Method for preparing vanadium pentoxide through sodium salt roasting
By using airflow suspension heat exchange device and high-pressure pulse processing technology in the sodium calcination process, the problems of long calcination time of the rotary kiln and low separation efficiency of vanadium and chromium are solved, and efficient preparation and low-cost production of vanadium pentoxide are achieved.
Patent Information
- Application Number
- CN202411011594.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing sodium-calcination calcination process, the rotary kiln has a long calcination time, high energy consumption, high production costs, and low separation efficiency of vanadium and chromium, which affects the yield and quality of vanadium pentoxide.
The airflow suspension heat exchange device is used for preheating and sodium calcination, combined with rod grinding and vanadium sinking treatment, and high-pressure pulse treatment technology is used to separate vanadium and chromium, shorten the vanadium sinking time and improve the recovery rate.
It shortens the calcination time, reduces production costs, improves the recovery rate of vanadium and chromium and the output of vanadium pentoxide, and improves the energy utilization rate and the recycling efficiency of chromium resources.
Smart Images

Figure CN118954590A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling of vanadium secondary resources, and more specifically, the invention relates to a method for preparing vanadium pentoxide by sodium roasting. Background Art
[0002] At present, the main process for preparing vanadium pentoxide is to mix the secondary vanadium resources obtained from smelting steel with vanadium-titanium magnetite with other raw materials, and then carry out sodium roasting, leaching, and silicon removal, and then convert the multivalent vanadium and chromium into pentavalent vanadium salt and hexavalent chromium solution, the main components of which are sodium orthovanadate and sodium chromate, with the chemical formula of Na3VO4 and Na2CrO4, and the molar ratio of vanadium to chromium in the solution is 1.3-2.2, and then acidification precipitation of vanadium, alkali dissolution and impurity removal, filtration and washing, and sodium roasting are used to obtain vanadium pentoxide. Among them, sodium roasting mainly adopts rotary kiln equipment, but there are problems such as the inner wall of the furnace body sticking and the inner wall diameter of the cylinder body becoming smaller, resulting in long calcination time, high energy consumption, low output, and increased production cost. At present, steel belt furnace calcination is also used, which is convenient for controlling the time and temperature, but the calcination temperature is too high, the steel belt loss is large, and the steel belt transmission is used, and the material loss is large. Therefore, how to solve the problems of rotary kiln calcination time and calcination efficiency in the prior art has become a difficult problem that needs to be solved urgently in this technical field. In addition, it is also of great significance to study how to separate vanadium and chromium in the solution during vanadium precipitation, improve the vanadium precipitation rate, and shorten the vanadium precipitation time. Summary of the invention
[0003] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0004] In order to achieve these objects and other advantages of the present invention, a method for preparing vanadium pentoxide by sodium roasting is provided, comprising the following steps:
[0005] Step 1: grind the vanadium slag, mix it evenly with the dried return slag, chromium secondary resources and soda ash to obtain raw material, send the raw material to an air suspension heat exchange device for preheating, and then send it to a rotary kiln for sodium roasting to obtain clinker;
[0006] Step 2, the clinker is mixed with pure water, rod milled for leaching, impurity remover is added, heat preservation and aging are carried out, and solid-liquid separation is carried out to obtain vanadium-chromium-rich leaching solution and returned slag, and the returned slag is dried and then used for mixing with vanadium slag in step 1;
[0007] Step 3, adding a vanadium precipitation agent to the vanadium-rich chromium leaching solution, adjusting the pH, stirring evenly, standing and stratifying, to obtain a chromium-rich clear solution and a vanadium-rich turbid solution, wherein the chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium and is used for chromium salt production, and the vanadium-rich turbid solution is filtered and washed to obtain a red cake;
[0008] Step 4: drying and roasting the red cake to obtain vanadium pentoxide.
[0009] Preferably, in the step 1, the vanadium slag is crushed and ground to 200-300 meshes.
[0010] Preferably, in step 1, in the raw meal, the total vanadium content is 5-15% by mass of V2O5, and the total chromium content is 10-15% by mass of Cr2O3; the mass ratio of soda ash to the total vanadium in the raw meal is 1.8-2.1:1.
[0011] Preferably, in step 1, the raw material is fed into an air suspension heat exchange device and preheated to a temperature of 280-350° C. and a water content of ≤8%; the sodium roasting temperature is 800-900° C. and the time is 3-5 hours.
[0012] Preferably, in the step 2, the mass ratio of clinker to pure water is 5-8:7-10; the rod mill leaching temperature is 90-100° C. for 1-2 h; and the heat preservation aging is carried out at 50-120° C. for 7-10 h.
[0013] Preferably, in step 2, the impurity remover is one or more of sodium aluminate, magnesium chloride, magnesium sulfate and aluminum sulfate, and the mass ratio of the impurity remover to the total vanadium is 1:5 to 6.5.
[0014] Preferably, in step 3, the vanadium precipitation agent is one or more of ammonium sulfate, ammonium chloride and ammonium bisulfate; NH4 + The molar ratio of V to vanadium in the chromium-rich leaching solution is 1:2-4.
[0015] Preferably, in step three, the pH is adjusted to 3.2-4.0 using a sulfuric acid solution having a volume fraction of 70-90%; and the standing time is 2.5-3.5 hours.
[0016] Preferably, in step 4, the drying is performed at 250-300° C. until the moisture content is 3-5%; the roasting temperature is 750-850° C., and the roasting time is 60-90 min.
[0017] Preferably, the airflow suspension heat exchange device comprises: a support frame, a reactor, an air duct connecting pipe, a reactor discharge pipe, a counterweight discharge valve, a discharge pipe and an air inlet;
[0018] The reactor comprises a primary reactor, a secondary reactor and a tertiary reactor, and the reactors of each stage are staggeredly distributed on the support frame; the reactor feed pipes are arranged below the primary reactor and the secondary reactor, and the discharge pipe is arranged below the tertiary reactor; every two adjacent reactors are connected in series through an air duct connecting pipe, and the air duct connecting pipe is connected and penetrated with the reactor feed pipe above, and a counterweight discharge valve is arranged in the middle; the air inlet is arranged below the air duct connecting pipe.
[0019] Preferably, the step three is replaced by: adding ammonium chloride, ammonium sulfate and PEG400 to ethanol, ultrasonically dispersing at 300-600W and 50-70khz for 20-40min, heating to 80-90°C to completely volatilize the ethanol, and obtaining a vanadium precipitator; adding the vanadium precipitator to the vanadium-rich chromium leaching solution, adjusting the pH to 3.0-4.0 with a sulfuric acid solution with a volume fraction of 80%, subjecting the reaction solution to a high-voltage pulse treatment, standing for 1-2h to separate layers, and obtaining a chromium-rich clear solution and The vanadium-rich turbid solution and the chromium-rich clear solution are sodium dichromate solutions containing hexavalent chromium, which are used for chromium salt production. The vanadium-rich turbid solution is filtered and washed to obtain a red cake. Among them, the specific parameters of the high-voltage pulse treatment are: pulse width 1 to 5 μs, pulse frequency 100 to 500 Hz, electric field strength 10 to 30 kV / cm, pulse number 5 to 10; the mass volume ratio of ammonium chloride, ammonium sulfate, PEG400 and ethanol is 1g: 0.2 to 1g: 0.1 to 0.5g: 40 to 100 mL.
[0020] The present invention has at least the following beneficial effects:
[0021] (1) The traditional sodium roasting-water leaching process for vanadium and chromium has the problems of long calcination time and high cost. The present invention adopts an air flow suspension heat exchange device to increase the initial temperature of the sodium roasting of the material, so that the redox reaction is more complete, the calcination effect is good, and the calcination time is short; at the same time, the method of the present invention can shorten the aspect ratio of the rotary kiln from the traditional 20 to 30:1 to 15 to 18:1, thereby reducing the area occupied by the process equipment and the fixed asset investment, and reducing the production cost;
[0022] (2) The present invention utilizes the waste heat tail gas generated by the rotary kiln to preheat the material, recover the waste heat, improve the energy utilization rate, and reduce the tail gas temperature; in the present invention, the chromium resources after the vanadium and chromium separation are returned to the chromium salt production system, the chromium resources are recovered, and the treatment cost of chromium-containing wastewater is reduced;
[0023] (3) The process for preparing vanadium pentoxide according to the present invention is short, the production cost is low, and the recovery rate of vanadium and chromium is high.
[0024] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a process flow chart of the present invention;
[0026] Figure 2 It is a schematic structural diagram of the airflow suspension heat exchange device of the present invention. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0028] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0029] The process of the present invention is as follows Figure 1 shown.
[0030] The structural schematic diagram of the air flow suspension heat exchange device of the present invention is as follows Figure 2 As shown, it includes: a support frame 1, a reactor 2, an air duct connecting pipe 3, a reactor feed pipe 4, a counterweight discharge valve 5, a discharge pipe 6 and an air inlet 7, wherein the reactor 2 includes a primary reactor 201, a secondary reactor 202, and a tertiary reactor 203; the primary reactor 201, the secondary reactor 202 and the tertiary reactor 203 are staggered on the support frame 1 from top to bottom; the reactor feed pipe 4 is arranged below the primary reactor 201 and the secondary reactor 202; the discharge pipe is arranged below the tertiary reactor 203, and the discharge pipe is connected to the rotary kiln to discharge the preheated raw material into the rotary kiln; each adjacent two reactors are connected in series through the air duct connecting pipe 3, and the air duct connecting pipe 3 is connected and connected to the upper reactor feed pipe 4, and a counterweight discharge valve 5 is arranged in the middle for connecting or closing; the air inlet 7 is arranged below the air duct connecting pipe 3, and the rotary kiln tail gas enters the air duct connecting pipe 3 through the air inlet 7.
[0031] When in use, the tail gas of the rotary kiln first enters the tertiary reactor 203 through the air inlet 7, and is transported from bottom to top to the secondary reactor 202 and the primary reactor 203 by the air duct connecting pipe 3 under the action of negative pressure. At the same time, the raw material is transported to the feed port of the air flow suspension heat exchange device through the elevator and enters the primary reactor 201. The raw material and the tail gas are heat exchanged in the primary reactor 201, and then the raw material falls from the reactor discharge pipe 4 onto the counterweight discharge valve 5. The counterweight discharge valve 5 exceeds the load-bearing material range, and the counterweight discharge valve 5 opens and starts to discharge. The raw material is brought into the adjacent secondary reactor 202 by the tail gas flow, and so on. The raw material enters each level of the reactor from top to bottom in turn and exchanges heat with the tail gas to achieve preheating. After the preheating of the raw material is completed, the raw material is discharged into the rotary kiln from the discharge pipe 6.
[0032] The initial temperature of the raw material entering the air suspension heat exchange device is 18-30°C and the water content is 8-15%. The initial temperature of the tail gas discharged into the air suspension heat exchange device is 400-650°C. The heat exchange time in the reactor is 40-60 minutes, so that the temperature of the raw material rises to 280-350°C and the water content is ≤8%.
[0033] Example 1
[0034] A method for preparing vanadium pentoxide by sodium roasting comprises the following steps:
[0035] Step 1: grind the vanadium slag to 220 mesh, and then mix it with the dried return slag, chromium secondary resources and soda ash to obtain raw material, send the raw material to an air suspension heat exchange device for preheating to 300°C and a water content of 6%, and then send it to a rotary kiln for sodium roasting at 870°C for 4.5 hours to obtain clinker; wherein the total vanadium content in the raw material is 10.55% by mass of V2O5, the total chromium content is 12.0% by mass of Cr2O3, and the mass ratio of soda ash to total vanadium is 2:1;
[0036] Step 2, the clinker and pure water are mixed in a mass ratio of 5:7, and the mixture is leached in a rod mill at 92°C for 1.5h, sodium aluminate is added, and the mixture is kept warm at 80°C for 8.5h, and the solid-liquid separation is performed to obtain a vanadium-rich chromium leaching solution and a return slag, and the return slag is dried and mixed with the vanadium slag in step 1, and the vanadium leaching rate is measured to be 90.93%, and the chromium leaching rate is 65.4%; wherein the mass ratio of sodium aluminate to total vanadium is 1:6;
[0037] Step 3: add ammonium sulfate, a vanadium precipitant, to the vanadium-rich chromium leaching solution, adjust the pH to 3.5 with a sulfuric acid solution with a volume fraction of 80%, stir evenly, let stand for 3 hours to separate, and obtain a chromium-rich clear solution and a vanadium-rich turbid solution. The chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium, which is used for chromium salt production. The vanadium-rich turbid solution is filtered and washed to obtain a red cake; wherein, NH4 + The molar ratio of V to that in the vanadium-rich chromium leaching solution is 1:3;
[0038] Step 4: Dry the red cake at 250° C. to a moisture content of 5%, and calcine at 800° C. for 75 min to obtain vanadium pentoxide.
[0039] Example 2
[0040] A method for preparing vanadium pentoxide by sodium roasting comprises the following steps:
[0041] Step 1: Grind the vanadium slag to 280 mesh, and then mix it evenly with the dried return slag, chromium secondary resources, and soda ash to obtain raw material, send the raw material into an air suspension heat exchange device for preheating to 350°C and a water content of 5%, and then send it to a rotary kiln for sodium roasting at 900°C for 4 hours to obtain clinker; wherein the total vanadium content in the raw material is 8.95% by mass of V2O5, the total chromium content is 11.92% by mass of Cr2O3, and the mass ratio of soda ash to total vanadium is 2:1;
[0042] Step 2, the clinker and pure water are mixed in a mass ratio of 6:8, and the mixture is leached in a rod mill at 95°C for 1.8h, aluminum sulfate is added, and the mixture is kept warm at 85°C for 8.5h, and the solid-liquid separation is performed to obtain a vanadium-rich chromium leaching solution and a return slag, and the return slag is dried and mixed with the vanadium slag in step 1, and the vanadium leaching rate is measured to be 95.2%, and the chromium leaching rate is 76.35%; wherein the mass ratio of aluminum sulfate to total vanadium is 1:5;
[0043] Step 3: add ammonium chloride, a vanadium precipitation agent, to the vanadium-rich chromium leaching solution, adjust the pH to 3.5 with a sulfuric acid solution with a volume fraction of 80%, stir evenly, stand for 3 hours to separate the layers, and obtain a chromium-rich clear solution and a vanadium-rich turbid solution. The chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium, which is used for chromium salt production. The vanadium-rich turbid solution is filtered and washed to obtain a red cake, and the vanadium precipitation rate is measured to be 97.25%; wherein, NH4 + The molar ratio of V to that in the vanadium-rich chromium leaching solution is 1:3.5;
[0044] Step 4: Dry the red cake at 300° C. to a moisture content of 3%, and calcine at 820° C. for 85 min to obtain vanadium pentoxide.
[0045] Example 3
[0046] In this embodiment, the step three is replaced by: adding ammonium chloride, a vanadium precipitation agent, to the vanadium-rich chromium leaching solution, adjusting the pH to 3.5 with a sulfuric acid solution having a volume fraction of 80%, subjecting the reaction solution to high-voltage pulse treatment, standing for 1.5 hours to separate layers, obtaining a chromium-rich clear solution and a vanadium-rich turbid solution, wherein the chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium, which is used for chromium salt production, and the vanadium-rich turbid solution is filtered and washed to obtain a red cake, and the vanadium precipitation rate is measured to be 99.06%; wherein the pulse width is 3 μs, the pulse frequency is 200 Hz, the electric field strength is 20 V / cm, and the number of pulses is 8. The remaining steps are the same as those in Example 2.
[0047] Example 4
[0048] In this embodiment, the step three is replaced by: adding ammonium chloride, ammonium sulfate and PEG400 to ethanol, ultrasonically dispersing at 400W and 60khz for 30min, heating to 80°C to completely volatilize the ethanol, and obtaining a vanadium precipitator; adding the vanadium precipitator to the vanadium-rich chromium leaching solution, adjusting the pH to 3.5 with a sulfuric acid solution having a volume fraction of 80%, subjecting the reaction solution to high-voltage pulse treatment, standing for 1.5h to separate layers, obtaining a chromium-rich clear solution and a vanadium-rich turbid solution, wherein the chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium, which is used for chromium salt production, and the vanadium-rich turbid solution is filtered and washed to obtain a red cake, and the vanadium precipitation rate is measured to be 99.83%; wherein the pulse width is 3μs, the pulse frequency is 200Hz, the electric field strength is 20kV / cm, and the pulse number is 8; the mass volume ratio of ammonium chloride, ammonium sulfate, PEG400 and ethanol is 1g:0.5g:0.2g:50mL. The remaining steps are the same as in Example 2.
[0049] In the vanadium precipitation process of Examples 3 to 4, the reaction solution is subjected to high-pressure pulse treatment, which is beneficial to the vanadium precipitation reaction, effectively shortens the reaction time, and makes the reaction between ammonium and vanadium more thorough, resulting in a higher vanadium precipitation rate, further shortening the time for preparing vanadium pentoxide; secondly, in Example 4, the vanadium precipitation agent is modified, and the prepared vanadium precipitation agent has better vanadium precipitation effect and a higher vanadium precipitation rate.
[0050] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for preparing vanadium pentoxide by sodium roasting, characterized in that: The following steps are involved: Step 1: grind the vanadium slag, mix it evenly with the dried return slag, chromium secondary resources and soda ash to obtain raw material, send the raw material to an air suspension heat exchange device for preheating, and then send it to a rotary kiln for sodium roasting to obtain clinker; Step 2, the clinker is mixed with pure water, rod milled for leaching, impurity remover is added, heat preservation and aging are carried out, and solid-liquid separation is carried out to obtain vanadium-chromium-rich leaching solution and returned slag, and the returned slag is dried and then used for mixing with vanadium slag in step 1; Step 3, adding a vanadium precipitation agent to the vanadium-rich chromium leaching solution, adjusting the pH, stirring evenly, standing and stratifying, to obtain a chromium-rich clear solution and a vanadium-rich turbid solution, wherein the chromium-rich clear solution is a sodium dichromate solution containing hexavalent chromium and is used for chromium salt production, and the vanadium-rich turbid solution is filtered and washed to obtain a red cake; Step 4: drying and roasting the red cake to obtain vanadium pentoxide.
2. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 1, the vanadium slag is crushed and ground into 200-300 meshes.
3. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 1, the total vanadium content in the raw material is 5-15% by mass of V2O5, and the total chromium content is 10-15% by mass of Cr2O3; the mass ratio of soda ash to the total vanadium in the raw material is 1.8-2.1:
1.
4. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 1, the raw material is fed into an air suspension heat exchange device and preheated to a temperature of 280-350° C. and a water content of ≤8%; the sodium roasting temperature is 800-900° C. and the time is 3-5 hours.
5. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 2, the mass ratio of clinker to pure water is 5-8:7-10; the rod mill leaching temperature is 90-100° C., and the time is 1-2 hours; and the heat preservation aging is carried out at 50-120° C. for 7-10 hours.
6. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 2, the impurity remover is one or more of sodium aluminate, magnesium chloride, magnesium sulfate and aluminum sulfate, and the mass ratio of the impurity remover to the total vanadium is 1:5 to 6.
5.
7. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 3, the vanadium precipitation agent is one or more of ammonium sulfate, ammonium chloride and ammonium bisulfate; NH4 + The molar ratio of V to that in the vanadium-rich chromium leaching solution is 1:2-4.
8. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step three, the pH is adjusted to 3.2 to 4.0 using a sulfuric acid solution having a volume fraction of 70 to 90%; and the standing time is 2.5 to 3.5 hours.
9. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: In the step 4, the drying is performed at 250-300° C. until the moisture content is 3-5%. The roasting temperature is 750-850° C., and the roasting time is 60-90 minutes.
10. The method for preparing vanadium pentoxide by sodium roasting as claimed in claim 1, characterized in that: The airflow suspension heat exchange device comprises: a support frame, a reactor, an air duct connecting pipe, a reactor discharge pipe, a counterweight discharge valve, a discharge pipe and an air inlet; The reactor comprises a primary reactor, a secondary reactor and a tertiary reactor, and the reactors of each stage are staggeredly distributed on the support frame; the reactor feed pipes are arranged below the primary reactor and the secondary reactor, and the discharge pipe is arranged below the tertiary reactor; every two adjacent reactors are connected in series through an air duct connecting pipe, and the air duct connecting pipe is connected and penetrated with the reactor feed pipe above, and a counterweight discharge valve is arranged in the middle; the air inlet is arranged below the air duct connecting pipe.