Production method of modified glass fiber powder

By mixing and crushing glass fiber with chopped glass fiber, and surface modification of sulfonated thixotropic agent and borane coupling agent, the problem of poor dispersion of glass fiber powder is solved, and its in coatings, plastics and The filling performance in rubber achieves better mechanical properties and scratch resistance.

CN118954942AInactive Publication Date: 2024-11-15ANHUI HUACHAO NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149399.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor dispersion of glass fiber powder limits its application effect, especially when the filling amount is large, the mechanical properties and scratch resistance of the product are insufficient.

Method used

Modified glass fiber powder is prepared by mixing and crushing glass fibers with chopped glass fibers, and adding sulfonated thixotropic agent and borane coupling agent during the grinding process to modify the surface, thereby improving its dispersion and interface bonding. strength.

Benefits of technology

Modified glass fiber powder maintains good mechanical properties and scratch resistance under large filling amounts, and has better performance than existing inorganic fillers, such as alumina and talc powder. It has a simple production process and low cost, and uses waste materials. Fiberglass cutter wire.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a production method of modified glass fiber powder, and belongs to the technical field of glass fiber powder.The production method comprises the steps that firstly, organic matter such as waxiness on the surfaces of waste cutting wires is removed through heat treatment, the waste cutting wires and chopped glass fibers are mixed, crushed and ground to prepare glass fiber powder, surface modification is conducted through a sulfonated thixotropic agent and a borane coupling agent, and the modified glass fiber powder is obtained. The chopped glass fiber powder is prepared. The modified glass fiber powder can be used for filling coatings, plastics and rubber, has better performance than alumina, heavy calcium powder, talcum powder and other inorganic fillers used in the prior art, is simple and convenient in production process, low in manufacturing cost and good in dispersity, utilizes waste glass fibers for cutting, and enables products to maintain good mechanical properties under the condition of large filling amount. The hardness and the scratch resistance of the filling surface are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass fiber powder, and particularly relates to a production method of modified glass fiber powder. Background Art

[0002] Glass fiber powder is glass fiber that is crushed and screened. It has the characteristics of heat resistance, wear resistance, corrosion resistance, and good electrical insulation. In the past, it was used as a high-temperature lubricant and release agent for rolled steel, steel pipes, and cast steel parts in the steel industry. Xie Songbo and others prepared SiO2 aerogel / glass fiber thermal insulation coating using SiO2 aerogel powder as filler, glass fiber powder as reinforcement, and fluorosilicone acrylic emulsion as film-forming material. Glass fiber powder is a short fiber with good dispersibility and fluidity. Compared with granular powder, it has the properties of fiber products such as enhanced crack resistance and wear resistance. In addition, glass fiber powder is not easy to sink, and can also improve the leveling of the coating. However, the poor dispersibility of glass fiber powder limits the effect of its application. As a technician in this field, it is urgent to develop a new production method for modified glass fiber powder. Summary of the invention

[0003] The purpose of the invention is to provide a method for producing modified glass fiber powder in view of the existing problems.

[0004] The present invention is achieved through the following technical solutions: A production method of modified glass fiber powder comprises the following steps: 1. heat-treating slit glass fiber yarns and feeding them into a crusher, then adding chopped glass fibers accounting for 5% to 10% of the mass of the slit glass fiber yarns, mixing and crushing them together, and continuing grinding to obtain glass fiber powder; 2. preparing a slurry with a solid content of 70 to 75% with water using the glass fiber powder obtained in the previous step, adding a sulfonated thixotropic agent solution into the slurry and stirring the slurry evenly, then de-agglomerating and breaking up the slurry, adding a borane coupling agent solution for surface modification, and then drying and sieving to obtain the modified glass fiber powder.

[0005] Furthermore, the process control conditions of the liquid phase dispersion process are stirring temperature of 30-45° C., 500-800 rpm, and stirring time of 10-20 min.

[0006] In the production process of glass fiber factories, it is inevitable to produce a certain amount of slit yarn, which is the waste product in glass fiber production.

[0007] Furthermore, the mass ratio of the slit glass fiber to the chopped glass fiber is 100:30-45.

[0008] The crushing efficiency can be improved by crushing the glass fiber cutter wire and the short glass fiber together. The size difference of the simple glass fiber cutter wire is small, and the addition of some short glass fibers can achieve the size difference. The glass fiber cutter wire generates stress under the collision of the size difference and breaks, thereby improving the crushing efficiency.

[0009] Furthermore, the sulfonated thixotropic agent is one of a sulfonated melamine resin or a sulfonated phenolic resin.

[0010] Furthermore, the sulfonated thixotropic agent solution is a 15-20% aqueous solution prepared by warm water at 40-50° C., and the amount of the sulfonated thixotropic agent solution added is 0.2-0.5% of the volume ratio of the slurry.

[0011] Furthermore, the borane coupling agent solution is an aqueous solution with a mass fraction of 10% to 15% of a water-soluble borane coupling agent, and the added amount is 3 to 5‰ of the mass of the powder.

[0012] Furthermore, the chopped glass fibers have a diameter of 10 μm to 13 μm and a chopped length of 4.5 mm to 18 mm.

[0013] Furthermore, the borane coupling agent is one of XY-633 and B-1816.

[0014] Furthermore, the heat treatment is performed at 600-700° C. for 10-15 minutes.

[0015] Beneficial effects of the present invention: The production method of chopped glass fiber powder disclosed in the present invention first removes organic matter such as wax on the surface of waste slit wire through heat treatment, prepares glass fiber powder by mixing, crushing and grinding with chopped glass fiber, and performs surface modification through sulfonated thixotropic agent and borane coupling agent to obtain chopped glass fiber powder. The modified glass fiber powder can be used to fill coatings, plastics and rubbers, and its performance is better than inorganic fillers such as alumina, heavy calcium powder and talcum powder used in the past. Its production process is simple and its manufacturing cost is low. It uses waste glass fiber slit wire, has low manufacturing cost and good dispersibility. In the case of a large filling amount, the product still maintains good mechanical properties, and improves the hardness and scratch resistance of the filling surface. DETAILED DESCRIPTION

[0016] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1

[0017] Raw materials and equipment: chopped glass fiber with a diameter of 13μm, chopped glass fiber with a length of 18mm, 45-count alkali-free glass fiber with a diameter of 16μm; borane coupling agent Xingye Petrochemical XY-633. Tianfeng Chemical SM-F sulfonated melamine resin.

[0018] The production method of modified glass fiber powder comprises the following steps: 1. heat-treating glass fiber slits and feeding them into a crusher, then adding chopped glass fibers which are 10% of the mass of the glass fiber slits and mixing and crushing them together, and continuing grinding for 100 minutes to obtain glass fiber powder, wherein the mass ratio of the glass fiber slits to the chopped glass fibers is 100:30; 2. preparing the glass fiber powder obtained in the previous step into a slurry with a solid content of 70% by water, adding a sulfonated thixotropic agent solution into the slurry and stirring evenly, wherein the sulfonated thixotropic agent solution is 4 The mass fraction of the aqueous solution is 15% prepared by warm water at 0°C, the amount of the sulfonated thixotropic agent solution added is 0.2% of the slurry volume ratio, and then after deagglomeration and dispersion, a borane coupling agent solution is added for surface modification treatment, and then dried and sieved to obtain a modified glass fiber powder with a particle size of 325 mesh and a moisture content of 0.10%. The borane coupling agent solution is an aqueous solution with a mass fraction of 10% of the water-soluble borane coupling agent, and the amount added is 3‰ of the powder mass. The stirring temperature is 30°C, 500rpm, and the stirring time is 10min.

[0019] 30% filled polyimide performance: tensile strength 175.5MPa; unnotched impact strength 49.3KJ / m 2 ; Flexural strength 198.4MPa; Vicat softening temperature 225℃; Heat deformation temperature 260℃; Rockwell hardness 115.

[0020] Comparative Example 1 The glass fiber powder obtained in step 1 of Example 1 is not subjected to the modification treatment in step 2.

[0021] 30% filled polyimide performance: tensile strength 100.2MPa; unnotched impact strength 28.4KJ / m 2 ; Bending strength 150MPa, Vicat softening temperature 220℃, heat deformation temperature 250℃, Rockwell hardness 110.

[0022] Comparative Example 2 The glass fiber powder obtained in step 1 of Example 1 is prepared with A-1100 coupling agent into a 2% by mass solution, which is then added dropwise to the glass fiber powder and stirred at high speed for 3 minutes; then dried at 100° C. for 3 hours to obtain the surface-treated glass fiber powder.

[0023] 30% filled polyimide performance: tensile strength 123.4MPa; unnotched impact strength 37.7KJ / m 2 ; Bending strength 164.2MPa, Vicat softening temperature 221℃, heat deformation temperature 253℃, Rockwell hardness 112.

[0024] Comparative Example 3 325 mesh calcium carbonate powder.

[0025] 30% filled polyimide performance: tensile strength 89.5MPa, unnotched impact strength 25.4KJ / m 2 ; Bending strength 128.6MPa; Vicat softening temperature 215℃; Heat deformation temperature 248℃, Rockwell hardness 105.

[0026] Note: Shandong Hongrun New Material Polyimide Molding Powder is prepared by mechanically mixing polyimide powder and the glass fiber powder of Example 1, Control Example 1, Control Example 2 and the heavy calcium carbonate powder of Control Example 3 at a mass ratio of 30%, and hot pressing the mixture at a molding temperature of 340°C and a pressure of 12 MPa, and then cooling the mixture to 100°C for demolding. The tensile strength, flexural strength, impact strength and other properties after filling are tested.

[0027] By comparison, it is found that the glass fiber powder of the unmodified control example 1 also has a certain filling effect, but it is not modified, and gaps and defects are easily generated on the surface of the filled glass fiber powder, which makes the strength after filling not high in comparison, and the impact toughness is also dwarfed, but it is significantly better than the calcium carbonate powder of the same particle size. After silane modification, the strength is improved to a certain extent, but the improvement is limited. The sulfonated thixotropic agent of Example 1 can significantly improve the fluidity of the glass fiber powder in the modification process. The sulfonated thixotropic agent itself is a sulfonated polymer resin, and can also improve the dispersibility of the glass fiber powder in the polymer matrix. The borane coupling agent can react with both the hydroxyl groups in the glass fiber and the long molecular chains of the polymer, thereby increasing the interfacial bonding strength between the resin and the glass fiber powder, and the filling effect is better. Example 2

[0028] Raw materials and equipment: chopped glass fiber with a diameter of 10μm, chopped glass fiber with a length of 4.5mm, 100-count alkali-free glass fiber with a diameter of 16μm; borane coupling agent Rongsheng B-1816; Rongsheng Chemical SMP-Ⅱ sulfonated phenolic resin.

[0029] The production method of modified glass fiber powder comprises the following steps: 1. heat-treating glass fiber slits and feeding them into a crusher, then adding chopped glass fibers which are 5% by weight of the glass fiber slits and mixing and crushing them together, and continuing grinding for 130 minutes to obtain glass fiber powder, wherein the mass ratio of the glass fiber slits to the chopped glass fibers is 100:45; 2. preparing the glass fiber powder obtained in the previous step into a slurry with a solid content of 75% by water, adding a sulfonated thixotropic agent solution into the slurry and stirring evenly, wherein the sulfonated thixotropic agent solution is 50 ℃ warm water prepared into an aqueous solution with a mass fraction of 20%, the sulfonated thixotropic agent solution is added in an amount of 0.5% of the slurry volume ratio, and then after de-agglomeration and dispersion, a borane coupling agent solution is added for surface modification treatment, and then dried and sieved to obtain a modified glass fiber powder with a particle size of 200 mesh and a moisture content of 0.10%. The borane coupling agent solution is an aqueous solution with a mass fraction of 15% of the water-soluble borane coupling agent, and the addition amount is 5‰ of the powder mass. The stirring temperature is 45℃, 800rpm, and the stirring time is 20min.

[0030] Note: The fiber diameter shall be tested in accordance with GB / T7690.5-2013 Test methods for reinforcing material yarns Part 5: Determination of glass fiber diameter; the moisture content shall be tested in accordance with GB / T9914.1-2013 Test methods for reinforced products Part 1: Determination of moisture content; the tensile strength shall be tested in accordance with GB / T 1040.2-2006. The unnotched impact strength shall be tested in accordance with GB / T 1043.1-2008. The flexural strength shall be tested in accordance with GB / T 9341-2008. The Vicat softening temperature shall be tested in accordance with GB / T 1633-2000. The heat deformation temperature shall be tested in accordance with GB / T 1634.2-2004. The Rockwell hardness shall be tested in accordance with GB / T 3398.2-2008.

Claims

1. A method for producing modified glass fiber powder, characterized in that: The following steps are involved:

1. Heat-treat the chopped glass fiber yarn and feed it into a crusher, then add chopped glass fibers accounting for 5% to 10% of the mass of the chopped glass fiber yarn, mix and crush them together, and continue grinding to obtain glass fiber powder; 2. Prepare the glass fiber powder obtained in the previous step into a slurry with a solid content of 70 to 75% with water, add a sulfonated thixotropic agent solution into the slurry and stir evenly, then add a borane coupling agent solution to perform surface modification treatment after de-agglomeration and then dry and sieve to obtain modified glass fiber powder.

2. The method for producing modified glass fiber powder according to claim 1, characterized in that: The process control conditions of the liquid phase dispersion process are stirring temperature of 30-45° C., 500-800 rpm, and stirring time of 10-20 min.

3. The method for producing modified glass fiber powder according to claim 1, characterized in that: The mass ratio of the slit glass fiber to the chopped glass fiber is 100:30-45.

4. The method for producing modified glass fiber powder according to claim 1, characterized in that: The sulfonated thixotropic agent is one of a sulfonated melamine resin and a sulfonated phenolic resin.

5. The method for producing modified glass fiber powder according to claim 1, characterized in that: The sulfonated thixotropic agent solution is a 15-20% aqueous solution prepared with warm water at 40-50° C., and the added amount of the sulfonated thixotropic agent solution is 0.2-0.5% of the volume ratio of the slurry.

6. The method for producing modified glass fiber powder according to claim 1, characterized in that: The borane coupling agent solution is an aqueous solution with a mass fraction of 10% to 15% of a water-soluble borane coupling agent, and the added amount is 3 to 5‰ of the mass of the powder.

7. The method for producing modified glass fiber powder according to claim 1, characterized in that: The chopped glass fibers have a diameter of 10 μm to 13 μm and a chopped length of 4.5 mm to 18 mm.

8. The method for producing modified glass fiber powder according to claim 1, characterized in that: The borane coupling agent is one of XY-633 and B-1816.