Method for producing low-alkali glass plate, and low-alkali glass plate
By adjusting the relationship between B2O3 content and β-OH value and the electric melting process, combined with overflow pull-down molding, the heat shrinkage control problem of low-alkali glass plates with high strain point and excellent bubble quality is solved, and the application of high-quality products is achieved Glass substrate for fine display.
Patent Information
- Application Number
- CN202410963984.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-25
- Filing Date
- 2021-06-21
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to achieve low alkali glass plates with high strain points and excellent bubble quality at the same time, and the heat shrinkage rate is difficult to control under high temperature conditions, affecting the electrical performance of the display.
By adjusting the relationship between B2O3 content and β-OH value (y = ax + b, 0.03 < a < 0.04 and 0.02 < b < 0.1), combined with the electromelt and clarification process, low components such as SiO2, Al2O3, B2O3 and others were prepared Alkaline glass plates and are molded by overflow pull-down method to reduce heat shrinkage.
It realizes a low-alkali glass plate with high strain point, low heat shrinkage and excellent bubble quality. It is suitable for glass substrates of high-fine displays, ensuring the electrical performance and surface quality of the display.
Smart Images

Figure CN118954946A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is a divisional application that entered the Chinese national stage on August 12, 2022, with the national application number 202180014537.1, and the invention name is “Method for manufacturing low-alkali glass sheet and low-alkali glass sheet”. Technical Field
[0003] The present invention relates to a low-alkali glass plate, and more particularly to a low-alkali glass plate suitable for a display having a thin film transistor (TFT) having an oxide film such as IGZO or a low temperature polycrystalline silicon (LTPS) film. Background Art
[0004] Flat panel displays usually use a glass plate as a supporting substrate. Circuit patterns such as TFTs are formed on the surface of the glass plate. Therefore, in order to avoid adverse effects on TFTs, low-alkali glass plates that substantially do not contain alkali metal components are used in such glass plates.
[0005] In addition, the glass plate is exposed to a high temperature atmosphere during the circuit pattern forming process such as the thin film forming process and the thin film patterning process. When the glass plate is exposed to a high temperature atmosphere, the structural relaxation of the glass will occur, so the volume of the glass plate will shrink (hereinafter, the shrinkage of the glass will be referred to as "thermal shrinkage"). If the glass plate undergoes thermal shrinkage during the circuit pattern forming process, the shape and size of the circuit pattern formed on the glass plate will deviate from the design value, making it difficult to obtain a flat panel display with the desired electrical performance. Therefore, for glass plates such as glass plates for flat panel displays that have thin film patterns such as circuit patterns formed on the surface, it is desirable to have a small thermal shrinkage rate.
[0006] In particular, in the case of a glass plate for a high-definition display having a TFT having an oxide film such as IGZO or a low-temperature polysilicon film, when the oxide film or the low-temperature polysilicon film is formed, it is exposed to a very high temperature atmosphere such as 450°C to 600°C, and thermal shrinkage is easily generated. However, since the circuit pattern is highly precise, it is difficult to obtain the desired electrical performance if thermal shrinkage occurs. Therefore, it is strongly desired that the thermal shrinkage rate of the glass plate used in such an application is very small.
[0007] In addition, as a method for forming a glass plate used in a flat panel display or the like, a float process, a down-draw process represented by an overflow down-draw process, and the like are known.
[0008] The float process is a method of forming a glass sheet by flowing molten glass onto a float kiln filled with molten tin, stretching it horizontally to form a glass ribbon, and then annealing the glass ribbon in an annealing furnace located downstream of the float kiln. In the float process, the conveying direction of the glass ribbon is horizontal, so it is easy to extend the annealing furnace. Therefore, it is easy to fully reduce the cooling rate of the glass ribbon in the annealing furnace. Therefore, the float process has the advantage of easily obtaining a glass sheet with a small thermal shrinkage rate.
[0009] However, the float process has disadvantages in that it is difficult to form a thin glass plate and that the surface of the glass plate must be polished after forming to remove tin adhering to the surface of the glass plate.
[0010] On the other hand, the down-draw method is a method of stretching molten glass downward to form a plate. The overflow down-draw method, which is one of the down-draw methods, is a method of forming a glass ribbon by stretching the molten glass overflowing from both sides of a forming body (forming body) with a roughly wedge-shaped cross section downward. The molten glass overflowing from both sides of the forming body flows down along the two sides of the forming body and converges below the forming body. Therefore, in the overflow down-draw method, the surface of the glass ribbon is not in contact with anything other than air, but is formed by surface tension, so even if the surface is not ground after forming, no foreign matter will be attached to the surface, and a glass plate with a flat surface can be obtained. In addition, according to the overflow down-draw method, it is also easy to form a thin glass plate.
[0011] On the other hand, in the down-draw method, the molten glass flows downward from the forming body. If a long annealing furnace is to be arranged below the forming body, the forming body must be arranged at a high place. However, in reality, due to the limitation of the ceiling height of the factory, the height at which the forming body can be arranged is limited. That is, in the down-draw method, there is a limitation on the length of the annealing furnace, and it is sometimes difficult to arrange a sufficiently long annealing furnace. When the length of the annealing furnace is short, the cooling rate of the glass ribbon becomes high, so it is difficult to form a glass sheet with a small thermal shrinkage rate.
[0012] Therefore, a technology for increasing the strain point of glass and reducing the thermal shrinkage of glass has been proposed. For example, a low-alkali glass composition with a high strain point is disclosed in Patent Document 1. In addition, the document states that the lower the β-OH value indicating the amount of water in the glass, the higher the strain point.
[0013] Prior art literature
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2013-151407 Summary of the invention
[0016] Technical problem that the invention aims to solve
[0017] likeFigure 1 As shown in FIG. 1 , the higher the strain point, the smaller the thermal shrinkage rate. However, since the glass whose composition is designed to have a high strain point has a high viscosity, there is a problem that defoaming is poor and it is difficult to obtain glass with excellent bubble quality.
[0018] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a low-alkali glass plate having a high strain point and excellent bubble quality, and a method for producing the same.
[0019] Technical solutions to the problem
[0020] The method for producing a low-alkali glass plate of the present invention is characterized by comprising: a batch material preparation step to produce a glass composition containing SiO in mass %. 2 50~70%、Al 2 O 3 15~25%, B 2 O 3 1.8~4.5%, MgO 0~10%, CaO 0~10%, SrO 0~10%, BaO 0~15%, ZnO 0~5%, ZrO 2 0~1%、TiO 2 0~5%、P 2 O 5 0~10%、SnO 2 The method comprises the following steps: preparing a batch of raw materials by a method of preparing a batch of raw materials with a low alkali content of 0.1 to 0.5%; a melting step of melting the prepared batch of raw materials; a clarification step of clarifying the molten glass; and a molding step of molding the clarified glass into a plate shape. 2 O 3 When the content of B is x (mass %) and the β-OH value of the obtained low-alkali glass plate is y ( / mm), the B 2 O 3 The content and β-OH value are adjusted so that the relationship y=ax+b, 0.03<a<0.04 and 0.02<b<0.1 holds true.
[0021] Here, "low-alkali glass" refers to glass to which no alkali metal oxide components are intentionally added. Specifically, it refers to the alkali metal oxide (Li 2 O、Na 2 O, and K 2 It should be noted that the content of alkali metal oxides in the glass composition is preferably 500 ppm or less, particularly preferably 300 ppm or less.
[0022] In the present invention, since the glass composition B used is 2 O 3The content of B is small, so a glass plate with a high strain point can be obtained. However, glass with a high strain point generally has high viscosity and it is difficult to achieve high bubble quality. Therefore, it is further found that in the present invention, by controlling B as in the above formula 2 O 3 content and β-OH value and contains SnO which has a clarifying effect at higher temperatures 2 As an essential ingredient, high foam quality can also be achieved.
[0023] In the production method of the present invention, it is preferable to obtain a glass composition containing SiO in mass %. 2 60~70%, B 2 O 3 1.8~3%, MgO 2~10%, BaO 0.1~15%, SnO 2 0.1~0.3% low alkali glass plate.
[0024] In the manufacturing method of the present invention, electric melting is preferably performed. Here, "electric melting" refers to a melting method in which electricity is passed through the glass, and the Joule heat generated thereby is used to heat the glass and melt the glass. In addition, the use of radiation heating by a heater or a burner as an auxiliary is not excluded.
[0025] If the above structure is adopted, the increase of moisture in the atmosphere can be suppressed. As a result, the supply of moisture from the atmosphere to the glass can be greatly suppressed, and glass with a high strain point can be easily manufactured. In addition, since the glass melt is heated by the heat (Joule heat) of the glass itself, the glass can be heated efficiently. Therefore, the raw material batch can be melted at a relatively low temperature.
[0026] In the manufacturing method of the present invention, it is preferred not to use radiation heating based on burner combustion. "Not using radiation heating based on burner combustion" means that radiation heating based on burner combustion is not performed at all during normal production, and does not exclude the use of a burner during production startup (temperature increase). In addition, it does not exclude the use of radiation heating based on a heater during production startup or normal production. It should be noted that the production startup refers to the period until the raw material batch is dissolved into a glass melt and can be electrically heated.
[0027] If the above structure is adopted, the amount of moisture contained in the atmosphere in the melting furnace becomes extremely small, and the moisture supplied from the atmosphere to the glass can be greatly reduced. As a result, glass with extremely low moisture content can be manufactured. In addition, the burner, flue, fuel tank, fuel supply path, air supply device (in the case of air combustion), oxygen generator (in the case of oxygen combustion), exhaust gas treatment device, dust collector and other equipment required for combustion heating are no longer needed, or they are greatly simplified, which can realize the compactness of the melting furnace and the reduction of equipment cost.
[0028] In the production method of the present invention, preferably, a nitrate raw material is contained in the raw material batch.
[0029] In the production method of the present invention, it is preferable to use boric anhydride as at least a part of the glass raw material serving as a boron source.
[0030] According to the above structure, the water content of the obtained glass can be reduced.
[0031] In the production method of the present invention, preferably, a hydroxide raw material is contained in the raw material batch.
[0032] According to the above structure, the water content of the obtained glass can be adjusted.
[0033] In the manufacturing method of the present invention, preferably, glass scraps are contained in the raw material, and at least a portion of the glass scraps is glass scraps containing glass having a β-OH value of 0.5 / mm or less. Here, "glass scraps" refer to defective glass produced in the manufacture of glass, or recycled glass recovered from the market. "β-OH value" refers to the value obtained by measuring the transmittance of glass using FT-IR and using the following formula.
[0034] β-OH value = (1 / X)log(T 1 / T 2 )
[0035] X: Glass wall thickness (mm)
[0036] T 1 :Reference wavelength 3846cm -1 Transmittance at (%)
[0037] T 2 :Hydroxy absorption wavelength 3600cm -1 Minimum transmittance near (%)
[0038] Since low-alkali glass has a high volume resistivity, it tends to be difficult to melt compared to glass containing alkali. Therefore, if the above structure is adopted, the melting of glass becomes easy and the water content of the obtained glass can be further reduced.
[0039] In the production method of the present invention, it is preferred to adjust glass raw materials and / or melting conditions so that the β-OH value of the obtained glass is less than 0.26 / mm.
[0040] If the above structure is adopted, it is easy to obtain glass with a high strain point and a low thermal shrinkage.
[0041] In the manufacturing method of the present invention, preferably, the obtained glass has a strain point of 700 °C or higher. Herein, the "strain point" is a value measured based on the method of ASTM C336-71.
[0042] If the above structure is adopted, glass with an extremely small thermal shrinkage rate can be obtained.
[0043] In the manufacturing method of the present invention, preferably, the obtained glass has a thermal shrinkage rate of 20 ppm or less. Herein, the "thermal shrinkage rate" refers to the value measured after heat treatment under the condition of heating the glass from room temperature to 500 °C at a rate of 5 °C / minute, holding it at 500 °C for 1 hour, and then cooling it at a rate of 5 °C / minute.
[0044] If the above structure is adopted, a glass plate suitable for forming an oxide TFT or a low-temperature polycrystalline silicon TFT can be obtained.
[0045] The low-alkali glass plate of the present invention is characterized in that, as the glass composition, in mass %, it contains: SiO 2 50 to 70%, Al 2 O 3 15 to 25%, B 2 O 3 1.8 to 4.5%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 10%, BaO 0 to 15%, ZnO 0 to 5%, ZrO 2 0 to 1%, TiO 2 0 to 5%, P 2 O 5 0 to 10%, SnO 2 0.1 to 0.5%, and the β-OH value is 0.1 / mm or more and less than 0.22 / mm. When the content of B 2 O 3 is set as x (mass %), and the β-OH value is set as y ( / mm), the relational expressions of y = ax + b, 0.03 < a < 0.04, and 0.02 < b < 0.1 are established.
[0046] In the low-alkali glass plate of the present invention, preferably, as the glass composition, in mass %, it contains: Al 2 O 3 15 to 21%, B 2 O 3 2 to 4%, MgO 0.1 to 10%, CaO 0.1 to 10%, ZrO 2 0 to 0.5%, TiO 2 0 to 1%.
[0047] In the low-alkali glass sheet of the present invention, preferably, as the glass composition, by mass%, it contains: SiO 2 60 to 70%, B 2 O 3 2 to 3%, MgO 2 to 10%, BaO 0.1 to 15%, SnO 2 0.1 to 0.3%.
[0048] In the low-alkali glass sheet of the present invention, preferably, the strain point is 700 °C or higher.
[0049] In the low-alkali glass sheet of the present invention, preferably, the thermal shrinkage rate is 20 ppm or less.
[0050] In the low-alkali glass sheet of the present invention, preferably, it is used as a glass sheet on which an oxide TFT or a low-temperature p-Si TFT is formed.
[0051] When forming an oxide TFT or a low-temperature polysilicon TFT on a substrate, the heat treatment temperature is high (around 450 to 600 °C), and the circuit pattern becomes finer. Therefore, in the glass sheet used for such applications, a glass sheet with a particularly small thermal shrinkage rate is required. Therefore, the advantages of using the glass sheet of the present invention with a high strain point are great.
[0052] The manufacturing method of the low-alkali glass sheet of the present invention is characterized in that, as the glass composition, by mass%, it contains: SiO 2 50 to 70%, Al 2 O 3 15 to 25%, B 2 O 3 1.8 to 3%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 10%, BaO 0 to 15%, ZnO 0 to 5%, ZrO 2 0 to 1%, TiO 2 0 to 5%, P 2 O 5 0 to 10%, SnO 2 0.1 to 0.5%, and the β-OH value is 0.1 / mm or more and less than 0.22 / mm. When the content of B 2 O 3 is set as x (mass%) and the β-OH value is set as y ( / mm), the content of B 2 O 3 and the β-OH value are adjusted so that the relational expression of y = ax + b, 0.03 < a < 0.04 and 0.05 < b < 0.1 holds.
[0053] The low-alkali glass sheet of the present invention is characterized in that, as the glass composition, by mass%, it contains: SiO 250 to 70%, Al 2 O 3 15 to 25%, B 2 O 3 1.8 to 3%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 10%, BaO 0 to 15%, ZnO 0 to 5%, ZrO 2 0 to 1%, TiO 2 0 to 5%, P 2 O 5 0 to 10%, SnO 2 0.1 to 0.5%, and the β-OH value is 0.1 / mm or more and less than 0.22 / mm. When the content of B 2 O 3 is set as x (mass %), and the β-OH value is set as y ( / mm), the relational expressions y = ax + b, 0.03 < a < 0.04, and 0.05 < b < 0.1 are established. Description of the Drawings
[0054] Figure 1 is a graph showing the relationship between the strain point and the thermal shrinkage rate of the glass.
[0055] Figure 2 is a top view for explaining the measurement sequence of the thermal shrinkage rate of the glass plate. Detailed Description of the Invention
[0056] Hereinafter, the method for manufacturing the low-alkali glass plate of the present invention will be described in detail.
[0057] The method of the present invention is a method for continuously manufacturing a low-alkali glass plate, including: a batch preparation step of preparing a raw material batch; a melting step of melting the prepared raw material batch; a clarification step of clarifying the melted glass; and a forming step of forming the clarified glass. Hereinafter, each step will be described in detail.
[0058] (1) Batch Preparation Step
[0059] First, glass raw materials are prepared so as to form a low-alkali glass. In the low-alkali glass, as the glass composition, by mass %, it contains: SiO 2 50 to 70%, Al 2 O 3 15 to 25%, B 2 O 3 1.8 to 4.5%, MgO 0 to 10%, CaO 0 to 10%, SrO 0 to 10%, BaO 0 to 15%, ZnO 0 to 5%, ZrO 2 0 to 1%, TiO 2 0 to 5%, P 2 O5 0~10%、SnO 2 0.1 to 0.5%. The reasons for limiting the content of each component as described above are described below. It should be noted that, unless otherwise specified, the % in the description of each component below refers to mass %. In addition, the raw materials used will be described later.
[0060] SiO 2 It is a component that forms the skeleton of glass. SiO 2 The lower limit of the content of SiO is preferably 50%, 51%, 51.5%, 52%, 55%, 58%, and particularly preferably 60%. 2 The upper limit of the content of SiO is preferably 70%, 69%, 68%, 67%, 66%, 65%, and particularly preferably 64%. 2 The content of SiO can be 50-70%, 50-69%, 50-68%, 51-67%, 51-66%, 51.5-65%, 52-64%, 55-64%, 58-64%, 60-64%, or 60-70%. 2 If the content of SiO is too low, the density becomes too high and the acid resistance tends to decrease. 2 If the content of is too much, the high temperature viscosity becomes high and the meltability is easily reduced. In addition, devitrified crystals such as cristobalite are easily precipitated and the liquidus temperature is easily increased.
[0061] Al 2 O 3 Al is a component that forms the glass skeleton, increases the strain point and Young's modulus, and suppresses phase separation. 2 O 3 The lower limit of the content of Al is preferably 15%, 15.5%, 16%, 16.5%, and particularly preferably 17%. 2 O 3 The upper limit of the content of Al is preferably 25%, 24%, 23%, 22%, 21.5%, 21%, 20.5%, and particularly preferably 20%. 2 O 3 The content of Al can be 15-25%, 15-24%, 15-23%, 15.5-22%, 16-21.5%, 16.5-21%, 17-20.5%, or 17-20%. 2 O 3 If the content of Al is too low, the strain point and Young's modulus are likely to decrease, and the glass is likely to separate into phases. 2 O 3 If the content of is too high, devitrified crystals such as mullite and anorthite are likely to precipitate, and the liquidus temperature is likely to rise.
[0062] B 2 O 3 It is a component that improves melting properties and resistance to devitrification. 2 O 3 The lower limit of the content of B is preferably 1.8%, 1.9%, and particularly preferably 2%. 2 O 3 The upper limit of the content of is preferably 4.5%, 4.2%, 4%, 3%, 2.9%, and particularly preferably 2.8%. 2 O 3 The content can be 1.8-4.5%, 1.8-4.2%, 1.8-4%, 1.8-3%, 1.9-3%, 2-3%, 2-2.9%, or 2-2.8%. 2 O 3 If the content of B is too low, the melting property and resistance to devitrification are likely to decrease, and the resistance to hydrofluoric acid-based liquid medicine is likely to decrease. In addition, the amount of water introduced from the batch may be excessively reduced. On the other hand, if B 2 O 3 If the content of is too much, the strain point and Young's modulus are likely to decrease. In addition, the amount of water introduced from the batch material increases.
[0063] MgO is a component that reduces high temperature viscosity and improves solubility. Among alkaline earth metal oxides, it is a component that significantly improves Young's modulus. The lower limit of the MgO content is preferably 0%, 0.1%, 1%, 1.5%, 2%, and particularly preferably 3%. In addition, the upper limit of the MgO content is preferably 10%, 9%, 8%, 7.5%, 7%, and particularly preferably 6%. For example, the MgO content can be 0-10%, 0.1-10%, 0.1-9%, 1-8%, 1-7.5%, 1.5-7.5%, 2-7%, 3-6%, or 2-10%. If the MgO content is too little, the solubility and Young's modulus are likely to decrease. On the other hand, if the MgO content is too much, the devitrification resistance becomes easy to decrease, and the strain point is easy to decrease.
[0064] CaO is a component that reduces high temperature viscosity and significantly improves solubility without reducing the strain point. In addition, among alkaline earth metal oxides, it is a component that reduces the cost of raw materials because the raw materials introduced are relatively cheap. The lower limit of the CaO content is preferably 0%, 0.1%, 1%, 2%, 3%, 3.5%, and particularly preferably 4%. In addition, the upper limit of the CaO content is preferably 10%, 9%, 8%, 7%, and particularly preferably 6%. For example, the CaO content can be 0-10%, 0.1-10%, 1-10%, 2-9%, 3-8%, 3.5-7%, or 4-6%. If the CaO content is too little, it is difficult to enjoy the above effects. On the other hand, if the CaO content is too much, the glass is prone to devitrification and the thermal expansion coefficient is prone to increase.
[0065] SrO is a component that suppresses phase separation and improves resistance to devitrification. Moreover, it is a component that reduces high-temperature viscosity and improves solubility without lowering the strain point. In addition, it is a component that suppresses the rise in liquidus temperature. The lower limit of the SrO content is preferably 0%, 0.1%, and particularly preferably 0.5%. In addition, the upper limit of the SrO content is preferably 10%, 9%, 8%, 7.5%, and particularly preferably 7%. For example, the SrO content can be 0-10%, 0-9%, 0-8%, 0.1-8%, 0.5-7.5%, or 0.5-7%. When the SrO content is too little, it is difficult to enjoy the above effects. On the other hand, when the SrO content is too much, devitrification crystals of the strontium silicate system are easily precipitated, and the resistance to devitrification becomes easily reduced.
[0066] BaO is a component that significantly improves resistance to devitrification. The lower limit of the BaO content is preferably 0%, 0.1%, and particularly preferably 0.5%. In addition, the upper limit of the BaO content is preferably 15%, 14%, 13%, 12%, 11%, and particularly preferably 10.5%. For example, the BaO content can be 0-15%, 0-14%, 0-13%, 0-12%, 0.1-11%, 0.5-10.5%, or 0.1-15%. When the BaO content is too little, it is difficult to enjoy the above-mentioned effects. On the other hand, when the BaO content is too much, the density becomes too high and the solubility is easily reduced. In addition, devitrification crystals containing BaO become easy to precipitate, and the liquidus temperature is easy to rise.
[0067] ZnO is a component that improves solubility. The content of ZnO is preferably 0 to 5%, 0 to 4%, 0 to 3%, and particularly preferably 0 to 2%. If the content of ZnO is too high, the glass is prone to devitrification and the strain point is prone to decrease.
[0068] ZrO 2 It is a component that improves chemical durability. ZrO 2 The lower limit of the content of ZrO is preferably 0%, and particularly preferably 0.01%. 2 The upper limit of the content of ZrO is preferably 1%, 0.5%, and particularly preferably 0.1%. 2 The content of ZrO can be 0-1%, 0-0.5%, or 0.01-0.1%. 2 If the content is too high, ZrSiO 4 of devitrified matter.
[0069] TiO 2 It is a component that reduces high temperature viscosity and improves solubility. It is also a component that inhibits the effects of exposure to sunlight. 2 The content of TiO is preferably 0 to 5%, 0 to 4%, 0 to 3%, 0 to 2%, 0 to 1%, and particularly preferably 0 to 0.1%.2 When the content of is too much, the glass will be colored and the transmittance will be easily reduced.
[0070] P 2 O 5 It is a component that increases the strain point and is a component that can suppress the precipitation of devitrified crystals of alkaline earth aluminosilicates such as anorthite. 2 O 5 The content is preferably 0 to 10%, 0 to 9%, 0 to 8%, 0 to 7%, 0 to 6%, and particularly preferably 0 to 5%. 2 O 5 If the content is too much, the glass will easily separate into phases.
[0071] SnO 2 It is a component that has a good clarifying effect in high temperature ranges, a component that increases the strain point, and a component that reduces high temperature viscosity. In addition, it has the advantage of not corroding molybdenum electrodes. SnO 2 The lower limit of the content of SnO is preferably 0.1%, particularly preferably 0.15%. 2 The upper limit of the content of SnO is preferably 0.5%, 0.45%, 0.4%, 0.35%, and particularly preferably 0.3%. 2 The content of SnO can be 0.1-0.5%, 0.1-0.45%, 0.1-0.4%, 0.1-0.35%, 0.1-0.3%, or 0.15-0.3%. 2 When the content of SnO is too small, it is difficult to enjoy the above-mentioned effects. 2 When the content of SnO is too high, 2 The devitrified crystals are easy to precipitate and promote the formation of ZrO 2 The precipitation of devitrified crystals.
[0072] In addition to the above components, other components such as Cl and F may be contained in an amount of 10% or less, particularly 5% or less in total. However, from the perspective of the environment and the prevention of electrode corrosion, it is preferred that As is substantially not contained. 2 O 3 , Sb 2 O 3 Here, "substantially free of" means that glass raw materials or glass scraps containing these components are not intentionally added to the glass batch. More specifically, in the obtained glass, arsenic is present in the form of As 2 O 3 50ppm or less, antimony as Sb 2 O 3 The content is calculated to be less than 50 ppm.
[0073] Next, the glass raw materials constituting the batch material will be described. It should be noted that the expression % in the following description of each raw material means mass % unless otherwise specified.
[0074] As a silicon source, silica sand (SiO 2 )wait.
[0075] As an aluminum source, aluminum oxide (Al 2 O 3 ), aluminum hydroxide (Al(OH) 3 )wait.
[0076] As a boron source, orthoboric acid (H 3 BO 3 ), boric anhydride (B 2 O 3 ). Orthoboric acid contains crystal water, so it is difficult to reduce the moisture content of the glass when it is used in a large proportion, but it has the effect of promoting the melting of the initial batch material, so it is preferably used. Specifically, relative to the boron source (B 2 O 3 The proportion of orthoboric acid used is preferably 0.1% or more, 0.5% or more, and particularly preferably 1% or more. In order to properly adjust the water content of the glass, it is preferred to increase the proportion of boric anhydride used. Specifically, relative to the boron source (B 2 O 3 The usage ratio of boric anhydride is preferably 50% or more, 70% or more, and particularly preferably 90% or more.
[0077] Alkaline earth metal sources can be calcium carbonate (CaCO 3 ), magnesium oxide (MgO), magnesium hydroxide (Mg(OH) 2 ), barium carbonate (BaCO 3 ), barium nitrate (Ba(NO 3 ) 2 ), strontium carbonate (SrCO 3 ), strontium nitrate (Sr(NO 3 ) 2 )wait.
[0078] As the zinc source, zinc oxide (ZnO) or the like can be used.
[0079] As a zirconium oxide source, zircon (ZrSiO 4 ) etc. It should be noted that, as the refractory constituting the melting furnace, when using a zirconia electrocasting refractory, a dense zircon or other Zr-containing refractory, there is elution of the zirconium oxide component from the refractory. These eluted components can also be used as a zirconium oxide source.
[0080] As a titanium source, titanium oxide (TiO 2 )wait.
[0081] As a phosphorus source, aluminum metaphosphate (Al(PO 3 ) 3 ), magnesium pyrophosphate (Mg 2 P 2 O 7 )wait.
[0082] As a tin source, tin oxide (SnO 2 ) etc. It should be noted that, when tin oxide is used, it is preferred to use an average particle size D 50 The average particle size of the tin oxide powder is 0.3 to 50 μm, 2 to 50 μm, and particularly 5 to 50 μm. 50 If the average particle size D of the tin oxide powder is smaller than 0.04 mm, the particles will aggregate and the production equipment will be easily clogged. 50 If the melting temperature is too high, the dissolution reaction of tin oxide powder into the glass melt will be slow, and the melt will not be clarified. As a result, oxygen cannot be fully released at the appropriate time of glass melting, bubbles are likely to remain in the glass product, and it is difficult to obtain a product with excellent bubble quality. In addition, SnO is likely to appear in the glass product. 2 The situation of crystallized insoluble matter.
[0083] In the present invention, chlorides may also be contained in the batch material. Chlorides function as a dehydrating agent that greatly reduces the water content of the glass. In addition, they have the effect of promoting the action of the tin compound as a clarifier. Furthermore, chlorides decompose and volatilize in a temperature range of 1200°C or more to produce a clarified gas, and the formation of a heterogeneous layer is suppressed by the stirring effect thereof. In addition, chlorides have the effect of taking in silica raw materials such as silica sand and dissolving them when they decompose. As chlorides, for example, chlorides of alkaline earth metals such as strontium chloride, aluminum chloride, etc., etc. can be used.
[0084] In the present invention, the batch material may contain a nitrate raw material. The nitrate raw material may be SnO 2 As a nitrate raw material, for example, barium nitrate (Ba(NO 3 ) 2 ), strontium nitrate (Sr(NO 3 ) 2 )wait.
[0085] In the present invention, the raw material batch may contain a hydroxide raw material. The hydroxide raw material may have an adjusted moisture content. As the hydroxide raw material, aluminum hydroxide (Al(OH) 3 )、Magnesium hydroxide (Mg(OH) 2), calcium hydroxide (Ca(OH) 2 )wait.
[0086] In the present invention, it is preferred that the batch material contains substantially no arsenic compounds and antimony compounds. If these components are contained, it will be difficult to perform long-term stable electric melting because they will corrode the molybdenum electrode. In addition, these components are not preferred in terms of the environment.
[0087] In the present invention, it is preferred to use glass scraps in addition to the above-mentioned glass raw materials. When glass scraps are used, the ratio of glass scraps to the total amount of the raw material batch is preferably 1% by mass or more, 5% by mass or more, and particularly preferably 10% by mass or more. There is no upper limit to the ratio of glass scraps, but it is preferably 50% by mass or less, 40% by mass or less, and particularly preferably 30% by mass or less. In addition, at least a portion of the glass scraps preferably used are low-moisture glass scraps composed of glass having a β-OH value of 0.5 / mm or less, 0.4 / mm or less, 0.35 / mm or less, 0.3 / mm or less, or 0.25 / mm or less. In addition, the lower limit of the β-OH value of the low-moisture glass scraps is not particularly limited, but is preferably 0.01 / mm or more, and particularly preferably 0.05 / mm or more.
[0088] The amount of low-water glass chips used is preferably 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more relative to the total amount of glass chips used, and it is particularly preferred that all of the low-water glass chips be low-water glass chips. If the β-OH value of the low-water glass chips is not sufficiently low, or if the proportion of low-water glass chips used is small, the effect of reducing the β-OH value of the obtained glass becomes small.
[0089] It should be noted that glass raw materials, glass scraps, or raw material batches prepared from them sometimes contain moisture. In addition, they sometimes absorb moisture from the atmosphere during storage. Therefore, in the present invention, it is preferred to introduce dry air into the raw material silo used for weighing and supplying each glass raw material, the furnace silo used for feeding the prepared raw material batches into the melting furnace, etc.
[0090] (2) Melting process
[0091] Next, the prepared raw material batch is melted.
[0092] For melting the raw material batch, a melting furnace capable of heating by radiant heat generated by combustion of a burner or Joule heat generated by energization between electrodes is used. It is particularly preferred to use a melting furnace capable of electric melting.
[0093] The melting furnace capable of electric melting has a plurality of electrodes composed of molybdenum, platinum, tin, etc., and electricity is applied between these electrodes to conduct electricity in the glass melt, and the glass is continuously melted by the Joule heat. As long as the β-OH can be controlled within the preferred range of the present invention, radiation heating based on a heater or a burner can also be used in combination. By using radiation heating based on a burner in combination, the initial raw material batch can be effectively melted.
[0094] As electrodes, platinum electrodes are preferably used. Since platinum electrodes have a high degree of freedom in configuration location and electrode shape, even for low-alkali glass that is difficult to energize, the best electrode configuration and electrode shape can be adopted, and heating by energization becomes easy. As the electrode shape, it is preferably rod-shaped. If it is rod-shaped, the desired number of electrodes can be configured at any position of the side wall surface and the bottom wall surface of the melting furnace in a manner to maintain the desired distance between electrodes. The configuration of the electrodes is preferably configured on the wall surface (side wall surface, bottom wall surface, etc.) of the melting furnace, especially on the bottom wall surface to shorten the distance between electrodes and configure multiple pairs. It should be noted that when the glass contains arsenic components and antimony components, due to the reasons already described, molybdenum electrodes cannot be used, and tin electrodes that are not corroded by these components need to be used instead. However, the configuration location and electrode shape of the tin electrode have very low degrees of freedom, so it is difficult to electrically melt the low-alkali glass.
[0095] The raw material batch put into the melting furnace is melted by radiation heat and Joule heat to form glass melt (molten glass). When chloride is contained in the raw material batch, the chloride decomposes and volatilizes, thereby taking away the moisture in the glass into the atmosphere and reducing the β-OH value of the glass. In addition, polyvalent oxides such as tin compounds contained in the raw material batch are dissolved in the glass melt and act as clarifiers. For example, the tin component releases oxygen bubbles during the heating process. The released oxygen bubbles expand the bubbles contained in the glass melt, float up and are removed from the glass. In addition, the tin component absorbs oxygen bubbles during the cooling process, thereby causing the bubbles remaining in the glass to disappear.
[0096] (3) Clarification process
[0097] Next, the molten glass is heated and clarified. The clarification step may be performed in a separate clarification tank or in a downstream portion of a melting furnace.
[0098] When the glass melt becomes higher in temperature than when it was melted, oxygen bubbles are released from the clarifier component through the above reaction, and the bubbles contained in the glass melt can be expanded, floated, and removed from the glass. At this time, the greater the difference between the temperature during melting and the temperature during clarification, the higher the clarification effect. Therefore, it is preferable to lower the temperature during melting as much as possible.
[0099] (4) Molding process
[0100] Next, the clarified glass is supplied to a forming device and formed into a plate shape. In addition, a stirring tank, a state adjustment tank, etc. may be arranged between the clarification tank and the forming device, and the glass is supplied to the forming device after passing through these devices. In addition, in order to prevent contamination of the glass, the connecting flow path connecting the melting furnace, the clarification tank, and the forming device (or the tanks arranged therebetween) is preferably made of platinum or a platinum alloy at least in contact with the glass.
[0101] The forming method is not particularly limited, but if the length of the annealing furnace is limited and it is difficult to reduce the down-drawing method of the thermal shrinkage, the effect of the present invention is easily obtained. As the down-drawing method, the overflow down-drawing method is preferably adopted. The overflow down-drawing method refers to a method in which molten glass is overflowed from both sides of a wedge-shaped groove-shaped refractory with a cross section, the molten glass after the overflow is merged at the lower end of the groove-shaped refractory, and the glass is formed into a plate-like method by extending and molding downward. In the overflow down-drawing method, the surface that should become the glass sheet surface does not contact the groove-shaped refractory, and is molded in the state of the free surface. Therefore, it is possible to manufacture a glass sheet with good surface quality without grinding at a low cost, and in addition, the large-scale and thinning of the glass are also easy. It should be noted that the structure and material of the groove-shaped refractory used in the overflow down-drawing method are not particularly limited as long as the desired size and surface accuracy can be achieved. In addition, when the extension molding is performed downward, the method of applying force is not particularly limited either. For example, a method of extending the glass by rotating a heat-resistant roller having a sufficiently large width in contact with the glass may be adopted, or a method of extending the glass by contacting a plurality of pairs of heat-resistant rollers only near the end surface of the glass may be adopted. It should be noted that, in addition to the overflow down-draw method, for example, a slit down-draw method may also be adopted.
[0102] The glass formed into a plate shape in this way is cut into predetermined sizes and subjected to various chemical or mechanical processing as necessary to form a glass plate.
[0103] Next, a low-alkali glass plate that can be produced by the method of the present invention will be described.
[0104] The heat shrinkage of the low-alkali glass plate obtained by the method of the present invention when the glass is heated from room temperature to 500°C at a rate of 5°C / min, and then cooled at a rate of 5°C / min after being kept at 500°C for 1 hour, is preferably 20 ppm or less, 19 ppm or less, 18 ppm or less, 17 ppm or less, 16 ppm or less, and particularly preferably 15 ppm or less in the case of oxide TFTs, and is preferably 14 ppm or less, 13 ppm or less, 12 ppm or less, 11 ppm or less, and particularly preferably 10 ppm or less in the case of polysilicon TFTs. If the heat shrinkage is large, it is difficult to use as a substrate for forming oxide TFTs or low-temperature polysilicon TFTs. It should be noted that the lower limit of the heat shrinkage is not limited, but is preferably 2 ppm or more, and particularly preferably 3 ppm or more.
[0105] For the low-alkali glass plate obtained by the method of the present invention, the β-OH value is preferably less than 0.26 / mm, less than 0.24 / mm, less than 0.22 / mm, and particularly preferably less than 0.20 / mm. If the β-OH value is too large, the strain point of the glass will not be sufficiently high, and it is difficult to significantly reduce the thermal shrinkage. In addition, the lower limit of the β-OH value is preferably more than 0.09 / mm, more than 0.1 / mm, more than 0.12 / mm, more than 0.14 / mm, and particularly preferably more than 0.15 / mm. If the β-OH value is too small, the glass blank must be melted at a high temperature, so the erosion of the refractory in contact with the glass melt becomes larger, and foreign matter caused by the refractory is likely to increase in the glass.
[0106] For the low-alkali glass plate obtained by the method of the present invention, it is preferred that B 2 O 3 When the content of is x (mass %) and the β-OH value is y ( / mm), the relationships y=ax+b, 0.03<a<0.04 and 0.02<b<0.1 hold. Thus, a low-alkali glass plate having a high strain point and excellent bubble quality can be easily obtained.
[0107] The strain point of the low-alkali glass obtained by the method of the present invention is preferably 700°C or more, 705°C or more, 710°C or more, 720°C or more, and particularly preferably 725°C or more. In this way, it is easy to suppress the thermal shrinkage of the glass plate in the manufacturing process of the oxide TFT or the low-temperature polysilicon TFT. If the strain point is too high, the temperature during molding or melting becomes too high, and the manufacturing cost of the glass plate is likely to rise. Therefore, the strain point is preferably 800°C or less, 790°C or less, and particularly preferably 780°C or less.
[0108] The low-alkali glass plate obtained by the method of the present invention preferably contains 10 2.5dPa·s is 1700°C or lower, 1640°C or lower, 1630°C or lower, 1620°C or lower, 1615°C or lower, and particularly preferably 1610°C or lower. 2.5 dPa·s, the glass becomes difficult to melt, the manufacturing cost of the glass plate increases, and defects such as bubbles are more likely to occur. 2.5 dPa·s is too low, it is difficult to design a high viscosity at the liquidus temperature. 2.5 The temperature of dPa·s is preferably 1490°C or higher, 1500°C or higher, and particularly preferably 1510°C or higher. 2.5 The "temperature in dPa·s" is a value measured by a platinum ball pulling method.
[0109] The low-alkali glass obtained by the method of the present invention preferably includes a glass having a liquidus temperature of less than 1300°C, less than 1290°C, less than 1280°C, less than 1270°C, less than 1260°C, and particularly less than 1250°C. In this way, devitrification crystals are not easily generated when manufacturing glass, and it is easy to prevent the situation of reduced productivity. Furthermore, since it is easy to form by overflow down-drawing, it is easy to improve the surface quality of the glass sheet and the manufacturing cost of the glass sheet can be reduced. Moreover, from the perspective of the large-scale glass sheet and the high-definition display in recent years, in order to suppress devitrification that may become a surface defect, it is of great significance to improve the resistance to devitrification. It should be noted that the liquidus temperature is an index of the resistance to devitrification, and the lower the liquidus temperature, the better the resistance to devitrification. “Liquid phase temperature” refers to the temperature at which glass powder that passes through a standard 30 mesh (500 μm) sieve and remains in a 50 mesh (300 μm) sieve is placed in a platinum boat, maintained in a temperature gradient furnace set at 1100°C to 1350°C for 24 hours, the platinum boat is taken out, and devitrification (crystalline foreign matter) is confirmed in the glass.
[0110] The low-alkali glass plate obtained by the method of the present invention preferably has a viscosity of 10 4.0 dPa·s or more, 10 4.1 dPa·s or more, 10 4.2 dPa·s or more, 10 4.3 dPa·s or more, 10 4.4 dPa·s or more, 10 4.5 dPa·s or more, 10 4.6 dPa·s or more, 10 4.7 dPa·s or more, 10 4.8 dPa·s or more, 10 4.9 dPa·s or more, especially 10 5.0dPa·s or more. In this way, devitrification is not likely to occur during molding, so it is easy to mold a glass sheet by an overflow down-draw method, and as a result, the surface quality of the glass sheet can be improved, and the manufacturing cost of the glass sheet can be reduced. It should be noted that the viscosity at the liquidus temperature is an indicator of moldability, and the higher the viscosity at the liquidus temperature, the higher the moldability. It should be noted that "viscosity at the liquidus temperature" refers to the viscosity of the glass at the liquidus temperature, which can be measured, for example, by a platinum ball pulling method.
[0111] Example
[0112] Next, the glass produced by the method of the present invention will be described. Table 1 shows Examples (No. 1 to 9) of the present invention.
[0113] [Table 1]
[0114] quality% No.1 No.2 No.3 No.4 No.5 No.6 No.7 No.8 No.9 <![CDATA[SiO 2 ]]> 60.80 61.75 59.75 60.83 59.75 60.86 60.80 60.80 59.85 <![CDATA[Al 2 THE 3 ]]> 20.0 19.0 19.0 18.5 18.0 19.0 20.0 19.0 19.0 <![CDATA[B 2 THE 3 ]]> 2.0 2.5 3.0 2.0 2.0 1.8 3.5 4.0 3.0 MgO 2.5 2.0 3.0 3.5 3.0 5.5 2.5 2.5 3.0 CaO 4.5 4.5 5.0 4.0 4.0 4.5 5.5 5.0 5.0 SrO 4.0 1.0 1.0 3.0 3.0 6.0 2.5 3.5 1.5 BaO 6.0 9.0 9.0 8.0 10.0 2.2 5.0 5.0 8.5 <![CDATA[SnO 2 ]]> 0.2 0.2 0.25 0.15 0.25 0.1 0.2 0.2 0.15 β-OH value ( / mm) 0.16 0.15 0.20 0.17 0.20 0.14 0.22 0.24 0.20 Strain point(℃) 746 740 730 738 733 725 725 715 720 Bubble quality ○ ○ ○ ○ ○ ○ ○ ○ ○ Thermal shrinkage (ppm) 10 12 13 11 12 13 14 16 15 y=ax+b ○ ○ ○ ○ ○ ○ ○ ○ ○
[0115] First, silica sand, aluminum oxide, boric anhydride, calcium carbonate, strontium nitrate, barium carbonate, aluminum metaphosphate, tin oxide (Japanese: second tin oxide), strontium chloride, and barium chloride were mixed and blended to obtain the composition shown in Table 1. In addition, glass chips (β-OH value of 0.1 / mm, 35% by mass relative to the total amount of the raw material batch) having the same composition as the target composition were used.
[0116] Next, the glass raw material is supplied to an electric melting furnace that is not burned by a burner and melted, and then the molten glass is clarified and homogenized in a clarification tank and an adjustment tank, and adjusted to a viscosity suitable for molding. In addition, the maximum temperature in the clarification tank is the temperature shown in Table 1. It should be noted that the maximum temperature in the clarification tank is confirmed by monitoring the temperature of platinum or platinum alloy attached to the inner wall of the clarification tank.
[0117] Next, the molten glass was supplied to an overflow down-draw molding apparatus, molded into a plate, and then cut to obtain a glass sample with a thickness of 0.5 mm. It should be noted that the molten glass from the melting furnace was supplied to the molding apparatus only in contact with platinum or a platinum alloy.
[0118] The obtained glass samples were evaluated for β-OH value, strain point, thermal shrinkage, bubble quality, and whether y=ax+b (x is B 2 O 3 The results are shown in Table 1.
[0119] As shown in Table 1, Examples No. 1 to 9 satisfy the above formula, with a β-OH value as low as 0.24 / mm or less, a strain point as high as 715°C or more, a heat shrinkage as low as 16 ppm or less, and excellent foam quality.
[0120] In addition, the β-OH value of glass is determined by measuring the transmittance of glass using FT-IR and using the following formula.
[0121] β-OH value = (1 / X) log10 (T 1 / T 2 )
[0122] X: Glass wall thickness (mm)
[0123] T 1 :Reference wavelength 3846cm -1 Transmittance at (%)
[0124] T 2 :Hydroxy absorption wavelength 3600cm -1 Minimum transmittance near (%)
[0125] The strain point was measured according to the method of ASTM C336-71.
[0126] The thermal shrinkage is determined by the following method. Figure 2 As shown in (a), a 160 mm × 30 mm long strip sample G is prepared as a glass plate sample. #1000 water-resistant abrasive paper is used to form a mark M at a position 20 to 40 mm away from the edge of the long side of the long strip sample G. Figure 2 As shown in (b), a long strip sample G with a mark M formed thereon is folded into two along a direction perpendicular to the mark M to make sample pieces Ga and Gb. Then, only one sample piece Gb is subjected to a heat treatment in which the temperature is raised from room temperature (25°C) to 500°C at a rate of 5°C / min, maintained at 500°C for 1 hour, and then cooled to room temperature at a rate of 5°C / min. After the above heat treatment, Figure 2 As shown in (c), the unheat-treated sample Ga and the heat-treated sample Gb are arranged side by side, and the positional displacement (ΔL) of the mark M in the two sample pieces Ga and Gb is read using a laser microscope. 1 , ΔL 2 ), the thermal shrinkage is calculated by the following formula. 0 is the initial distance between markers M.
[0127] Thermal shrinkage = [{ΔL 1 (μm)+ΔL 2 (μm)}×10 3 ] / l 0 (mm)(ppm)
[0128] The bubble quality was determined by counting bubbles with a diameter of 100 μm or more, with a count of 0.05 bubbles / kg or less being indicated as “0”, and a count of more than 0.05 bubbles / kg being indicated as “×”.
[0129] Will satisfy y = ax + b (x is B 2 O 3 The case where the formula (content (mass %) was satisfied, y was the β-OH value ( / mm), 0.03<a<0.04 and 0.02<b<0.1) was regarded as “0”, and the case where it was not satisfied was regarded as “×”.
[0130] Industrial Applicability
[0131] According to the present invention, it is possible to easily obtain a glass plate having a high strain point, good bubble quality, and a small thermal shrinkage rate suitable for manufacturing oxide TFTs or low-temperature polysilicon TFTs.
Claims
1. A method for manufacturing a low-alkali glass plate, characterized in that: include: a batch material preparation step of preparing a raw material batch material so as to produce a low-alkali glass having a glass composition containing, by mass%, SiO2 50-70%, Al2O3 15-25%, B2O3 1.8-4.5%, MgO 2-10%, CaO 0-10%, SrO 2.5-6%, BaO 0-8.5%, ZnO 0-5%, ZrO2 0-1%, TiO2 0-5%, P2O 50-10%, and SnO2 0.1-0.5%; a melting process, melting the prepared raw material batch; The clarification process clarifies the molten glass; as well as The forming process is to form the clarified glass into a plate shape. The content of B2O3 in mass % is set to x, and the thickness of the obtained low-alkali glass plate is set to mm. -1 When the β-OH value in units is y, the B2O3 content and the β-OH value are adjusted so that the relationships y=ax+b, 0.03<a<0.04 and 0.02<b<0.1 hold.
2. The method for manufacturing a low-alkali glass plate according to claim 1, wherein: A low-alkali glass plate containing, in terms of mass %, SiO2 60-70%, B2O3 1.8-3%, MgO 2-10%, BaO 0.1-8.5%, and SnO2 0.1-0.3% was obtained.
3. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: The prepared raw material batch is electro-melted.
4. The method for producing a low-alkali glass plate according to claim 3, wherein: During the melting process, radiant heating based on burner combustion is not used.
5. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: Nitrate raw materials are included in the raw material batch.
6. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: Boric anhydride is used as at least a part of the glass raw material as a boron source.
7. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: The raw material batch contains a hydroxide raw material.
8. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: The raw material batch contains glass cullets, and at least a portion of the glass cullets is glass cullets containing glass having a β-OH value of 0.5 / mm or less.
9. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: Glass raw materials and / or melting conditions are adjusted so that the β-OH value of the obtained glass is less than 0.26 / mm.
10. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: The strain point of the obtained glass is 700° C. or higher.
11. The method for producing a low-alkali glass plate according to claim 1 or 2, wherein: The thermal shrinkage of the obtained glass was 20 ppm or less.
12. A low-alkali glass plate, characterized in that: The glass composition comprises, in mass%, 50-70% SiO2, 15-25% Al2O3, 1.8-4.5% B2O3, 2-10% MgO, 0-10% CaO, 2.5-6% SrO, 0-8.5% BaO, 0-5% ZnO, 0-1% ZrO2, 0-5% TiO2, 0-10% P2O5, and 0.1-0.5% SnO2, and has a β-OH value of not less than 0.1 / mm and less than 0.22 / mm. The content of B2O3 in mass % is x, and the content in mm -1 When the β-OH value in units of α is denoted as y, the following relationships hold: y=ax+b, 0.03<a<0.04, and 0.02<b<0.
1.
13. The low-alkali glass plate according to claim 12, wherein The glass composition includes, by mass%, 15 to 21% Al2O3, 2 to 4% B2O3, 2 to 10% MgO, 0.1 to 10% CaO, 0 to 0.5% ZrO2, and 0 to 1% TiO2.
14. The low-alkali glass plate according to claim 12 or 13, wherein The glass composition includes, by mass%, 60-70% SiO2, 2-3% B2O3, 2-10% MgO, 0.1-8.5% BaO, and 0.1-0.3% SnO2.
15. The low-alkali glass plate according to claim 12 or 13, wherein The strain point is 700°C or higher.
16. The low-alkali glass plate according to claim 12 or 13, wherein: The thermal shrinkage is less than 20ppm.
17. The low-alkali glass plate according to claim 12 or 13, wherein Used as a glass plate for forming oxide TFTs or low-temperature p-Si TFTs.
18. A method for manufacturing a low-alkali glass plate, characterized in that: The low-alkali glass plate comprises, as a glass composition, in mass %, 50-70% SiO2, 15-25% Al2O3, 1.8-3% B2O3, 2-10% MgO, 0-10% CaO, 2.5-6% SrO, 0-8.5% BaO, 0-5% ZnO, 0-1% ZrO2, 0-5% TiO2, 50-10% P2O, and 0.1-0.5% SnO2, and has a β-OH value of 0.1 / mm or more and less than 0.22 / mm. The content of B2O3 in mass % is x, and the content in mm -1 When the β-OH value in units is y, the B2O3 content and the β-OH value are adjusted so that the relationships y=ax+b, 0.03<a<0.04 and 0.05<b<0.1 hold.
19. A low-alkali glass plate, characterized in that: The glass composition comprises, in mass%, 50-70% SiO2, 15-25% Al2O3, 1.8-3% B2O3, 2-10% MgO, 0-10% CaO, 2.5-6% SrO, 0-8.5% BaO, 0-5% ZnO, 0-1% ZrO2, 0-5% TiO2, 0-10% P2O5, and 0.1-0.5% SnO2, and has a β-OH value of not less than 0.1 / mm and less than 0.22 / mm. The content of B2O3 in mass % is x, and the content in mm -1 When the β-OH value in units of α is denoted as y, the following relationships hold: y=ax+b, 0.03<a<0.04, and 0.05<b<0.1.
Citation Information
Patent Citations
Alkali-free glass
JP2013151407A
Glass
CN110088053A
Alkali-free glass substrate production method
CN110114318A
Method for producing alkali-free glass substrate, and alkali-free glass substrate
CN111051255A