond the second gas chamber cover plate to the semi-enclosed square barrel-shaped gas chamber substrate through the transparent vacuum mold box to obtain an atomic vapor chamber.
2. The method for manufacturing an atomic vapor chamber according to claim 1, characterized in that: The material of the glass substrate used to make the square barrel-shaped gas chamber base, the first gas chamber cover plate, and the second gas chamber cover plate is one of borosilicate glass and quartz glass.
3. The method for manufacturing an atomic vapor chamber according to claim 1, characterized in that: The steps of machining a prefabricated through hole in the air chamber cavity on a cubic glass substrate using laser induced etching technology to obtain a square barrel-shaped air chamber matrix are as follows: Using a laser device to irradiate a predetermined area of the cubic glass substrate from top to bottom, so as to form a modified area of a predetermined pattern on the cubic glass substrate; The cubic glass substrate with the predetermined area modified is placed in the etching tank of the etching equipment, and the etching is performed for a predetermined time using a corrosive liquid to form a prefabricated through hole in the inner cavity of the air chamber that passes through the upper and lower parts on the cubic glass substrate to obtain the square barrel-shaped air chamber matrix.
4. The method for manufacturing an atomic vapor chamber according to claim 1, characterized in that: The cross-sectional shape of the prefabricated through hole in the inner cavity of the air chamber is one of a circle, a rectangle and a regular polygon.
5. The method for manufacturing an atomic vapor chamber according to any one of claims 1 to 4, characterized in that: After the step of obtaining the square barrel-shaped air chamber matrix, the method further includes polishing the prefabricated through hole in the air chamber inner cavity of the square barrel-shaped air chamber matrix through a polishing process to control the inner wall surface roughness Ra value of the prefabricated through hole in the air chamber inner cavity to be less than or equal to 0.2 μm.
6. The method for manufacturing an atomic vapor chamber according to claim 5, characterized in that: The step of polishing the prefabricated through hole in the inner cavity of the square barrel-shaped air chamber substrate by a polishing process to control the inner wall surface roughness Ra value of the prefabricated through hole in the inner cavity of the air chamber to be less than or equal to 0.2μm also includes controlling the hole wall thickness of the prefabricated through hole in the inner cavity of the air chamber to be greater than or equal to 0.5mm.
7. The method for manufacturing an atomic vapor chamber according to any one of claims 1 to 4, characterized in that: After the step of processing the two glass substrates for sealing into the first air chamber sealing plate and the second air chamber sealing plate, it also includes polishing the surface of the first air chamber sealing plate and the second air chamber sealing plate to control the surface roughness Ra value of the first air chamber sealing plate and the second air chamber sealing plate to less than 0.2μm.
8. Atomic vapor chamber, characterized in that The atomic vapor chamber is manufactured by the atomic vapor chamber manufacturing method according to any one of claims 1 to 7.