One-dimensional Li1.2 [Mn0. 54Ni0. 13Co0. 13] O2 ternary positive electrode material as well as preparation method and application thereof
By preparing one-dimensional Li1.2 [Mn0.54Ni0.13Co0.13]O2 ternary positive electrode material, the ratio of lithium-rich manganese-based material is solved by using one-dimensional precursor template and liquid phase complexing method, combined with low-temperature and high-temperature sintering technology. The problems of poor performance and low Coulomb efficiency have achieved a high energy density lithium-ion battery positive electrode material.
Patent Information
- Application Number
- CN202411013642.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Lithium-rich manganese-based positive electrode materials face problems such as poor rate performance, low first-time Coulomb efficiency and voltage platform attenuation, which limits their application in high-energy density lithium-ion batteries.
The preparation method of one-dimensional Li1.2 [Mn0.54Ni0.13Co0.13]O2 ternary positive electrode material is adopted, and Mn, Co, Ni is uniformly bound in an alkaline environment through one-dimensional precursor template method and liquid phase complexing method. A combination of ionic, low-temperature sintering and high-temperature sintering produces materials with graded dielectric structures and rich structural defects, improving electrochemical activity and conductivity.
The rate performance and cycle stability of lithium-rich manganese-based materials are significantly improved, the lithium ion transmission dynamics are enhanced, and the energy storage advantages of high energy density are achieved, solving the problems of poor rate performance and low Coulomb efficiency for the first time.
Smart Images

Figure CN118954623A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of design and preparation of lithium ion battery electrode materials, and particularly relates to a one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material and its preparation method and application. Background Art
[0002] As a green and high-energy portable energy storage technology, lithium-ion batteries are a powerful driving force for the rapid development of multiple industrial fields such as electronic devices, mobile communications, and electric transportation. However, the ever-increasing industrial demand has put forward almost harsh requirements and challenges for energy storage systems. The development of lithium-ion battery technology with high energy and high power density has always been the focus and difficulty of common concern in academia and industry at home and abroad. As we all know, electrode materials are the most critical factor restricting the electrochemical performance of lithium-ion batteries, especially positive electrode materials. The manufacturing technology based on precision manufacturing to reduce the proportion of inactive substances in electrode materials to increase battery energy density has reached its limit. At the same time, the capacity potential of current commercial positive electrode materials has also approached the theoretical limit, which makes the development of positive electrode materials with high energy and high power density imminent.
[0003] At present, commercial power battery positive electrode materials mainly include two categories: lithium iron phosphate and ternary positive electrode. Lithium iron phosphate has higher safety and cycle life, but the energy density is too low (~160Wh / kg). In comparison, the ternary positive electrode can provide a higher energy density (230~260Wh / kg). However, the current high-nickel ternary development route is at the expense of material safety, rate performance and cycle life. Even in exchange for a higher capacity, it still cannot meet the increasingly demanding application requirements (>400Wh / kg). Therefore, it is urgent to carry out research on alternative high-capacity positive electrode materials. Compared with the development route of high-nickel ternary, another high-manganese ternary material development route also contains huge potential, especially the lithium-rich manganese-based ternary material system (theoretical specific capacity>350mAh·g -1 , reversible specific capacity>250mAh·g -1 ), is one of the positive electrode materials with the highest discharge specific capacity at present. At the same time, manganese resources are abundant, and if industrialized, the production cost of positive electrode materials can be further reduced. Therefore, among many alternative positive electrode materials, lithium-rich manganese-based positive electrode materials have great market potential.
[0004] Although lithium-rich manganese-based materials have many advantages, they also face some problems that need to be solved urgently. Low first coulombic efficiency, poor rate performance and cycle life, and voltage platform attenuation caused by micro-defects in the material structure are key problems facing lithium-rich manganese-based materials, which seriously restrict the application of lithium-rich manganese-based positive electrode materials.
[0005] In the prior art, lithium-rich manganese-based materials are usually modified by methods such as doping, acid treatment, heat treatment, coating, pre-cycling, and atmosphere treatment. These methods have a certain degree of effect on improving the electrochemical properties of lithium-rich manganese-based materials, but they cannot completely solve these shortcomings, especially the shortcomings of poor rate performance of lithium-rich manganese-based materials. The design of appropriate mesoscale structures is an effective strategy to solve the low rate problem of lithium-rich manganese-based materials. However, due to the complexity of the lithium-rich manganese-based material system, the easy occurrence of component segregation during high-temperature sintering, and the destruction of the precursor structure by high lithium salt content, etc., the preparation of lithium-rich manganese-based mesoscale structures is difficult and the preparation cost is extremely high. It is extremely difficult to improve the rate performance of lithium-rich manganese-based materials through this technical approach, which seriously limits its application in high-energy-density lithium-ion batteries. Summary of the invention
[0006] In view of the above problems, the present invention provides a one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material and its preparation method and application. The positive electrode material prepared by the preparation method of the present invention has the advantages of special hierarchical mesoscale structure, large free space, rich structural defects, high electrochemical activity, and high conductivity, showing the energy storage advantage of high energy density, and effectively solving the problems of poor rate performance and low first coulombic efficiency of lithium-rich manganese-based positive electrode material system.
[0007] The present invention provides a one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material comprises the following steps:
[0008] Dissolving a manganese salt, a cobalt salt, and a nickel salt in a first solvent to obtain a first solution;
[0009] dissolving the one-dimensional precursor template in a second solvent to obtain a second solution;
[0010] dissolving a lithium salt in a third solvent to obtain a third solution;
[0011] After the first solution, the second solution and the third solution are uniformly mixed, an alkaline complexing agent is added, and the pH is adjusted to 10-12 to slow down the component segregation, thereby obtaining a fourth solution; for example, the pH is 10, 11, 12, etc.;
[0012] Evaporating the solvent in the fourth solution to obtain a precursor powder;
[0013] In an inert atmosphere, the precursor powder is sintered at 350°C to 500°C to decompose the inorganic salt to obtain an oxide precursor. Then, in an oxygen atmosphere, the oxide precursor is sintered at 700°C to 900°C to allow the four metal ions of Mn, Co, Ni, and Li to fully diffuse into the crystal structure of the precursor template, causing a phase transition to generate a lithium-rich manganese-based ternary phase to obtain Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material.
[0014] In a preferred embodiment of the present invention, the time of a sintering is 4 hours to 6 hours. For example, the time of a sintering is 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, etc. However, it is not limited to the listed values, and other values not listed in the above range are also applicable.
[0015] In a preferred embodiment of the present invention, the secondary sintering time is 5h to 10h. The secondary sintering time is 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, etc. However, it is not limited to the listed values, and other values not listed in the above numerical range are also applicable.
[0016] In a preferred embodiment of the present invention, the one-dimensional precursor template is a one-dimensional manganese oxide nanomaterial, a one-dimensional cobalt oxide nanomaterial or a one-dimensional shuttle-structured manganese-nickel-cobalt ternary oxide.
[0017] In a preferred embodiment of the present invention, the manganese salt is selected from manganese sulfate, manganese carbonate or manganese nitrate; the nickel salt is selected from nickel sulfate, nickel carbonate or nickel nitrate; the cobalt salt is selected from cobalt sulfate, cobalt carbonate or cobalt nitrate; and the lithium salt is selected from lithium nitrate or lithium carbonate.
[0018] In a preferred embodiment of the present invention, the alkaline complexing agent is aqueous ammonia.
[0019] In a preferred embodiment of the present invention, the first solvent, the second solution and the third solution are all selected from anhydrous ethanol or acetone.
[0020] The second object of the present invention is to provide Li prepared by the above preparation method 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material.
[0021] The third object of the present invention is to provide the above-mentioned Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]Application of O2 ternary cathode materials in lithium-ion batteries.
[0022] In a preferred embodiment of the present invention, Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material, conductive material and binder are added to the fourth solvent, dispersed evenly and coated on aluminum foil, dried, cut and pressed to obtain a positive electrode;
[0023] The lithium-ion battery is assembled in the order of positive electrode housing, positive electrode, separator, negative electrode, electrolyte and negative electrode housing.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) Due to the constraints of key factors such as the complexity of the material system, high phase formation temperature, and high lithium content, the design and preparation of the mesoscale structure of lithium-rich manganese-based materials have been greatly hindered. The present invention adopts a sacrificial template method, using a one-dimensional oxide as a precursor template while also serving as the corresponding manganese raw material, nickel raw material, or cobalt raw material, and through a liquid phase complexation method, in an alkaline environment, Mn, Co, and Ni ions are more evenly combined together, and can be fully mixed with the precursor template to slow down the component segregation during the sintering process. Then, a low-energy atmosphere sintering method is used, that is, a low-temperature sintering method is a primary sintering at 350°C to 500°C, and a secondary sintering is performed at 700°C to 900°C. The in-situ sacrificial template method is used to prepare a type of high-energy-density one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material. The positive electrode material prepared by the present invention has the advantages of special hierarchical mesoscale structure, large free space, rich structural defects, high electrochemical activity, and high conductivity, etc. It shows the advantage of high energy density energy storage, and effectively solves the problems of poor rate performance and low first coulomb efficiency of lithium-rich manganese-based positive electrode material system. It is an excellent high-energy positive electrode active material for lithium-ion batteries and can be used to design high energy density energy storage devices.
[0026] (2) According to the preparation method of the present invention, the problems of collapse of lithium-rich manganese-based mesoscale structures and component bias under high-temperature sintering can be effectively overcome, and a one-dimensional lithium-rich manganese-based positive electrode material can be successfully prepared. The electrochemical performance of lithium-rich manganese-based materials can be improved through mesoscale structure design. Designing lithium-rich manganese-based materials into a one-dimensional structure, especially a one-dimensional hierarchical structure spanning multiple scales, can effectively shorten the migration path of lithium ions and enhance the lithium ion transmission kinetics. At the same time, as the specific surface area of the material increases, it can also provide more active sites and improve the utilization efficiency of the active material, which will significantly improve the rate performance and the first coulombic efficiency.
[0027] (3) Designing lithium-rich manganese-based materials into a one-dimensional structure, especially a porous nanotube structure, can provide a large free space. This will effectively alleviate the large volume change of the electrode material caused by lithium insertion / extraction during the charge and discharge cycle, improve the stability of the electrode material, and effectively improve the cycle performance and rate performance of the lithium-rich manganese-based material, providing a practical way to solve the low rate problem faced by the lithium-rich manganese-based material.
[0028] (4) Through the present invention, a type of one-dimensional lithium-rich manganese-based material complex mesoscale structure design and preparation method is provided. The developed preparation method is simple in process and easy to operate, which provides a feasible method for improving the problems faced by lithium-rich manganese-based positive electrode materials. The prepared one-dimensional lithium-rich manganese-based material is applied to lithium-ion battery positive electrode materials to prepare high energy density energy storage devices.
[0029] (5) According to the method of the present invention, one-dimensional lithium-rich manganese-based nanorod active positive electrode material, one-dimensional lithium-rich manganese-based porous nanorod active positive electrode material, one-dimensional lithium-rich manganese-based nanotube active positive electrode material, one-dimensional lithium-rich manganese-based porous nanotube active positive electrode material, one-dimensional lithium-rich manganese-based spindle structure active positive electrode material, and one-dimensional lithium-rich manganese-based spindle porous structure active positive electrode material can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a scanning electron microscope image of the one-dimensional lithium-rich manganese-based porous nanorod active positive electrode material of Example 3.
[0031] Figure 2 This is a scanning electron microscope image of the one-dimensional lithium-rich manganese-based porous nanotube active positive electrode material of Example 7.
[0032] Figure 3 This is a scanning electron microscope image of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure active positive electrode material of Example 11.
[0033] Figure 4 X-ray diffraction patterns of the one-dimensional lithium-rich manganese-based porous nanorods of Example 3, the one-dimensional lithium-rich manganese-based porous nanotubes of Example 7, and the one-dimensional lithium-rich manganese-based shuttle-shaped porous structures of Example 11.
[0034] Figure 5 This is the charge and discharge cycle rate diagram of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure sample in Example 11.
[0035] Figure 6 This is the charge and discharge curve diagram of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure sample in Example 11 at different current densities of 0.1C-5C. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Chinese invention patent CN117446874A discloses a one-dimensional LiMn 1 / 3 Ni 1 / 3 Co 1 / 3 O2 ternary layered oxide positive electrode material and preparation method thereof, and 111 type LiMn 1 / 3 Ni 1 / 3 Co 1 / 3 Compared with the O2 ternary positive electrode material system, the lithium-rich manganese-based Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary cathode material system has a higher difficulty in micro-nano structure design. The difference between the two systems is that Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 needs to generate a ternary lithium-rich manganese-based phase at a higher temperature, generally 850-900°C, while LiMn 1 / 3 Ni 1 / 3 Co 1 / 3 The phase formation temperature of O2 is 800-850℃. During the preparation process, the higher the sintering temperature, the larger the size of the nanocrystals, the greater the stress / strain generated, and the easier it is to cause the micro-nano structure of the precursor to collapse, making it impossible for the micro-nano structure to transition to the positive electrode material. Therefore, the preparation of one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary cathode materials have higher requirements on precursor templates and preparation processes. 1.2 [Mn 0.54 Ni 0.13 Co 0.13 In order to prevent the one-dimensional hierarchical structure of the O2 ternary positive electrode material from collapsing, the ternary phase formation temperature needs to be lowered as much as possible. This can be achieved by refining the precursor grain size, and more delicate process control is required during the operation.
[0038] At the same time, with LiMn 1 / 3 Ni 1 / 3 Co 1 / 3 Compared with O2, due to Li 1.2 [Mn 0.54Ni 0.13 Co 0.13 ] The content ratio of the three transition metal elements Mn, Ni, and Co in ]O2 is unbalanced, so it is easier to cause component segregation during the sintering process, which is also a problem that needs to be solved urgently. Based on this, the present invention provides a Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] The preparation method of O2 ternary positive electrode material needs to avoid component segregation during the preparation process. The specific technical scheme is as follows:
[0039] A kind of Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material comprises the following steps:
[0040] Dissolving a manganese salt, a cobalt salt, and a nickel salt in a first solvent to obtain a first solution;
[0041] dissolving the one-dimensional precursor template in a second solvent to obtain a second solution;
[0042] dissolving a lithium salt in a third solvent to obtain a third solution;
[0043] After the first solution, the second solution, and the third solution are evenly mixed, an alkaline complexing agent is added, and the pH is adjusted to 10-12 to obtain a fourth solution; the reason for adjusting the pH in the present invention is that the Mn, Co, and Ni ions are more evenly combined together, and can be fully mixed with the precursor template to slow down component segregation. When the pH value is low, the three ions of Mn, Co, and Ni are not fully combined. When the pH value is high, it is easy to cause the formation of large agglomerates, which cannot be evenly mixed with the precursor template. Therefore, the pH should be controlled between 10-12.
[0044] Evaporating the solvent in the fourth solution to obtain a precursor powder;
[0045] In an inert atmosphere, the precursor powder is sintered at 350°C to 500°C to decompose the inorganic salt to obtain an oxide precursor. Then, in an oxygen atmosphere, the oxide precursor is sintered at 700°C to 900°C for a second time. The purpose of the second sintering is to allow the four metal ions of Mn, Co, Ni, and Li to fully diffuse into the crystal structure of the precursor template, undergo a phase change at high temperature, and generate a lithium-rich manganese-based ternary phase to obtain Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material.
[0046] In order to fully decompose the inorganic salt, the preferred sintering time in the present invention is 4 to 6 hours.
[0047] In order to generate a high-purity lithium-rich manganese-based ternary phase, the preferred secondary sintering time in the present invention is 5 h to 10 h.
[0048] When selecting a one-dimensional precursor template, the present invention first requires the template to have a one-dimensional structure, and secondly, the composition of the template needs to contain one or more elements of Mn, Ni, and Co, but oxide templates of other transition metal elements cannot be selected, which will lead to the introduction of impurity elements into the prepared electrode material, seriously deteriorating the electrochemical performance of the lithium-rich manganese-based positive electrode material. Preferably, the one-dimensional precursor template is a one-dimensional manganese oxide nanomaterial, a one-dimensional cobalt oxide nanomaterial, or a one-dimensional shuttle-shaped structure manganese-nickel-cobalt ternary oxide.
[0049] It can be understood that the present invention has no particular limitation on lithium salts, nickel salts, cobalt salts and manganese salts. Lithium salts, nickel salts and cobalt salts familiar to those skilled in the art can be used. Those skilled in the art can select and adjust according to actual application conditions, product quality and product performance. Preferably, the manganese salt is selected from manganese sulfate, manganese carbonate or manganese nitrate; the nickel salt is selected from nickel sulfate, nickel carbonate or nickel nitrate; the cobalt salt is selected from cobalt sulfate, cobalt carbonate or cobalt nitrate; and the lithium salt is selected from lithium nitrate or lithium carbonate.
[0050] It should be noted that Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] In the O2 ternary positive electrode material, the ratio of the amount of lithium, manganese, cobalt and nickel is 1.2:0.54:0.13:0.13. In the present invention, the one-dimensional precursor template is used not only as a template, but also as a raw material for synthesizing positive electrode materials. Manganese salt, cobalt salt, nickel salt and lithium salt are calculated according to the ratio. Since the total amount of manganese salt, the total amount of nickel salt or the total amount of cobalt salt is related to the selected one-dimensional precursor template, it is necessary to make corresponding deductions according to the amount of template used; or if only the one-dimensional precursor template provides manganese, cobalt and nickel, there is no need to add additional manganese salt, cobalt salt and nickel salt. For example, if the selected one-dimensional precursor template is a one-dimensional manganese oxide nanomaterial, all manganese salts are converted into the amount of template used; if the selected precursor template is a one-dimensional cobalt oxide nanomaterial, all cobalt salts are converted into the amount of template used; if the selected precursor template is a one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide template, manganese, cobalt and nickel are converted into the amount of template used according to the proportion;
[0051] The alkaline complexing agent is ammonia water. The reason why ammonia water is selected as the alkaline complexing agent used in the present invention is that ammonia water is weakly alkaline and the pH value of the solution is easy to control. At the same time, ammonia water is easy to decompose and will not introduce other impurity elements into the electrode material system.
[0052] In the following specific embodiments, unless otherwise specified, all raw materials can be commercially available or prepared according to existing preparation methods, and the present invention is not limited thereto. It should be noted that the β-MnO2 single crystal nanotubes used in the present invention are prepared according to the preparation method in Section 2.1.1 of "Mesoporous multi-valence manganeseoxides composite nanotubes boosting long-life lithium-ion batteries" published by Zhou Junxiang et al. in "Dalton Transactions".
[0053] The Mn3O4 mesoporous polycrystalline nanotube template was prepared according to the preparation method in Section 2.1.2 of "Mesoporous multi-valence manganese oxides composite nanotubes boosting long-life lithium-ion batteries" published by Zhou Junxiang et al. in "Dalton Transactions" to obtain Mn3O4@CNT.
[0054] The α-MnO2 single crystal nanotube precursor template used in the present invention is prepared by referring to the preparation method in “Synthesis of single-crystal tetragonal α-MnO2 nanotubes” published by Luo J et al. in “The Journal of Physical Chemistry C”.
[0055] The one-dimensional cobalt oxide precursor template used in the present invention is basically the same as the method for preparing β-MnO2 NT in Section 2.1.1 of "Mesoporous multi-valence manganese oxides composite nanotubes boosting long-life lithium-ion batteries" published by Zhou Junxiang et al. in "Dalton Transactions", except that the manganese salt in the preparation process needs to be replaced with the corresponding cobalt salt.
[0056] The one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide template used in the present invention is prepared by a hydrothermal method combined with an atmosphere annealing process, and the specific preparation steps are as follows:
[0057] Dissolve 5.4mmol manganese nitrate, 1.3mmol cobalt nitrate, 1.3mmol nickel nitrate, 38mmol urea, and 14mmol ammonium fluoride in 70ml ultrapure water and stir well. Then, hydrothermally heat at 120℃ for 5h, filter and dry to obtain the hydrothermal product of manganese nickel cobalt hydroxide, i.e., a one-dimensional shuttle-shaped manganese nickel cobalt ternary oxide precursor template.
[0058] The one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide precursor template needs to be annealed at 400° C. for 2 hours in an argon or air atmosphere before use to obtain a one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide template.
[0059] Example 1
[0060] The preparation method of a lithium-rich manganese-based nanorod ternary positive electrode active material of the present invention comprises the following specific steps:
[0061] Step 1, dissolving 0.614 mmol nickel nitrate and 0.614 mmol cobalt nitrate in 20 ml ultrapure water to obtain a first solution;
[0062] Step 2, adding 2.55 mmol of β-MnO2 single crystal nanotube template to 10 ml of ultrapure water and stirring evenly to obtain a second solution;
[0063] Step 3, dissolving 6.81 mmol lithium nitrate in 10 ml ultrapure water to obtain a third solution;
[0064] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, add ammonia water, and adjust the pH value to 10 to obtain a fourth solution;
[0065] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 50° C., and after drying, obtain a uniformly mixed precursor powder;
[0066] Step 6, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0067] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 800° C. for 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0068] Example 2
[0069] The preparation method of a lithium-rich manganese-based nanorod ternary positive electrode active material of the present invention comprises the following specific steps:
[0070] Step 1, dissolving 0.614 mmol nickel chloride and 0.614 mmol cobalt chloride in 20 ml ultrapure water to obtain a first solution;
[0071] Step 2, adding 2.55 mmol of α-MnO2 single crystal nanotube template into 10 ml of ultrapure water and stirring evenly to obtain a second solution;
[0072] Step 3, dissolving 6.81 mmol lithium nitrate in 10 ml ultrapure water to obtain a third solution;
[0073] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, add ammonia water, and adjust the pH value to 10 to obtain a fourth solution;
[0074] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 50° C., and after drying, obtain a uniformly mixed precursor powder;
[0075] Step 6, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0076] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 800° C. for 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0077] Example 3
[0078] The preparation method of a lithium-rich manganese-based porous nanorod ternary positive electrode active material of the present invention comprises the following specific steps:
[0079] Step 1, dissolving 0.614 mmol nickel nitrate and 0.614 mmol cobalt nitrate in 20 ml ultrapure water to obtain a first solution;
[0080] Step 2, adding 0.85 mmol of Mn3O4 mesoporous polycrystalline nanotube template to 10 ml of ultrapure water and stirring evenly to obtain a second solution;
[0081] Step 3, dissolving 6.81 mmol lithium nitrate in 10 ml ultrapure water to obtain a third solution;
[0082] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, add ammonia water, and adjust the pH value to 10 to obtain a fourth solution;
[0083] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 50° C., and after drying, obtain a uniformly mixed precursor powder;
[0084] Step 6, sintering the precursor at 400° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0085] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0086] Example 4
[0087] The preparation method of a lithium-rich manganese-based porous nanorod ternary positive electrode active material of the present invention comprises the following specific steps:
[0088] Step 1, dissolving 0.614 mmol nickel chloride and 0.614 mmol manganese chloride in 20 ml ultrapure water to obtain a first solution;
[0089] Step 2, adding 0.85 mmol of Co3O4 mesoporous polycrystalline nanotube template to 10 ml of ultrapure water and stirring evenly to obtain a second solution;
[0090] Step 3, dissolving 6.81 mmol lithium nitrate in 10 ml ultrapure water to obtain a third solution;
[0091] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, add ammonia water, and adjust the pH value to 10 to obtain a fourth solution;
[0092] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 50° C., and after drying, obtain a uniformly mixed precursor powder;
[0093] Step 6, sintering the precursor at 400° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0094] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0095] Example 5
[0096] The preparation method of a lithium-rich manganese-based nanotube ternary positive electrode active material of the present invention comprises the following specific steps:
[0097] Step 1, dissolving 0.30 mmol nickel nitrate and 0.30 mmol cobalt nitrate in 20 ml anhydrous ethanol to obtain a first solution;
[0098] Step 2, adding 1.25 mmol of β-MnO2 single crystal nanotube template into 10 ml of anhydrous ethanol and stirring evenly to obtain a second solution;
[0099] Step 3, dissolving 1.66 mmol of lithium carbonate in 10 ml of anhydrous ethanol to obtain a third solution;
[0100] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, and add ammonia water to adjust the pH value to 11 to obtain a fourth solution;
[0101] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 40° C., and after drying, obtain a uniformly mixed precursor powder;
[0102] Step 6, sintering the precursor at 500° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0103] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0104] Example 6
[0105] The preparation method of a lithium-rich manganese-based nanotube ternary positive electrode active material of the present invention comprises the following specific steps:
[0106] Step 1, dissolving 0.30 mmol nickel chloride and 0.30 mmol cobalt chloride in 20 ml anhydrous ethanol to obtain a first solution;
[0107] Step 2, adding 1.25 mmol of α-MnO2 single crystal nanotube template into 10 ml of anhydrous ethanol and stirring evenly to obtain a second solution;
[0108] Step 3, dissolving 1.66 mmol of lithium carbonate in 10 ml of anhydrous ethanol to obtain a third solution;
[0109] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, and add ammonia water to adjust the pH value to 11 to obtain a fourth solution;
[0110] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 40° C., and after drying, obtain a uniformly mixed precursor powder;
[0111] Step 6, sintering the precursor at 500° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0112] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0113] Example 7
[0114] The preparation method of a lithium-rich manganese-based porous nanotube ternary positive electrode active material of the present invention comprises the following specific steps:
[0115] Step 1, dissolving 0.30 mmol nickel nitrate and 0.30 mmol cobalt nitrate in 20 ml anhydrous ethanol to obtain a first solution;
[0116] Step 2, adding 1.25 mmol of β-MnO2 mesoporous single crystal nanotubes into 10 ml of anhydrous ethanol and stirring evenly to obtain a second solution;
[0117] Step 3, dissolving 3.32 mmol lithium nitrate in 10 ml anhydrous ethanol to obtain a third solution;
[0118] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, and add ammonia water to adjust the pH value to 11 to obtain a fourth solution;
[0119] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 40° C., and after drying, obtain a uniformly mixed precursor powder;
[0120] Step 6, sintering the precursor at 500° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0121] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0122] Example 8
[0123] The preparation method of a lithium-rich manganese-based porous nanotube ternary positive electrode active material of the present invention comprises the following specific steps:
[0124] Step 1, dissolving 0.30 mmol nickel chloride and 0.30 mmol cobalt chloride in 20 ml anhydrous ethanol to obtain a first solution;
[0125] Step 2, adding 1.25 mmol of Mn3O4 mesoporous polycrystalline nanotubes into 10 ml of anhydrous ethanol and stirring evenly to obtain a second solution;
[0126] Step 3, dissolving 3.32 mmol lithium nitrate in 10 ml anhydrous ethanol to obtain a third solution;
[0127] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, and add ammonia water to adjust the pH value to 11 to obtain a fourth solution;
[0128] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 40° C., and after drying, obtain a uniformly mixed precursor powder;
[0129] Step 6, sintering the precursor at 500° C. for 8 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0130] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0131] Example 9
[0132] The preparation method of a lithium-rich shuttle-shaped ternary positive electrode active material of the present invention comprises the following specific steps:
[0133] Step 1, adding 2 mmol of a one-dimensional shuttle-shaped structure manganese-nickel-cobalt ternary oxide precursor template to 20 ml of ultrapure water and mixing and stirring to obtain a first mixed solution;
[0134] Step 2, dissolving 5.33 mmol lithium nitrate in 10 ml ultrapure water to obtain a second solution;
[0135] Step 3, under continuous stirring, slowly add the second solution to the first mixed solution, mix well, add ammonia water, adjust the pH value to 10, and obtain a third solution;
[0136] Step 4, continuously stirring and heating to slowly evaporate the water in the third solution at 55° C., and after drying, obtain a uniformly mixed precursor powder;
[0137] Step 5, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0138] Step six, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0139] Example 10
[0140] The preparation method of a lithium-rich shuttle-shaped ternary positive electrode active material of the present invention comprises the following specific steps:
[0141] Step 1, dissolving 0.54 mmol manganese nitrate, 0.13 mmol cobalt nitrate, and 0.13 mmol nickel nitrate in 20 ml ultrapure water to obtain a first solution;
[0142] Step 2, adding 2 mmol of a one-dimensional shuttle-shaped structure manganese-nickel-cobalt ternary oxide precursor template to 15 ml of ultrapure water and stirring evenly to obtain a second solution;
[0143] Step 3, dissolving 7.992 mmol lithium nitrate in 10 ml ultrapure water to obtain a third solution;
[0144] Step 4, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, add ammonia water, and adjust the pH value to 10 to obtain a fourth solution;
[0145] Step 5, continuously stirring and heating to slowly evaporate the water in the fourth solution at 55° C., and after drying, obtain a uniformly mixed precursor powder;
[0146] Step 6, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0147] Step seven, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 750° C. for a sintering time of 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0148] Embodiment 11
[0149] The present invention provides a method for preparing a lithium-rich spindle-shaped porous ternary positive electrode active material, and the specific steps are as follows:
[0150] Step 1, heat treating a one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide precursor template at 400° C. in air for 2 hours to obtain a one-dimensional shuttle-shaped porous manganese-nickel-cobalt ternary oxide template;
[0151] Step 2, adding 2 mmol of the one-dimensional shuttle-shaped porous structure manganese-nickel-cobalt ternary oxide template to 20 ml of ultrapure water and mixing and stirring to obtain a first mixed solution;
[0152] Step 4, dissolving 2.67 mmol lithium carbonate in 10 ml ultrapure water to obtain a second solution;
[0153] Step 5, under continuous stirring, slowly adding the second solution to the first mixed solution, mixing evenly, adding ammonia water, adjusting the pH value to 11, and obtaining a third solution;
[0154] Step 6, continuously stirring and heating to slowly evaporate the water in the third solution at 55° C., and after drying, obtain a uniformly mixed precursor powder;
[0155] Step 7, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0156] Step eight, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 800° C. for 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0157] Example 12
[0158] The present invention provides a method for preparing a lithium-rich spindle-shaped porous ternary positive electrode active material, and the specific steps are as follows:
[0159] Step 1, heat treating a one-dimensional shuttle-shaped manganese-nickel-cobalt ternary oxide precursor template at 400° C. in air for 2 hours to obtain a one-dimensional shuttle-shaped porous manganese-nickel-cobalt ternary oxide template;
[0160] Step 2, dissolving 0.54 mmol manganese nitrate, 0.13 mmol cobalt nitrate, and 0.13 mmol nickel nitrate in 20 ml ultrapure water to obtain a first solution;
[0161] Step 3, adding 2 mmol of the one-dimensional shuttle-shaped porous structure manganese-nickel-cobalt ternary oxide template to 15 ml of ultrapure water and stirring evenly to obtain a second solution;
[0162] Step 4, dissolving 3.99 mmol lithium carbonate in 10 ml ultrapure water to obtain a third solution;
[0163] Step 5, under continuous stirring, uniformly mix the first solution, the second solution, and the third solution, and add ammonia water to adjust the pH value to 11 to obtain a fourth solution;
[0164] Step 6, continuously stirring and heating to slowly evaporate the water in the fourth solution at 55° C., and after drying, obtain a uniformly mixed precursor powder;
[0165] Step 7, sintering the precursor at 450° C. for 5 h in an Ar atmosphere to preliminarily decompose the inorganic salt to obtain an oxide powder precursor;
[0166] Step eight, in air, the low-temperature sintered oxide powder precursor is subjected to high-temperature sintering at a temperature of 800° C. for 5 hours to generate a lithium-rich manganese-based ternary phase, thereby obtaining a lithium-rich manganese-based nanorod positive electrode active material.
[0167] Examples 3, 7, and 11 illustrate the physical and electrochemical properties of three ternary positive electrode active materials, namely, one-dimensional lithium-rich manganese-based porous nanorods, one-dimensional lithium-rich manganese-based porous nanotubes, and one-dimensional lithium-rich manganese-based spindle-shaped porous structures prepared by the present invention.
[0168] Figure 1 This is a scanning electron microscope photo of the one-dimensional lithium-rich manganese-based porous nanorod ternary positive electrode active material prepared in Example 3. Figure 1 It can be seen that the lithium-rich manganese-based ternary cathode material presents a typical one-dimensional rod-like nanostructure at the nanoscale, with a diameter of 600-1000nm and a length of 5-10μm. Observing at a smaller scale, it can be found that the nanorods are stacked with nanoparticles, and the nanoparticles are not completely densely packed and connected, but have abundant mesoporous pores, thus forming a hierarchical one-dimensional porous nanorod structure.
[0169] Figure 2 This is a scanning electron microscope photograph of the one-dimensional lithium-rich manganese-based porous nanotube ternary positive electrode active material of Example 7. Figure 2 It can be seen that the lithium-rich manganese-based ternary cathode material presents a one-dimensional tubular nanostructure at the nanoscale, with a diameter of 500-1000nm and a length of 3-6μm. At a smaller scale, it can be observed that the lithium-rich manganese-based porous nanotubes are stacked by nanoparticles, and there are abundant mesoporous pores between the nanoparticles, forming lithium-rich manganese-based nanotubes with a hierarchical porous structure.
[0170] Figure 3 This is a scanning electron microscope photograph of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure ternary positive electrode active material of Example 11. Figure 3 It can be seen that the lithium-rich manganese-based ternary cathode material presents a clear one-dimensional shuttle-shaped structure at the nanoscale, with a diameter of 300-500nm and a length of 1-2μm. At a smaller scale, it can be observed that the lithium-rich manganese-based shuttle-shaped structure is composed of nanoparticles stacked together, and abundant pores are formed between the nanoparticles, forming a lithium-rich manganese-based shuttle-shaped structure with a hierarchical porous structure.
[0171] Figure 4 The X-ray diffraction patterns of the one-dimensional lithium-rich manganese-based porous nanorods of Example 3, the one-dimensional lithium-rich manganese-based porous nanotubes of Example 7, and the one-dimensional lithium-rich manganese-based shuttle-shaped porous structures of Example 11 are shown in Table 1. The horizontal axis is twice the diffraction angle, recorded as 2-θ, in degrees; the vertical axis is the X-ray intensity, in au. Figure 4It can be seen that the samples in Example 3, the samples in Example 6, and the samples in Example 11 all have similar X-ray diffraction spectra, and the angles and crystal planes indicated by the diffraction peaks are consistent. The results show that although the samples prepared in these three examples have different micro-nano structures, the physical phases are consistent. Through physical phase retrieval, it can be determined that the diffraction peaks all point to the α-NaFeO2 phase, and the corresponding PDF card is 81-1953.
[0172] Figure 5 This is a charge-discharge cycle rate diagram of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure ternary positive electrode active material sample prepared in Example 11. The horizontal axis is the number of cycles, in units of circles; the vertical axis is the specific capacity of the material, in units of mAh·g -1 .Depend on Figure 5 It can be seen that the electrode materials have good rate performance. This is due to the hierarchical mesoscale structure design. The existence of the shuttle-shaped porous structure can not only effectively alleviate the large stress / strain of the electrode material during the lithium insertion and extraction process, and slow down the pulverization and deactivation of the material, but the rich pore structure can also provide multiple lithium ion transmission channels, enhance the electrode reaction kinetics, and improve the rate performance of the electrode material.
[0173] Figure 6 This is a charge-discharge curve of the one-dimensional lithium-rich manganese-based spindle-shaped porous structure ternary positive electrode active material sample prepared in Example 11 at different current densities of 0.1C-5C. The abscissa is the specific capacity of the material, in units of mAh·g -1 , the vertical axis is voltage, the unit is V. Figure 6 It can be seen that the charge and discharge curve of the sample shows the characteristics of a typical lithium-rich manganese-based ternary cathode material, further proving that the synthesized electrode material is a lithium-rich manganese-based ternary cathode material, namely Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2.
[0174] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0175] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The following steps are involved: Dissolving a manganese salt, a cobalt salt, and a nickel salt in a first solvent to obtain a first solution; dissolving the one-dimensional precursor template in a second solvent to obtain a second solution; dissolving a lithium salt in a third solvent to obtain a third solution; After the first solution, the second solution and the third solution are uniformly mixed, an alkaline complexing agent is added, and the pH is adjusted to 10-12 to slow down the component segregation, thereby obtaining a fourth solution; Evaporating the solvent in the fourth solution to obtain a precursor powder; In an inert atmosphere, the precursor powder is sintered at 350°C to 500°C to decompose the inorganic salt to obtain an oxide precursor. Then, in an oxygen atmosphere, the oxide precursor is sintered at 700°C to 900°C to allow the four metal ions of Mn, Co, Ni, and Li to fully diffuse into the crystal structure of the precursor template, undergoing a phase transition to generate a lithium-rich manganese-based ternary phase, and obtaining a one-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material.
2. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The sintering time is 4h to 6h.
3. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The secondary sintering time is 5h to 10h.
4. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The one-dimensional precursor template is a one-dimensional manganese oxide nanomaterial, a one-dimensional cobalt oxide nanomaterial or a one-dimensional shuttle-shaped structured manganese-nickel-cobalt ternary oxide.
5. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The manganese salt is selected from manganese sulfate, manganese carbonate or manganese nitrate; the nickel salt is selected from nickel sulfate, nickel carbonate or nickel nitrate; the cobalt salt is selected from cobalt sulfate, cobalt carbonate or cobalt nitrate; the lithium salt is selected from lithium nitrate or lithium carbonate.
6. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The alkaline complexing agent is ammonia water.
7. A one-dimensional Li according to claim 1 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] A method for preparing an O2 ternary positive electrode material, characterized in that: The first solvent, the second solution and the third solution are all selected from anhydrous ethanol or acetone.
8. A one-dimensional Li prepared by the preparation method according to any one of claims 1 to 7 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material.
9. A one-dimensional Li as claimed in claim 8 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]Application of O2 ternary positive electrode materials in lithium-ion batteries.
10. A one-dimensional Li according to claim 8 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ] The application of O2 ternary positive electrode material in lithium ion battery is characterized in that: One-dimensional Li 1.2 [Mn 0.54 Ni 0.13 Co 0.13 ]O2 ternary positive electrode material, conductive material and binder are added to the fourth solvent, dispersed evenly and coated on aluminum foil, dried, cut and pressed to obtain a positive electrode; The lithium-ion battery is assembled in the order of positive electrode housing, positive electrode, separator, negative electrode, electrolyte and negative electrode housing.